Preparation method of high-voltage lithium battery with flame-retardant polymer solid electrolyte
By using fluorine-containing acrylate and multifunctional acrylate crosslinking agent in lithium batteries, the adverse effects of existing flame retardant electrolytes on the performance of lithium batteries are solved, and good resistance of high-voltage lithium batteries is achieved. Fueling effect and cycle stability.
Patent Information
- Application Number
- CN202411402399.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-09
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing solid or liquid flame retardant electrolytes have adverse effects on the performance of lithium batteries, especially under high voltage conditions, which can easily lead to increased risk of electrochemical decomposition and thermal runaway.
The flame-retardant polymer solid electrolyte combined with fluorine-containing acrylate monomer and a polyfunctional acrylate crosslinking agent is used to inject prefabricated precursor liquid into a lithium battery and stand at high temperature to form good flame retardant and optimized electrochemistry. Performance of electrolyte.
Improves the cycle stability and flame retardant effect of lithium batteries, reduces the risk of thermal runaway in the battery, maintains good battery performance, and generates an electrolyte membrane in situ, reduces the solid/solid interface impedance, and improves the positive and negative electrode materials. Interface stability.
Smart Images

Figure CN119050489A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium batteries, and in particular to a method for preparing a high-voltage lithium battery with a flame-retardant polymer solid electrolyte. Background Art
[0002] As the market's requirements for lithium battery energy density become higher and higher, high-voltage lithium batteries are gradually entering the market. Common lithium batteries are equipped with carbonate electrolytes, which have poor electrochemical stability. When the voltage of the lithium battery is high, the carbonate electrolyte is prone to electrochemical decomposition. When catalyzed by transition metal ions in the positive electrode, the degree of oxidative decomposition of the carbonate electrolyte is more intense. Therefore, as the battery capacity increases, the risk of thermal runaway of the battery will further increase.
[0003] Introducing phosphorus-containing flame retardants into the electrolyte is also one of the carbonate electrolytes. The introduction of flame retardants makes the electrolyte exhibit good flame retardancy, but it will have an adverse effect on battery performance. The method of using ionic liquids as electrolytes is also a carbonate electrolyte, but the viscosity of ionic liquids is relatively large, which reduces the conductivity of the electrolyte, thereby having an adverse effect on battery performance. Therefore, there is a technical problem that existing solid or liquid flame retardant electrolytes will have an adverse effect on battery performance.
[0004] Therefore, it is necessary to provide a method for preparing a high-voltage lithium battery with a flame-retardant polymer solid electrolyte to solve the above technical problems. Summary of the invention
[0005] The present invention provides a method for preparing a high-voltage lithium battery with a flame-retardant polymer solid electrolyte, which effectively solves the technical problem that the existing solid or liquid flame-retardant electrolyte has an adverse effect on battery performance.
[0006] A method for preparing a lithium battery having a flame retardant polymer solid electrolyte, comprising the following steps:
[0007] S1: using lithium salt as solute and plasticizer as solvent to prepare a solution of preset concentration, wherein the preset concentration is the molar concentration of the lithium salt in the plasticizer of 0.8 mol / L-2 mol / L;
[0008] S2: adding a fluorinated acrylate monomer and a multifunctional acrylate crosslinking agent to the solution obtained in step S1 according to a set stoichiometric ratio to obtain a mixed solution, and then adding an initiator, and mixing them evenly to obtain a precursor solution; wherein the stoichiometric ratio of the fluorinated acrylate monomer to the multifunctional acrylate crosslinking agent is in the range of 1:1-1:3, and the total mass of the fluorinated acrylate monomer and the multifunctional acrylate crosslinking agent in the mixed solution is 20-90% by mass; the mass of the initiator is 1-10% of the total mass of the fluorinated acrylate monomer and the multifunctional acrylate crosslinking agent;
[0009] S3: Assembling a lithium battery with a negative electrode of a lithium battery, a positive electrode of a lithium battery and a separator;
[0010] S4: injecting the precursor solution obtained in step S4 into the lithium battery, leaving it at room temperature for 48 hours, and subjecting the precursor solution to a high-temperature standing operation in the temperature range of 50-100° C., and obtaining a lithium battery with a flame-retardant polymer solid electrolyte after leaving it at high temperature for 4-24 hours.
[0011] In the method for preparing a lithium battery with a flame-retardant polymer solid electrolyte of the present invention, in step S2, the mass fraction of the total mass of the fluorine-containing acrylate monomer and the multifunctional acrylate crosslinking agent in the solution is 50-75%.
[0012] In the method for preparing a high-voltage lithium battery with a flame-retardant polymer solid electrolyte described in the present invention, in the step S3, the injection amount of the precursor solution is determined by the battery capacity of the lithium battery, the injection amount of the precursor solution is 2-6g / Ah, the high-temperature standing temperature is 60-80°C, and the high-temperature standing time is 8-12 hours.
[0013] In the preparation method of a high-voltage lithium battery with a flame-retardant polymer solid electrolyte described in the present invention, the fluorine-containing acrylate monomer is composed of one or more combinations of octafluoro-1,6-hexanediol diacrylate, 2,2,3,3,4,4,5,5-octafluoro-1,6-dimethylacrylate, 2,2,3,3,4,4-hexafluoro-1,5-pentyl diacrylate, and 1,1'-(2,2,3,3,4,4-hexafluoro-1,5-pentanediyl)bis(2-methyl-2-acrylate).
[0014] In the preparation method of the high-voltage lithium battery with a flame-retardant polymer solid electrolyte described in the present invention, the multifunctional acrylate crosslinking agent is composed of one or more combinations of trimethylolpropane triacrylate, ethoxylated trimethylolpropane triacrylate, pentaerythritol tetraacrylate, and polydipentaerythritol hexaacrylate.
[0015] In the preparation method of a high-voltage lithium battery with a flame-retardant polymer solid electrolyte described in the present invention, the initiator is composed of one or more combinations of azobisisobutyronitrile, azobisisoheptanenitrile, dibenzoyl peroxide, dodecyl peroxide, diethylhexyl peroxydicarbonate, and tert-butyl peroxypentanoate.
[0016] In the preparation method of a high-voltage lithium battery with a flame-retardant polymer solid electrolyte described in the present invention, the plasticizer is composed of one or more combinations of fluoroethylene carbonate, 2,2,2-trifluoro-N,N-dimethylacetamide, methyl trifluoroethyl carbonate, ethyl trifluoroethyl carbonate, 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether, and 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether.
[0017] In the preparation method of the high-voltage lithium battery with a flame-retardant polymer solid electrolyte described in the present invention, the lithium salt is composed of one or more combinations of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium hexafluoroarsenate, lithium difluorooxalatoborate, lithium perchlorate, lithium bis(oxalatoborate), lithium trichloromethylsulfonate, lithium bis(trifluoromethylsulfonyl imide), and lithium bis(fluorosulfonyl imide).
[0018] In the preparation method of a high-voltage lithium battery with a flame-retardant polymer solid electrolyte described in the present invention, the negative electrode of the lithium battery is any one of graphite, soft carbon, hard carbon, silicon, and lithium metal; the positive electrode of the lithium battery is any one of a nickel-cobalt-manganese ternary material, a nickel-cobalt-aluminum ternary material, lithium cobaltate, and lithium manganate; and the diaphragm is any one of a polyethylene diaphragm, a polypropylene diaphragm, a polyimide diaphragm, a cellulose diaphragm, a glass fiber diaphragm, a polyethylene terephthalate diaphragm, and a non-woven fabric diaphragm.
[0019] A method for preparing a high voltage lithium battery, comprising:
[0020] Weigh 1.519 g of lithium hexafluorophosphate, where the lithium hexafluorophosphate is a lithium salt, and dissolve the 1.519 g of lithium hexafluorophosphate in 10 ml of a first mixed solution of fluoroethylene carbonate and 2,2,2-trifluoro-N,N-dimethylacetamide to form an electrolyte, where the fluoroethylene carbonate and 2,2,2-trifluoro-N,N-dimethylacetamide are plasticizers, wherein the mass ratio of the fluoroethylene carbonate to the 2,2,2-trifluoro-N,N-dimethylacetamide is 1:3;
[0021] Take 3.999g of the electrolyte, add 0.740g of octafluoro-1,6-hexanediol diacrylate and 0.593g of trimethylolpropane triacrylate to the 3.999g electrolyte, the stoichiometric number of octafluoro-1,6-hexanediol diacrylate is 2mmol, and the stoichiometric number of trimethylolpropane triacrylate is 2mmol, to form a second mixed solution, and the mass fraction of the electrolyte in the second mixed solution is 75%, octafluoro-1,6-hexanediol diacrylate is a fluorine-containing acrylate monomer, and trimethylolpropane triacrylate is a multifunctional acrylate crosslinking agent. After the second mixed solution is uniformly stirred, 0.026g of azobisisobutyronitrile is added to the second mixed solution to form a third mixed solution, azobisisobutyronitrile is an initiator, and the third mixed solution is stirred for 30 minutes to obtain a precursor solution having a flame-retardant polymer solid electrolyte;
[0022] A soft-pack lithium-ion battery is assembled using graphite as the negative electrode of the lithium battery, high-voltage lithium cobalt oxide as the positive electrode of the lithium battery, and polypropylene as the separator, and 5.000g of the precursor solution is weighed and injected into the lithium battery; after being left at room temperature for 48 hours, a high-temperature static operation at 60°C is performed for 8 hours, thereby obtaining a high-voltage lithium battery with a flame-retardant polymer solid electrolyte.
