Ultrahigh molecular weight polyolefin diaphragm and preparation method thereof
By using ultra-high molecular weight polyethylene and micron- or sub-micron-scale sodium chloride particles in lithium-ion battery separators, combined with the process of first extraction and then stretching, the separator electrolyte infiltrates slowly and the ionic conductivity is low in the prior art. The problem has achieved efficient lithium ion transmission and improved battery safety performance.
Patent Information
- Application Number
- CN202411181336.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-27
AI Technical Summary
While the existing lithium-ion battery separators improve the electrolyte infiltration rate and ionic conductivity, it is difficult to take into account safety performance, especially in the fast charging process, which is likely to lead to the risk of battery short circuit.
Upper high molecular weight polyethylene diaphragm and its preparation method are adopted. By introducing micron- or sub-micron-scale sodium chloride particles into the diaphragm, and using a special process of extraction and then stretching, the median pore size and maximum pore size of the diaphragm are controlled. , ensure high ionic conductivity and good safety performance.
It achieves a balance of high ion conductivity and safety performance in lithium-ion battery separators, avoids the risk of battery short circuits, and meets the demand for lithium-ion passing rate in the fast charging industry.
Smart Images

Figure CN119050601A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of lithium-ion battery materials, and in particular to an ultra-high molecular weight polyolefin diaphragm and a preparation method thereof. Background Art
[0002] As a porous and highly functional material, lithium-ion battery separators not only transmit lithium ions, but also isolate positive and negative electrodes to avoid direct contact between positive and negative electrode materials and cause short circuits. As a channel for lithium ion transmission in the battery, lithium-ion battery separators are crucial to the speed of lithium ion transmission and diffusion. The quality of their performance plays a key role in the characteristics of the battery. The better the electrolyte infiltration ability of the separator, the higher the ion conductivity, which is more conducive to the transmission of lithium ions in the separator, increases the ion conduction efficiency, and is conducive to rapid charging and discharging of the battery.
[0003] At present, there are two main means to improve the electrolyte infiltration speed and ion conductivity of the diaphragm. One is to improve the pore structure of the base membrane, increase the porosity of the base membrane, reduce the tortuosity and increase the through holes. The larger the porosity, the more pores in the diaphragm, and the easier it is for lithium ions to migrate. The smaller the tortuosity and the more through holes, the shorter the lithium ion transmission path and the faster the migration speed. However, the large number of holes and the increase in through holes will lead to a decrease in the strength of the diaphragm. During the preparation process, the risk of the diaphragm being pierced by foreign objects and causing a short circuit will increase. The second is to coat and modify the surface of the base membrane. Common coatings include inorganic coatings such as alumina or boehmite, and organic coatings such as PVDF. Although traditional coating modifications can improve the liquid absorption and liquid retention capabilities to a certain extent, there are still problems with slow electrolyte infiltration and low ion conductivity.
[0004] The median pore size of ordinary lithium battery wet-process diaphragms is generally between 30nm and 40nm, which cannot meet the fast charging industry's requirements for lithium ion pass rate. The current fast charging diaphragm process is generally a non-woven fabric process, which can indeed meet high lithium ion pass rate, but it is very dangerous and can easily cause battery short circuits. Therefore, how to simultaneously have high ionic conductivity and high safety performance is a key issue that needs to be solved. Summary of the invention
[0005] Therefore, the main purpose of the present application is to provide an ultra-high molecular weight polyolefin membrane and a preparation method thereof, so as to further optimize the above-mentioned problems.
[0006] In order to solve the above technical problems, the purpose of the present application is to provide an ultra-high molecular weight polyolefin membrane, characterized in that it includes ultra-high molecular weight polyethylene, the average molecular weight of the ultra-high molecular weight polyethylene is ≥1 million, wherein the median pore size of the ultra-high molecular weight polyolefin membrane is 0.04μm~1μm, the