[0023] Compared with the prior art, the present invention has the following beneficial effects: the present invention provides a method for preparing a high-voltage lithium battery with a flame-retardant polymer solid electrolyte. In the electrolyte of the battery, the monomer contains a large amount of fluorine element, so that the electrolyte has good flame retardancy. At the same time, the electrolyte of the battery contains a fluorine plasticizer, which optimizes the electrochemical properties of the electrolyte and improves the cycle stability of the high-voltage lithium battery with a flame-retardant polymer solid electrolyte. Therefore, the high-voltage lithium battery with a flame-retardant polymer solid electrolyte has a good flame retardant effect. Moreover, the high-voltage lithium battery with a flame-retardant polymer solid electrolyte can also maintain good battery performance. The technical problem that the existing solid or liquid flame-retardant electrolytes have an adverse effect on battery performance is effectively solved. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments. The drawings described below are only drawings corresponding to some embodiments of the present invention.
[0025] Figure 1 The present invention is a process flow chart of a method for preparing a high-voltage lithium battery with a flame-retardant polymer solid electrolyte. DETAILED DESCRIPTION
[0026] The technical solution of the invention will be described in detail below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the invention and are not used to limit the scope of the invention. After reading the invention, various equivalent forms of modifications to the invention made by those skilled in the art all fall within the scope defined by the claims attached to this application.
[0027] The terms "first", "second", etc. in the present invention are used for descriptive purposes only and should not be understood as indicating or implying relative importance, and should not be used as a limitation on the order of precedence.
[0028] The present invention provides a method for preparing a lithium battery having a flame retardant polymer solid electrolyte, which comprises the following steps:
[0029] S1: using lithium salt as solute and plasticizer as solvent to prepare a solution of preset concentration, wherein the preset concentration is the molar concentration of the lithium salt in the plasticizer of 0.8 mol / L-2 mol / L;
[0030] S2: adding a fluorinated acrylate monomer and a multifunctional acrylate crosslinking agent to the solution obtained in step S1 according to a set stoichiometric ratio to obtain a mixed solution, and then adding an initiator, and mixing them evenly to obtain a precursor solution; wherein the stoichiometric ratio of the fluorinated acrylate monomer to the multifunctional acrylate crosslinking agent is in the range of 1:1-1:3, and the total mass of the fluorinated acrylate monomer and the multifunctional acrylate crosslinking agent in the mixed solution is 20-90% by mass; the mass of the initiator is 1-10% of the total mass of the fluorinated acrylate monomer and the multifunctional acrylate crosslinking agent;
[0031] S3: Assembling a lithium battery with a negative electrode of a lithium battery, a positive electrode of a lithium battery and a separator;
[0032] S4: injecting the precursor solution obtained in step S2 into the lithium battery, leaving it at room temperature for 48 hours, and then subjecting the precursor solution to a high-temperature standing operation in the temperature range of 50-100° C., and obtaining a lithium battery with a flame-retardant polymer solid electrolyte after leaving it at high temperature for 4-24 hours.
[0033] In step S2 of the present invention, the total mass fraction of the fluorine-containing acrylate monomer and the multifunctional acrylate cross-linking agent in the solution is 50-75%.
[0034] In step S4 of the present invention, the injection amount of the precursor solution is determined by the battery capacity of the lithium battery, the injection amount of the precursor solution is 2-6 g / Ah, the high temperature standing temperature is 60-80° C., and the high temperature standing time is 8-12 hours.
[0035] In the present invention, the fluorine-containing acrylate monomer is composed of one or more combinations of octafluoro-1,6-hexanediol diacrylate, 2,2,3,3,4,4,5,5-octafluoro-1,6-dimethylacrylate, 2,2,3,3,4,4-hexafluoro-1,5-pentyl diacrylate, and 1,1'-(2,2,3,3,4,4-hexafluoro-1,5-pentanediyl)bis(2-methyl-2-acrylate).
[0036] In the present invention, the multifunctional acrylate crosslinking agent is composed of one or more combinations of trimethylolpropane triacrylate, ethoxylated trimethylolpropane triacrylate, pentaerythritol tetraacrylate, and polydipentaerythritol hexaacrylate.
[0037] In the present invention, the initiator is composed of one or more combinations of azobisisobutyronitrile, azobisisoheptylnitrile, dibenzoyl peroxide, dodecyl peroxide, diethylhexyl peroxydicarbonate, and tert-butyl peroxyvalerate.
[0038] In the present invention, the plasticizer is composed of one or more combinations of fluoroethylene carbonate, 2,2,2-trifluoro-N,N-dimethylacetamide, methyl trifluoroethyl carbonate, ethyl trifluoroethyl carbonate, 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether, and 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether.
[0039] In the present invention, the lithium salt is composed of one or more combinations of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium hexafluoroarsenate, lithium difluorooxalatoborate, lithium perchlorate, lithium bisoxalatoborate, lithium trichloromethylsulfonate, lithium bistrifluoromethylsulfonyl imide, and lithium bisfluorosulfonyl imide.
[0040] In the present invention, the negative electrode of the lithium battery is any one of graphite, soft carbon, hard carbon, silicon, and lithium metal; the positive electrode of the lithium battery is any one of nickel-cobalt-manganese ternary material, nickel-cobalt-aluminum ternary material, lithium cobalt oxide, and lithium manganese oxide; the diaphragm is any one of polyethylene diaphragm, polypropylene diaphragm, polyimide diaphragm, cellulose diaphragm, glass fiber diaphragm, polyethylene terephthalate diaphragm, and non-woven fabric diaphragm.
[0041] The present invention also provides a method for preparing a high-voltage lithium battery. Example 1 of the method for preparing a high-voltage lithium battery is as follows:
[0042] Weigh 1.519 g of lithium hexafluorophosphate, where the lithium hexafluorophosphate is a lithium salt, and dissolve the 1.519 g of lithium hexafluorophosphate in 10 ml of a first mixed solution of fluoroethylene carbonate and 2,2,2-trifluoro-N,N-dimethylacetamide to form an electrolyte, where the fluoroethylene carbonate and 2,2,2-trifluoro-N,N-dimethylacetamide are plasticizers, wherein the mass ratio of the fluoroethylene carbonate to the 2,2,2-trifluoro-N,N-dimethylacetamide is 1:3;
[0043] 3.999 g of electrolyte is taken, and 0.740 g of octafluoro-1,6-hexanediol diacrylate and 0.593 g of trimethylolpropane triacrylate are added to the 3.999 g of electrolyte, the stoichiometric ratio of octafluoro-1,6-hexanediol diacrylate is 2 mmol, and the stoichiometric ratio of trimethylolpropane triacrylate is 2 mmol, to form a second mixed solution, and the mass fraction of the electrolyte in the second mixed solution is 75%, octafluoro-1,6-hexanediol diacrylate is a fluorine-containing acrylate monomer, and trimethylolpropane triacrylate is a multifunctional acrylate crosslinking agent. After the second mixed solution is uniformly stirred, 0.026 g of azobisisobutyronitrile is added to the second mixed solution to form a third mixed solution, and azobisisobutyronitrile is an initiator. The third mixed solution is stirred for 30 minutes to obtain a precursor solution having a flame-retardant polymer solid electrolyte;
[0044] A soft-pack lithium-ion battery is assembled using graphite as the negative electrode of the lithium battery, high-voltage lithium cobalt oxide as the positive electrode of the lithium battery, and polypropylene as the separator. 5.000g of the precursor solution is weighed and injected into the lithium battery. After being placed at room temperature for 48 hours, a high-temperature static operation at 60°C for 8 hours is performed to obtain a high-voltage lithium battery with a flame-retardant polymer solid electrolyte.
[0045] Example 2 of the preparation method of the high voltage lithium battery is as follows:
[0046] Weigh 1.519 g of lithium hexafluorophosphate, where the lithium hexafluorophosphate is a lithium salt, and dissolve the 1.519 g of lithium hexafluorophosphate in 10 ml of a first mixed solution of fluoroethylene carbonate and 2,2,2-trifluoro-N,N-dimethylacetamide to form an electrolyte, where the fluoroethylene carbonate and 2,2,2-trifluoro-N,N-dimethylacetamide are plasticizers, wherein the mass ratio of the fluoroethylene carbonate to the 2,2,2-trifluoro-N,N-dimethylacetamide is 1:3;
[0047] 3.999 g of electrolyte is taken, and 7.40 g of octafluoro-1,6-hexanediol diacrylate and 0.593 g of trimethylolpropane triacrylate are added to the 3.999 g of electrolyte, the stoichiometric ratio of octafluoro-1,6-hexanediol diacrylate is 20 mmol, and the stoichiometric ratio of trimethylolpropane triacrylate is 2 mmol, to form a second mixed solution, and the mass fraction of the electrolyte in the second mixed solution is 75%, octafluoro-1,6-hexanediol diacrylate is a fluorine-containing acrylate monomer, and trimethylolpropane triacrylate is a multifunctional acrylate crosslinking agent. After the second mixed solution is uniformly stirred, 0.026 g of azobisisobutyronitrile is added to the second mixed solution to form a third mixed solution, and azobisisobutyronitrile is an initiator. The third mixed solution is stirred for 30 minutes to obtain a precursor solution having a flame-retardant polymer solid electrolyte;
[0048] A soft-pack lithium-ion battery is assembled using graphite as the negative electrode of the lithium battery, high-voltage lithium cobalt oxide as the positive electrode of the lithium battery, and polypropylene as the separator. 5.000g of the precursor solution is weighed and injected into the lithium battery. After being placed at room temperature for 48 hours, a high-temperature static operation at 60°C for 8 hours is performed to obtain a high-voltage lithium battery with a flame-retardant polymer solid electrolyte.
[0049] Example 3 of the preparation method of the high voltage lithium battery is as follows:
[0050] Weigh 1.519 g of lithium hexafluorophosphate, where the lithium hexafluorophosphate is a lithium salt, and dissolve the 1.519 g of lithium hexafluorophosphate in a first mixed solution of 10 ml of fluoroethylene carbonate and 2,2,2-trifluoro-N,N-dimethylacetamide to form an electrolyte, where the fluoroethylene carbonate and 2,2,2-trifluoro-N,N-dimethylacetamide are plasticizers, wherein the mass ratio of the fluoroethylene carbonate to the 2,2,2-trifluoro-N,N-dimethylacetamide is 1:3;
[0051] 3.999 g of electrolyte is taken, and 2.960 g of octafluoro-1,6-hexanediol diacrylate and 0.593 g of trimethylolpropane triacrylate are added to the 3.999 g of electrolyte, the stoichiometric ratio of octafluoro-1,6-hexanediol diacrylate is 8 mmol, and the stoichiometric ratio of trimethylolpropane triacrylate is 2 mmol, to form a second mixed solution, and the mass fraction of the electrolyte in the second mixed solution is 75%, octafluoro-1,6-hexanediol diacrylate is a fluorine-containing acrylate monomer, and trimethylolpropane triacrylate is a multifunctional acrylate crosslinking agent. After the second mixed solution is uniformly stirred, 0.026 g of azobisisobutyronitrile is added to the second mixed solution to form a third mixed solution, wherein azobisisobutyronitrile is an initiator, and the third mixed solution is stirred for 30 minutes to obtain a precursor solution having a flame-retardant polymer solid electrolyte;
[0052] A soft-pack lithium-ion battery is assembled using graphite as the negative electrode of the lithium battery, high-voltage lithium cobalt oxide as the positive electrode of the lithium battery, and polypropylene as the separator. 5.000g of the precursor solution is weighed and injected into the lithium battery. After being placed at room temperature for 48 hours, a high-temperature static operation at 60°C for 8 hours is performed to obtain a high-voltage lithium battery with a flame-retardant polymer solid electrolyte.
[0053] Example 4 of the preparation method of the high voltage lithium battery is as follows:
[0054] Weigh 1.519 g of lithium hexafluorophosphate, where the lithium hexafluorophosphate is a lithium salt, and dissolve the 1.519 g of lithium hexafluorophosphate in a first mixed solution of 10 ml of fluoroethylene carbonate and 2,2,2-trifluoro-N,N-dimethylacetamide to form an electrolyte, where the fluoroethylene carbonate and 2,2,2-trifluoro-N,N-dimethylacetamide are plasticizers, wherein the mass ratio of the fluoroethylene carbonate to the 2,2,2-trifluoro-N,N-dimethylacetamide is 1:3;
[0055] 3.999 g of electrolyte is taken, and 2.220 g of octafluoro-1,6-hexanediol diacrylate and 0.593 g of trimethylolpropane triacrylate are added to the 3.999 g of electrolyte, the stoichiometric ratio of octafluoro-1,6-hexanediol diacrylate is 6 mmol, and the stoichiometric ratio of trimethylolpropane triacrylate is 2 mmol, to form a second mixed solution, and the mass fraction of the electrolyte in the second mixed solution is 75%, octafluoro-1,6-hexanediol diacrylate is a fluorine-containing acrylate monomer, and trimethylolpropane triacrylate is a multifunctional acrylate crosslinking agent. After the second mixed solution is uniformly stirred, 0.026 g of azobisisobutyronitrile is added to the second mixed solution to form a third mixed solution, and azobisisobutyronitrile is an initiator. The third mixed solution is stirred for 30 minutes to obtain a precursor solution having a flame-retardant polymer solid electrolyte;
[0056] A soft-pack lithium-ion battery is assembled using graphite as the negative electrode of the lithium battery, high-voltage lithium cobalt oxide as the positive electrode of the lithium battery, and polypropylene as the separator. 5.000g of the precursor solution is weighed and injected into the lithium battery. After being placed at room temperature for 48 hours, a high-temperature static operation at 60°C for 8 hours is performed to obtain a high-voltage lithium battery with a flame-retardant polymer solid electrolyte.
[0057] Example 5 of the preparation method of the high voltage lithium battery is as follows:
[0058] Weigh 1.519 g of lithium hexafluorophosphate, where the lithium hexafluorophosphate is a lithium salt, and dissolve the 1.519 g of lithium hexafluorophosphate in a first mixed solution of 10 ml of fluoroethylene carbonate and 2,2,2-trifluoro-N,N-dimethylacetamide to form an electrolyte, where the fluoroethylene carbonate and 2,2,2-trifluoro-N,N-dimethylacetamide are plasticizers, wherein the mass ratio of the fluoroethylene carbonate to the 2,2,2-trifluoro-N,N-dimethylacetamide is 1:3;
[0059] 3.999 g of electrolyte is taken, and 0.740 g of octafluoro-1,6-hexanediol diacrylate and 1.186 g of trimethylolpropane triacrylate are added to the 3.999 g of electrolyte, the stoichiometric ratio of octafluoro-1,6-hexanediol diacrylate is 2 mmol, and the stoichiometric ratio of trimethylolpropane triacrylate is 4 mmol, to form a second mixed solution, and the mass fraction of the electrolyte in the second mixed solution is 75%, octafluoro-1,6-hexanediol diacrylate is a fluorine-containing acrylate monomer, and trimethylolpropane triacrylate is a multifunctional acrylate crosslinking agent. After the second mixed solution is uniformly stirred, 0.026 g of azobisisobutyronitrile is added to the second mixed solution to form a third mixed solution, and azobisisobutyronitrile is an initiator. The third mixed solution is stirred for 30 minutes to obtain a precursor solution having a flame-retardant polymer solid electrolyte;
[0060] A soft-pack lithium-ion battery is assembled using graphite as the negative electrode of the lithium battery, high-voltage lithium cobalt oxide as the positive electrode of the lithium battery, and polypropylene as the separator. 5.000g of the precursor solution is weighed and injected into the lithium battery. After being placed at room temperature for 48 hours, a high-temperature static operation at 60°C for 8 hours is performed to obtain a high-voltage lithium battery with a flame-retardant polymer solid electrolyte.
[0061] In Example 2-5, the reaction process is the same as in Example 1, except that the stoichiometric ratio of the fluorinated acrylate monomer octafluoro-1,6-hexanediol diacrylate and the multifunctional acrylate crosslinking agent trimethylolpropane triacrylate is changed, as shown in Table 1.
[0062] Table 1
[0063] Stoichiometric ratio Conductivity (mS / cm) Limiting oxygen index Example 1 1:1 2.19 26 Example 2 10:1 1.02 33 Example 3 4:1 1.15 29 Example 4 3:1 1.84 27 Example 5 1:2 2.66 22
[0064] The higher the limiting oxygen index, the better the flame retardant effect of the lithium battery; the higher the conductivity, the better the battery performance. The standard of the limiting oxygen index is set to 25. If the limiting oxygen index is greater than or equal to 25, it meets the standard of lithium battery flame retardancy. If the limiting oxygen index is less than 25, it does not meet the standard of lithium battery flame retardancy. In Table 1, Example 1, Example 2, Example 3 and Example 4 meet the standard of lithium battery flame retardancy. In addition, the conductivity of Example 1 is greater than the conductivity of Example 3, and the conductivity of Example 1 is greater than the conductivity of Example 4.
[0065] The preparation method of Example 1 can make the battery performance better, so Example 1 is the best example.
[0066] Example 6 of the preparation method of the high voltage lithium battery is as follows:
[0067] Weigh 1.519 g of lithium hexafluorophosphate, where the lithium hexafluorophosphate is a lithium salt, and dissolve the 1.519 g of lithium hexafluorophosphate in 10 ml of a first mixed solution of fluoroethylene carbonate and 2,2,2-trifluoro-N,N-dimethylacetamide to form an electrolyte, where the fluoroethylene carbonate and 2,2,2-trifluoro-N,N-dimethylacetamide are plasticizers, wherein the mass ratio of the fluoroethylene carbonate to the 2,2,2-trifluoro-N,N-dimethylacetamide is 1:3;
[0068] 4.2656 g of electrolyte was taken, and 0.740 g of octafluoro-1,6-hexanediol diacrylate and 0.593 g of trimethylolpropane triacrylate were added to the 4.2656 g electrolyte, the stoichiometric ratio of octafluoro-1,6-hexanediol diacrylate was 2 mmol, and the stoichiometric ratio of trimethylolpropane triacrylate was 2 mmol, to form a second mixed solution, octafluoro-1,6-hexanediol diacrylate was a fluorine-containing acrylate monomer, and trimethylolpropane triacrylate was a multifunctional acrylate crosslinking agent. After the second mixed solution was uniformly stirred, 0.026 g of azobisisobutyronitrile was added to the second mixed solution to form a third mixed solution, and azobisisobutyronitrile was used as an initiator. The third mixed solution was stirred for 30 minutes to obtain a precursor solution having a flame-retardant polymer solid electrolyte;
[0069] A soft-pack lithium-ion battery is assembled using graphite as the negative electrode of the lithium battery, high-voltage lithium cobalt oxide as the positive electrode of the lithium battery, and polypropylene as the separator. 5.000g of the precursor solution is weighed and injected into the lithium battery. After being placed at room temperature for 48 hours, a high-temperature static operation at 60°C for 8 hours is performed to obtain a high-voltage lithium battery with a flame-retardant polymer solid electrolyte.
[0070] Example 7 of the preparation method of the high voltage lithium battery is as follows:
[0071] Weigh 1.519 g of lithium hexafluorophosphate, where the lithium hexafluorophosphate is a lithium salt, and dissolve the 1.519 g of lithium hexafluorophosphate in 10 ml of a first mixed solution of fluoroethylene carbonate and 2,2,2-trifluoro-N,N-dimethylacetamide to form an electrolyte, where the fluoroethylene carbonate and 2,2,2-trifluoro-N,N-dimethylacetamide are plasticizers, wherein the mass ratio of the fluoroethylene carbonate to the 2,2,2-trifluoro-N,N-dimethylacetamide is 1:3;
[0072] 3.57244 g of electrolyte was taken, and 0.740 g of octafluoro-1,6-hexanediol diacrylate and 0.593 g of trimethylolpropane triacrylate were added to the 3.57244 g electrolyte, the stoichiometric ratio of octafluoro-1,6-hexanediol diacrylate was 2 mmol, and the stoichiometric ratio of trimethylolpropane triacrylate was 2 mmol, to form a second mixed solution, octafluoro-1,6-hexanediol diacrylate was a fluorine-containing acrylate monomer, and trimethylolpropane triacrylate was a multifunctional acrylate crosslinking agent. After the second mixed solution was uniformly stirred, 0.026 g of azobisisobutyronitrile was added to the second mixed solution to form a third mixed solution, and azobisisobutyronitrile was used as an initiator. The third mixed solution was stirred for 30 minutes to obtain a precursor solution having a flame-retardant polymer solid electrolyte;
[0073] A soft-pack lithium-ion battery is assembled using graphite as the negative electrode of the lithium battery, high-voltage lithium cobalt oxide as the positive electrode of the lithium battery, and polypropylene as the separator. 5.000g of the precursor solution is weighed and injected into the lithium battery. After being placed at room temperature for 48 hours, a high-temperature static operation at 60°C for 8 hours is performed to obtain a high-voltage lithium battery with a flame-retardant polymer solid electrolyte.
[0074] Example 8 of the preparation method of the high voltage lithium battery is as follows:
[0075] Weigh 1.519 g of lithium hexafluorophosphate, where the lithium hexafluorophosphate is a lithium salt, and dissolve the 1.519 g of lithium hexafluorophosphate in a first mixed solution of 10 ml of fluoroethylene carbonate and 2,2,2-trifluoro-N,N-dimethylacetamide to form an electrolyte, where the fluoroethylene carbonate and 2,2,2-trifluoro-N,N-dimethylacetamide are plasticizers, wherein the mass ratio of the fluoroethylene carbonate to the 2,2,2-trifluoro-N,N-dimethylacetamide is 1:3;
[0076] 2.666 g of electrolyte was taken, and 0.740 g of octafluoro-1,6-hexanediol diacrylate and 0.593 g of trimethylolpropane triacrylate were added to the 2.666 g electrolyte, the stoichiometric ratio of octafluoro-1,6-hexanediol diacrylate was 2 mmol, and the stoichiometric ratio of trimethylolpropane triacrylate was 2 mmol, to form a second mixed solution, octafluoro-1,6-hexanediol diacrylate was a fluorine-containing acrylate monomer, and trimethylolpropane triacrylate was a multifunctional acrylate crosslinking agent. After the second mixed solution was uniformly stirred, 0.026 g of azobisisobutyronitrile was added to the second mixed solution to form a third mixed solution, azobisisobutyronitrile was used as an initiator, and the third mixed solution was stirred for 30 minutes to obtain a precursor solution having a flame-retardant polymer solid electrolyte;
[0077] A soft-pack lithium-ion battery is assembled using graphite as the negative electrode of the lithium battery, high-voltage lithium cobalt oxide as the positive electrode of the lithium battery, and polypropylene as the separator. 5.000g of the precursor solution is weighed and injected into the lithium battery. After being placed at room temperature for 48 hours, a high-temperature static operation at 60°C for 8 hours is performed to obtain a high-voltage lithium battery with a flame-retardant polymer solid electrolyte.
[0078] Example 9 of the method for preparing the high voltage lithium battery is as follows:
[0079] Weigh 1.519 g of lithium hexafluorophosphate, where the lithium hexafluorophosphate is a lithium salt, and dissolve the 1.519 g of lithium hexafluorophosphate in 10 ml of a first mixed solution of fluoroethylene carbonate and 2,2,2-trifluoro-N,N-dimethylacetamide to form an electrolyte, where the fluoroethylene carbonate and 2,2,2-trifluoro-N,N-dimethylacetamide are plasticizers, wherein the mass ratio of the fluoroethylene carbonate to the 2,2,2-trifluoro-N,N-dimethylacetamide is 1:3;
[0080] 1.75956 g of electrolyte was taken, and 0.740 g of octafluoro-1,6-hexanediol diacrylate and 0.593 g of trimethylolpropane triacrylate were added to 1.7595 g of electrolyte, the stoichiometric ratio of octafluoro-1,6-hexanediol diacrylate was 2 mmol, and the stoichiometric ratio of trimethylolpropane triacrylate was 2 mmol, to form a second mixed solution, octafluoro-1,6-hexanediol diacrylate was a fluorine-containing acrylate monomer, and trimethylolpropane triacrylate was a multifunctional acrylate crosslinking agent. After the second mixed solution was uniformly stirred, 0.026 g of azobisisobutyronitrile was added to the second mixed solution to form a third mixed solution, and azobisisobutyronitrile was used as an initiator. The third mixed solution was stirred for 30 minutes to obtain a precursor solution having a flame-retardant polymer solid electrolyte;
[0081] A soft-pack lithium-ion battery is assembled using graphite as the negative electrode of the lithium battery, high-voltage lithium cobalt oxide as the positive electrode of the lithium battery, and polypropylene as the separator. 5.000g of the precursor solution is weighed and injected into the lithium battery. After being placed at room temperature for 48 hours, a high-temperature static operation at 60°C for 8 hours is performed to obtain a high-voltage lithium battery with a flame-retardant polymer solid electrolyte.
[0082] In Examples 6-9, the reaction process is the same as in Example 1, except that the mass fraction of the electrolyte formed by mixing the lithium salt and the plasticizer in the second mixed solution is changed, as shown in Table 2.
[0083] Table 2
[0084]
[0085]
[0086] The higher the limiting oxygen index, the better the flame retardant effect of the lithium battery; the higher the conductivity, the better the battery performance. The standard of the limiting oxygen index is set to 25. If the limiting oxygen index is greater than or equal to 25, it meets the standard of lithium battery flame retardancy. If the limiting oxygen index is less than 25, it does not meet the standard of lithium battery flame retardancy. In Table 2, Example 1, Example 7, Example 8 and Example 9 meet the standard of lithium battery flame retardancy. In addition, the conductivity of Example 1 is greater than the conductivity of Example 7, the conductivity of Example 1 is greater than the conductivity of Example 8, and the conductivity of Example 1 is greater than the conductivity of Example 9. The preparation method of Example 1 can make the battery performance better, and therefore, Example 1 is the best embodiment.
[0087] Embodiment 10 of the method for preparing the high voltage lithium battery is as follows:
[0088] Weigh 1.519 g of lithium hexafluorophosphate, where the lithium hexafluorophosphate is a lithium salt, and dissolve the 1.519 g of lithium hexafluorophosphate in 10 ml of a first mixed solution of fluoroethylene carbonate and 2,2,2-trifluoro-N,N-dimethylacetamide to form an electrolyte, where the fluoroethylene carbonate and 2,2,2-trifluoro-N,N-dimethylacetamide are plasticizers, wherein the mass ratio of the fluoroethylene carbonate to the 2,2,2-trifluoro-N,N-dimethylacetamide is 1:3;
[0089] 3.999 g of electrolyte is taken, and 0.740 g of octafluoro-1,6-hexanediol diacrylate and 0.593 g of trimethylolpropane triacrylate are added to the 3.999 g of electrolyte, the stoichiometric ratio of octafluoro-1,6-hexanediol diacrylate is 2 mmol, and the stoichiometric ratio of trimethylolpropane triacrylate is 2 mmol, to form a second mixed solution, and the mass fraction of the electrolyte in the second mixed solution is 75%, octafluoro-1,6-hexanediol diacrylate is a fluorine-containing acrylate monomer, and trimethylolpropane triacrylate is a multifunctional acrylate crosslinking agent. After the second mixed solution is uniformly stirred, 0.026 g of azobisisobutyronitrile is added to the second mixed solution to form a third mixed solution, and azobisisobutyronitrile is an initiator. The third mixed solution is stirred for 30 minutes to obtain a precursor solution having a flame-retardant polymer solid electrolyte;
[0090] A soft-pack lithium-ion battery is assembled using graphite as the negative electrode of the lithium battery, high-voltage lithium cobalt oxide as the positive electrode of the lithium battery, and polypropylene as the separator. 5.000g of the precursor solution is weighed and injected into the lithium battery. After being placed at room temperature for 48 hours, a high-temperature static operation at 40°C is performed for 8 hours to obtain a high-voltage lithium battery with a flame-retardant polymer solid electrolyte.
[0091] Example 11 of the method for preparing the high voltage lithium battery is as follows:
[0092] Weigh 1.519 g of lithium hexafluorophosphate, where the lithium hexafluorophosphate is a lithium salt, and dissolve the 1.519 g of lithium hexafluorophosphate in 10 ml of a first mixed solution of fluoroethylene carbonate and 2,2,2-trifluoro-N,N-dimethylacetamide to form an electrolyte, where the fluoroethylene carbonate and 2,2,2-trifluoro-N,N-dimethylacetamide are plasticizers, wherein the mass ratio of the fluoroethylene carbonate to the 2,2,2-trifluoro-N,N-dimethylacetamide is 1:3;
[0093] 3.999 g of electrolyte is taken, and 0.740 g of octafluoro-1,6-hexanediol diacrylate and 0.593 g of trimethylolpropane triacrylate are added to the 3.999 g of electrolyte, the stoichiometric ratio of octafluoro-1,6-hexanediol diacrylate is 2 mmol, and the stoichiometric ratio of trimethylolpropane triacrylate is 2 mmol, to form a second mixed solution, and the mass fraction of the electrolyte in the second mixed solution is 75%, octafluoro-1,6-hexanediol diacrylate is a fluorine-containing acrylate monomer, and trimethylolpropane triacrylate is a multifunctional acrylate crosslinking agent. After the second mixed solution is uniformly stirred, 0.026 g of azobisisobutyronitrile is added to the second mixed solution to form a third mixed solution, and azobisisobutyronitrile is an initiator. The third mixed solution is stirred for 30 minutes to obtain a precursor solution having a flame-retardant polymer solid electrolyte;
[0094] A soft-pack lithium-ion battery is assembled using graphite as the negative electrode of the lithium battery, high-voltage lithium cobalt oxide as the positive electrode of the lithium battery, and polypropylene as the separator. 5.000g of the precursor solution is weighed and injected into the lithium battery. After being placed at room temperature for 48 hours, a high-temperature static operation at 70°C is performed for 8 hours to obtain a high-voltage lithium battery with a flame-retardant polymer solid electrolyte.
[0095] Embodiment 12 of the method for preparing the high voltage lithium battery is as follows:
[0096] Weigh 1.519 g of lithium hexafluorophosphate, where the lithium hexafluorophosphate is a lithium salt, and dissolve the 1.519 g of lithium hexafluorophosphate in 10 ml of a first mixed solution of fluoroethylene carbonate and 2,2,2-trifluoro-N,N-dimethylacetamide to form an electrolyte, where the fluoroethylene carbonate and 2,2,2-trifluoro-N,N-dimethylacetamide are plasticizers, wherein the mass ratio of the fluoroethylene carbonate to the 2,2,2-trifluoro-N,N-dimethylacetamide is 1:3;
[0097] 3.999 g of electrolyte is taken, and 0.740 g of octafluoro-1,6-hexanediol diacrylate and 0.593 g of trimethylolpropane triacrylate are added to the 3.999 g of electrolyte, the stoichiometric ratio of octafluoro-1,6-hexanediol diacrylate is 2 mmol, and the stoichiometric ratio of trimethylolpropane triacrylate is 2 mmol, to form a second mixed solution, and the mass fraction of the electrolyte in the second mixed solution is 75%, octafluoro-1,6-hexanediol diacrylate is a fluorine-containing acrylate monomer, and trimethylolpropane triacrylate is a multifunctional acrylate crosslinking agent. After the second mixed solution is uniformly stirred, 0.026 g of azobisisobutyronitrile is added to the second mixed solution to form a third mixed solution, and azobisisobutyronitrile is an initiator. The third mixed solution is stirred for 30 minutes to obtain a precursor solution having a flame-retardant polymer solid electrolyte;
[0098] A soft-pack lithium-ion battery is assembled using graphite as the negative electrode of the lithium battery, high-voltage lithium cobalt oxide as the positive electrode of the lithium battery, and polypropylene as the separator. 5.000g of the precursor solution is weighed and injected into the lithium battery. After being placed at room temperature for 48 hours, a high-temperature static operation at 80°C is performed for 8 hours to obtain a high-voltage lithium battery with a flame-retardant polymer solid electrolyte.
[0099] Example 13 of the preparation method of the high voltage lithium battery is as follows,
[0100] Weigh 1.519 g of lithium hexafluorophosphate, where the lithium hexafluorophosphate is a lithium salt, and dissolve the 1.519 g of lithium hexafluorophosphate in a first mixed solution of 10 ml of fluoroethylene carbonate and 2,2,2-trifluoro-N,N-dimethylacetamide to form an electrolyte, where the fluoroethylene carbonate and 2,2,2-trifluoro-N,N-dimethylacetamide are plasticizers, wherein the mass ratio of the fluoroethylene carbonate to the 2,2,2-trifluoro-N,N-dimethylacetamide is 1:3;
[0101] 3.999 g of electrolyte is taken, and 0.740 g of octafluoro-1,6-hexanediol diacrylate and 0.593 g of trimethylolpropane triacrylate are added to the 3.999 g of electrolyte, the stoichiometric ratio of octafluoro-1,6-hexanediol diacrylate is 2 mmol, and the stoichiometric ratio of trimethylolpropane triacrylate is 2 mmol, to form a second mixed solution, and the mass fraction of the electrolyte in the second mixed solution is 75%, octafluoro-1,6-hexanediol diacrylate is a fluorine-containing acrylate monomer, and trimethylolpropane triacrylate is a multifunctional acrylate crosslinking agent. After the second mixed solution is uniformly stirred, 0.026 g of azobisisobutyronitrile is added to the second mixed solution to form a third mixed solution, and azobisisobutyronitrile is an initiator. The third mixed solution is stirred for 30 minutes to obtain a precursor solution having a flame-retardant polymer solid electrolyte;
[0102] A soft-pack lithium-ion battery is assembled using graphite as the negative electrode of the lithium battery, high-voltage lithium cobalt oxide as the positive electrode of the lithium battery, and polypropylene as the separator. 5.000g of the precursor solution is weighed and injected into the lithium battery. After being placed at room temperature for 48 hours, a high-temperature static operation of 100°C is performed for 8 hours to obtain a high-voltage lithium battery with a flame-retardant polymer solid electrolyte.
[0103] In Examples 10-13, the reaction process is the same as in Example 1, except that the temperature of the high temperature static state is changed, as shown in Table 3.
[0104] Table 3
[0105] Static temperature (℃) Conductivity (mS / cm) Limiting oxygen index Example 1 60 2.39 26 Example 10 40 3.85 20 Embodiment 11 70 2.15 26 Example 12 80 2.19 26 Embodiment 13 100 1.61 25
[0106] The higher the limiting oxygen index, the better the flame retardant effect of the lithium battery; the higher the conductivity, the better the battery performance. The standard of the limiting oxygen index is set to 25. If the limiting oxygen index is greater than or equal to 25, it meets the standard for lithium battery flame retardancy. If the limiting oxygen index is less than 25, it does not meet the standard for lithium battery flame retardancy. In Table 3, Example 1, Example 11, Example 12 and Example 13 meet the standard for lithium battery flame retardancy. In addition, the conductivity of Example 1 is greater than the conductivity of Example 11, the conductivity of Example 1 is greater than the conductivity of Example 12, and the conductivity of Example 1 is greater than the conductivity of Example 13. The preparation method of Example 1 can make the battery performance better, and therefore, Example 1 is the best embodiment.
[0107] Example 14 of the method for preparing the high voltage lithium battery is as follows:
[0108] Weigh 1.519 g of lithium hexafluorophosphate, where the lithium hexafluorophosphate is a lithium salt, and dissolve the 1.519 g of lithium hexafluorophosphate in a first mixed solution of 10 ml of fluoroethylene carbonate and 2,2,2-trifluoro-N,N-dimethylacetamide to form an electrolyte, where the fluoroethylene carbonate and 2,2,2-trifluoro-N,N-dimethylacetamide are plasticizers, wherein the mass ratio of the fluoroethylene carbonate to the 2,2,2-trifluoro-N,N-dimethylacetamide is 1:3;
[0109] 3.999 g of electrolyte is taken, and 0.740 g of octafluoro-1,6-hexanediol diacrylate and 0.593 g of trimethylolpropane triacrylate are added to the 3.999 g of electrolyte, the stoichiometric ratio of octafluoro-1,6-hexanediol diacrylate is 2 mmol, and the stoichiometric ratio of trimethylolpropane triacrylate is 2 mmol, to form a second mixed solution, and the mass fraction of the electrolyte in the second mixed solution is 75%, octafluoro-1,6-hexanediol diacrylate is a fluorine-containing acrylate monomer, and trimethylolpropane triacrylate is a multifunctional acrylate crosslinking agent. After the second mixed solution is uniformly stirred, 0.026 g of azobisisobutyronitrile is added to the second mixed solution to form a third mixed solution, and azobisisobutyronitrile is an initiator. The third mixed solution is stirred for 30 minutes to obtain a precursor solution having a flame-retardant polymer solid electrolyte;
[0110] A soft-pack lithium-ion battery is assembled using graphite as the negative electrode of the lithium battery, high-voltage lithium cobalt oxide as the positive electrode of the lithium battery, and polypropylene as the separator. 5.000g of the precursor solution is weighed and injected into the lithium battery. After being placed at room temperature for 48 hours, a high-temperature static operation at 60°C is performed for 6 hours to obtain a high-voltage lithium battery with a flame-retardant polymer solid electrolyte.
[0111] Example 15 of the method for preparing the high voltage lithium battery is as follows,
[0112] Weigh 1.519 g of lithium hexafluorophosphate, where the lithium hexafluorophosphate is a lithium salt, and dissolve the 1.519 g of lithium hexafluorophosphate in 10 ml of a first mixed solution of fluoroethylene carbonate and 2,2,2-trifluoro-N,N-dimethylacetamide to form an electrolyte, where the fluoroethylene carbonate and 2,2,2-trifluoro-N,N-dimethylacetamide are plasticizers, wherein the mass ratio of the fluoroethylene carbonate to the 2,2,2-trifluoro-N,N-dimethylacetamide is 1:3;
[0113] 3.999 g of electrolyte is taken, and 0.740 g of octafluoro-1,6-hexanediol diacrylate and 0.593 g of trimethylolpropane triacrylate are added to the 3.999 g of electrolyte, the stoichiometric ratio of octafluoro-1,6-hexanediol diacrylate is 2 mmol, and the stoichiometric ratio of trimethylolpropane triacrylate is 2 mmol, to form a second mixed solution, and the mass fraction of the electrolyte in the second mixed solution is 75%, octafluoro-1,6-hexanediol diacrylate is a fluorine-containing acrylate monomer, and trimethylolpropane triacrylate is a multifunctional acrylate crosslinking agent. After the second mixed solution is uniformly stirred, 0.026 g of azobisisobutyronitrile is added to the second mixed solution to form a third mixed solution, and azobisisobutyronitrile is an initiator. The third mixed solution is stirred for 30 minutes to obtain a precursor solution having a flame-retardant polymer solid electrolyte;
[0114] A soft-pack lithium-ion battery is assembled using graphite as the negative electrode of the lithium battery, high-voltage lithium cobalt oxide as the positive electrode of the lithium battery, and polypropylene as the separator. 5.000g of the precursor solution is weighed and injected into the lithium battery. After being placed at room temperature for 48 hours, a high-temperature static operation at 60°C for 10 hours is performed to obtain a high-voltage lithium battery with a flame-retardant polymer solid electrolyte.
[0115] Example 16 of the method for preparing the high voltage lithium battery is as follows:
[0116] Weigh 1.519 g of lithium hexafluorophosphate, where the lithium hexafluorophosphate is a lithium salt, and dissolve the 1.519 g of lithium hexafluorophosphate in a first mixed solution of 10 ml of fluoroethylene carbonate and 2,2,2-trifluoro-N,N-dimethylacetamide to form an electrolyte, where the fluoroethylene carbonate and 2,2,2-trifluoro-N,N-dimethylacetamide are plasticizers, wherein the mass ratio of the fluoroethylene carbonate to the 2,2,2-trifluoro-N,N-dimethylacetamide is 1:3;
[0117] 3.999 g of electrolyte is taken, and 0.740 g of octafluoro-1,6-hexanediol diacrylate and 0.593 g of trimethylolpropane triacrylate are added to the 3.999 g of electrolyte, the stoichiometric ratio of octafluoro-1,6-hexanediol diacrylate is 2 mmol, and the stoichiometric ratio of trimethylolpropane triacrylate is 2 mmol, to form a second mixed solution, and the mass fraction of the electrolyte in the second mixed solution is 75%, octafluoro-1,6-hexanediol diacrylate is a fluorine-containing acrylate monomer, and trimethylolpropane triacrylate is a multifunctional acrylate crosslinking agent. After the second mixed solution is uniformly stirred, 0.026 g of azobisisobutyronitrile is added to the second mixed solution to form a third mixed solution, and azobisisobutyronitrile is an initiator. The third mixed solution is stirred for 30 minutes to obtain a precursor solution having a flame-retardant polymer solid electrolyte;
[0118] A soft-pack lithium-ion battery is assembled using graphite as the negative electrode of the lithium battery, high-voltage lithium cobalt oxide as the positive electrode of the lithium battery, and polypropylene as the separator. 5.000g of the precursor solution is weighed and injected into the lithium battery. After being placed at room temperature for 48 hours, a high-temperature static operation at 60°C for 12 hours is performed to obtain a high-voltage lithium battery with a flame-retardant polymer solid electrolyte.
[0119] Example 17 of the method for preparing the high voltage lithium battery is as follows,
[0120] Weigh 1.519 g of lithium hexafluorophosphate, where the lithium hexafluorophosphate is a lithium salt, and dissolve the 1.519 g of lithium hexafluorophosphate in a first mixed solution of 10 ml of fluoroethylene carbonate and 2,2,2-trifluoro-N,N-dimethylacetamide to form an electrolyte, where the fluoroethylene carbonate and 2,2,2-trifluoro-N,N-dimethylacetamide are plasticizers, wherein the mass ratio of the fluoroethylene carbonate to the 2,2,2-trifluoro-N,N-dimethylacetamide is 1:3;
[0121] 3.999 g of electrolyte is taken, and 0.740 g of octafluoro-1,6-hexanediol diacrylate and 0.593 g of trimethylolpropane triacrylate are added to the 3.999 g of electrolyte, the stoichiometric ratio of octafluoro-1,6-hexanediol diacrylate is 2 mmol, and the stoichiometric ratio of trimethylolpropane triacrylate is 2 mmol, to form a second mixed solution, and the mass fraction of the electrolyte in the second mixed solution is 75%, octafluoro-1,6-hexanediol diacrylate is a fluorine-containing acrylate monomer, and trimethylolpropane triacrylate is a multifunctional acrylate crosslinking agent. After the second mixed solution is uniformly stirred, 0.026 g of azobisisobutyronitrile is added to the second mixed solution to form a third mixed solution, and azobisisobutyronitrile is an initiator. The third mixed solution is stirred for 30 minutes to obtain a precursor solution having a flame-retardant polymer solid electrolyte;
[0122] A soft-pack lithium-ion battery is assembled using graphite as the negative electrode of the lithium battery, high-voltage lithium cobalt oxide as the positive electrode of the lithium battery, and polypropylene as the separator. 5.000g of the precursor solution is weighed and injected into the lithium battery. After being placed at room temperature for 48 hours, a high-temperature static operation at 60°C for 24 hours is performed to obtain a high-voltage lithium battery with a flame-retardant polymer solid electrolyte.
[0123] In Examples 14-17, the reaction process is the same as in Example 1, except that the high temperature standing time is changed, as shown in Table 4.
[0124] Table 4
[0125] Standing time (h) Conductivity (mS / cm) Limiting oxygen index Example 1 8 2.39 26 Embodiment 14 6 2.67 22 Embodiment 15 10 2.30 26 Example 16 12 2.17 26 Embodiment 17 24 1.94 25
[0126] The higher the limiting oxygen index, the better the flame retardant effect of the lithium battery; the higher the conductivity, the better the battery performance. The standard of the limiting oxygen index is set to 25. If the limiting oxygen index is greater than or equal to 25, it meets the standard of lithium battery flame retardancy. If the limiting oxygen index is less than 25, it does not meet the standard of lithium battery flame retardancy. In Table 4, Example 1, Example 15, Example 16 and Example 17 meet the standard of lithium battery flame retardancy. In addition, the conductivity of Example 1 is greater than the conductivity of Example 15, the conductivity of Example 1 is greater than the conductivity of Example 16, and the conductivity of Example 1 is greater than the conductivity of Example 17. The preparation method of Example 1 can make the battery performance better, and therefore, Example 1 is the best embodiment.
[0127] Therefore, combining the above embodiments and the results of the circuit rate and limiting oxygen index in Table 1, Table 2, Table 3, and Table 4, it can be concluded that Embodiment 1 is the optimal embodiment.
[0128] The present invention also provides two comparative examples, wherein comparative example 1 is,
[0129] Weigh 1.519 g of lithium hexafluorophosphate, which is a lithium salt, and dissolve the 1.519 g of lithium hexafluorophosphate in 10 ml of a first mixed solution of ethylene carbonate, dimethyl carbonate, and ethyl methyl carbonate to form an electrolyte, wherein the ethylene carbonate, dimethyl carbonate, and ethyl methyl carbonate are plasticizers, wherein the volume ratio of the ethylene carbonate, dimethyl carbonate, and ethyl methyl carbonate is 1:1:1;
[0130] 3.999 g of electrolyte was taken, and 0.740 g of octafluoro-1,6-hexanediol diacrylate and 0.593 g of trimethylolpropane triacrylate were added to 3.999 g of electrolyte to form a second mixed solution, wherein octafluoro-1,6-diol diacrylate was a fluorine-containing acrylate monomer, and trimethylolpropane triacrylate was a multifunctional acrylate crosslinking agent. After the second mixed solution was uniformly stirred, 0.026 g of azobisisobutyronitrile was added to the second mixed solution to form a third mixed solution, wherein azobisisobutyronitrile was an initiator, and the third mixed solution was stirred for 30 minutes to obtain a precursor solution having a flame-retardant polymer solid electrolyte;
[0131] A soft-pack lithium-ion battery is assembled using graphite as the negative electrode of the lithium battery, high-voltage lithium cobalt oxide as the positive electrode of the lithium battery, and polypropylene as the separator. 5.000g of the precursor solution is weighed and injected into the lithium battery. After being placed at room temperature for 48 hours, a high-temperature static operation of 60°C is performed for 8 hours to obtain a high-voltage lithium battery with a flame-retardant polymer solid electrolyte.
[0132] The reaction process of Comparative Example 1 is the same as that of Example 1, except that the type of plasticizer is changed. Specifically, the plasticizer is changed to a mixed solution of ethylene carbonate, dimethyl carbonate, and ethyl methyl carbonate, wherein the volume ratio of the three is 1:1:1. The conductivity of the obtained electrolyte is 2.38 mS cm-1, and the limiting oxygen index is 16.
[0133] Comparative Example 2 is,
[0134] Weigh 1.519 g of lithium hexafluorophosphate, which is a lithium salt, and dissolve the 1.519 g of lithium hexafluorophosphate in a first mixed solution of 10 ml of fluoroethylene carbonate and 2,2,2-trifluoro-N,N-dimethylacetamide to form an electrolyte, wherein the fluoroethylene carbonate and 2,2,2-trifluoro-N,N-dimethylacetamide are plasticizers, wherein the mass ratio of the fluoroethylene carbonate to the 2,2,2-trifluoro-N,N-dimethylacetamide is 1:3;
[0135] 3.999 g of the electrolyte was taken, and 0.740 g of 1,6-hexanediol diacrylate and 0.593 g of trimethylolpropane triacrylate were added to 3.999 g of the electrolyte to form a second mixed solution, wherein 1,6-hexanediol diacrylate was a monomer, and trimethylolpropane triacrylate was a multifunctional acrylate crosslinker. After the second mixed solution was uniformly stirred, 0.026 g of azobisisobutyronitrile was added to the second mixed solution to form a third mixed solution, wherein azobisisobutyronitrile was an initiator, and the third mixed solution was stirred for 30 minutes to obtain a precursor solution having a flame-retardant polymer solid electrolyte;
[0136] A soft-pack lithium-ion battery is assembled using graphite as the negative electrode of the lithium battery, high-voltage lithium cobalt oxide as the positive electrode of the lithium battery, and polypropylene as the separator. 5.000g of the precursor solution is weighed and injected into the lithium battery. After being placed at room temperature for 48 hours, a high-temperature static operation of 60°C is performed for 8 hours to obtain a high-voltage lithium battery with a flame-retardant polymer solid electrolyte.
[0137] Comparative Example 2 The reaction process is the same as that of Example 1, except that the type of monomer is changed. Specifically, the monomer is changed to 1,6-hexanediol diacrylate. The conductivity of the obtained electrolyte is 2.21 mS cm-1, and the limiting oxygen index is 21.
[0138] From the measured limiting oxygen index, it can be seen that compared with Example 1, Comparative Examples 1 and 2 are flammable. The reason is that Comparative Example 1 contains a large amount of flammable solvent, and the fluorine atoms in the skeleton are difficult to play a flame retardant role. In Comparative Example 2, the skeleton does not contain fluorine, the fluorine content in the system is greatly reduced, and the flame retardant effect is weakened. Therefore, compared with Comparative Examples 1 and 2, Example 1 is still the best example.
[0139] The present invention provides a method for preparing a high-voltage lithium battery with a flame-retardant polymer solid electrolyte. In the electrolyte of the battery, the monomer contains a large amount of fluorine elements, so that the electrolyte has good flame retardancy. At the same time, the electrolyte of the battery contains a fluorine plasticizer, which optimizes the electrochemical properties of the electrolyte, so that the battery has good self-extinguishing properties, and improves the cycle stability of the high-voltage lithium battery with a flame-retardant polymer solid electrolyte. Therefore, the high-voltage lithium battery with a flame-retardant polymer solid electrolyte has a good flame retardant effect, which improves the safety of the battery. Moreover, the high-voltage lithium battery with a flame-retardant polymer solid electrolyte can also maintain good battery performance. The technical problem that the existing solid or liquid flame-retardant electrolyte has an adverse effect on battery performance is effectively solved. In addition, the electrolyte of the battery is generated in situ between the electrodes, reducing the solid / solid interface impedance and improving the cycle performance of the battery. In the present invention, the electrolyte can form a stable passivation film on the surface of the positive and negative electrodes, effectively improving the stability of the positive and negative electrode materials and the positive and negative electrode interfaces, and thus optimizing the cycle stability of the battery. The capacity retention rate of the LCO / Gr battery with a flame-retardant polymer solid electrolyte after 250 cycles at a rate of 0.5C is 96.8%, wherein the LCO / Gr battery is a lithium cobalt oxide battery. The preparation of the battery with a flame-retardant polymer solid electrolyte is based on an in-situ free radical polymerization mechanism, without the need to prepare an electrolyte membrane separately, and has a fast reaction rate and no by-products, and is suitable for industrial production.
[0140] In summary, although the present invention has been disclosed as above in terms of preferred embodiments, the above preferred embodiments are not intended to limit the present invention. A person skilled in the art may make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention shall be based on the scope defined in the claims.
Claims
1. A method for preparing a high voltage lithium battery with a flame retardant polymer solid electrolyte, characterized in that: It includes the following steps: S1: using lithium salt as solute and plasticizer as solvent to prepare a solution of preset concentration, wherein the preset concentration is the molar concentration of the lithium salt in the plasticizer of 0.8 mol / L-2 mol / L; S2: adding a fluorinated acrylate monomer and a multifunctional acrylate crosslinking agent to the solution obtained in step S1 according to a set stoichiometric ratio to obtain a mixed solution, and then adding an initiator, and mixing them evenly to obtain a precursor solution; wherein the stoichiometric ratio of the fluorinated acrylate monomer to the multifunctional acrylate crosslinking agent is in the range of 1:1-1:3, and the total mass of the fluorinated acrylate monomer and the multifunctional acrylate crosslinking agent in the mixed solution is 20-90% by mass; the mass of the initiator is 1-10% of the total mass of the fluorinated acrylate monomer and the multifunctional acrylate crosslinking agent; S3: Assembling a lithium battery with a negative electrode of a lithium battery, a positive electrode of a lithium battery and a separator; S4: injecting the precursor solution obtained in step S2 into the lithium battery, leaving it at room temperature for 48 hours, and then subjecting the precursor solution to a high-temperature standing operation in the temperature range of 50-100° C., and obtaining a lithium battery with a flame-retardant polymer solid electrolyte after leaving it at high temperature for 4-24 hours.
2. The method for preparing a high voltage lithium battery with a flame retardant polymer solid electrolyte according to claim 1, characterized in that: In the step S2, the mass fraction of the total mass of the fluorine-containing acrylate monomer and the multifunctional acrylate cross-linking agent in the solution is 50-75%.
3. The method for preparing a high voltage lithium battery with a flame retardant polymer solid electrolyte according to claim 1, characterized in that: In the step S4, the injection amount of the precursor solution is determined by the battery capacity of the lithium battery, the injection amount of the precursor solution is 2-6 g / Ah, the high temperature standing temperature is 60-80° C., and the high temperature standing time is 8-12 hours.
4. The method for preparing a high voltage lithium battery with a flame retardant polymer solid electrolyte according to claim 1, characterized in that: The fluorine-containing acrylate monomer is composed of one or more combinations of octafluoro-1,6-hexanediol diacrylate, 2,2,3,3,4,4,5,5-octafluoro-1,6-dimethylacrylate, 2,2,3,3,4,4-hexafluoro-1,5-pentyl diacrylate, and 1,1'-(2,2,3,3,4,4-hexafluoro-1,5-pentanediyl)bis(2-methyl-2-acrylate).
5. The method for preparing a high voltage lithium battery with a flame retardant polymer solid electrolyte according to claim 1, characterized in that: The multifunctional acrylate crosslinking agent is composed of one or more combinations of trimethylolpropane triacrylate, ethoxylated trimethylolpropane triacrylate, pentaerythritol tetraacrylate and polydipentaerythritol hexaacrylate.
6. The method for preparing a high voltage lithium battery with a flame retardant polymer solid electrolyte according to claim 1, characterized in that: The initiator is composed of one or more combinations of azobisisobutyronitrile, azobisisoheptylnitrile, dibenzoyl peroxide, dodecyl peroxide, diethylhexyl peroxydicarbonate, and tert-butyl peroxyvalerate.
7. The method for preparing a high voltage lithium battery with a flame retardant polymer solid electrolyte according to claim 1, characterized in that: The plasticizer is composed of one or more combinations of fluoroethylene carbonate, 2,2,2-trifluoro-N,N-dimethylacetamide, methyl trifluoroethyl carbonate, ethyl trifluoroethyl carbonate, 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether, and 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether.
8. The method for preparing a high voltage lithium battery with a flame retardant polymer solid electrolyte according to claim 1, characterized in that: The lithium salt is composed of one or more combinations of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium hexafluoroarsenate, lithium difluorooxalatoborate, lithium perchlorate, lithium bisoxalatoborate, lithium trichloromethylsulfonate, lithium bistrifluoromethylsulfonyl imide, and lithium bisfluorosulfonyl imide.
9. The method for preparing a high voltage lithium battery with a flame retardant polymer solid electrolyte according to claim 1, characterized in that: The negative electrode of the lithium battery is any one of graphite, soft carbon, hard carbon, silicon, and lithium metal; the positive electrode of the lithium battery is any one of nickel-cobalt-manganese ternary material, nickel-cobalt-aluminum ternary material, lithium cobalt oxide, and lithium manganese oxide; the diaphragm is any one of polyethylene diaphragm, polypropylene diaphragm, polyimide diaphragm, cellulose diaphragm, glass fiber diaphragm, polyethylene terephthalate diaphragm, and non-woven fabric diaphragm.
10. A method for preparing a high voltage lithium battery, characterized in that: These include, Weigh 1.519 g of lithium hexafluorophosphate, where the lithium hexafluorophosphate is a lithium salt, and dissolve the 1.519 g of lithium hexafluorophosphate in 10 ml of a first mixed solution of fluoroethylene carbonate and 2,2,2-trifluoro-N,N-dimethylacetamide to form an electrolyte, where the fluoroethylene carbonate and 2,2,2-trifluoro-N,N-dimethylacetamide are plasticizers, wherein the mass ratio of the fluoroethylene carbonate to the 2,2,2-trifluoro-N,N-dimethylacetamide is 1:3; Take 3.999g of the electrolyte, add 0.740g of octafluoro-1,6-hexanediol diacrylate and 0.593g of trimethylolpropane triacrylate to 3.999g of the electrolyte, the stoichiometric number of octafluoro-1,6-hexanediol diacrylate is 2mmol, and the stoichiometric number of trimethylolpropane triacrylate is 2mmol, to form a second mixed solution, and the mass fraction of the electrolyte in the second mixed solution is 75%, octafluoro-1,6-hexanediol diacrylate is a fluorine-containing acrylate monomer, and trimethylolpropane triacrylate is a multifunctional acrylate crosslinking agent. After the second mixed solution is uniformly stirred, 0.026g of azobisisobutyronitrile is added to the second mixed solution to form a third mixed solution, azobisisobutyronitrile is an initiator, and the third mixed solution is stirred for 30 minutes to obtain a precursor solution having a flame-retardant polymer solid electrolyte; A soft-pack lithium-ion battery is assembled using graphite as the negative electrode of the lithium battery, high-voltage lithium cobalt oxide as the positive electrode of the lithium battery, and polypropylene as the separator, and 5.000g of the precursor solution is weighed and injected into the lithium battery; after being left at room temperature for 48 hours, a high-temperature static operation at 60°C is performed for 8 hours, thereby obtaining a high-voltage lithium battery with a flame-retardant polymer solid electrolyte.
Citation Information
Patent Citations
High-safety solid-state electrolyte, preparation method and application thereof
CN111969245A
Flame-retardant flexible composite gel electrolyte material and preparation method and application thereof
CN115207461A
Carbon dioxide-based poly-cyclic carbonate electrolyte as well as preparation method and application thereof
CN116979140A
Elastic flame-retardant gel polymer electrolyte, preparation method thereof and lithium battery
CN118472371A
Wide-temperature-range solid electrolyte, preparation method and application of wide-temperature-range solid electrolyte in solid-state lithium metal battery
CN118610568A
Cited By
In-situ cross-linked flame-retardant polymer electrolyte and precursor solution and battery thereof
CN121149395A
In-situ crosslinking flame-retardant polymer electrolyte, precursor liquid thereof and battery
CN121149395B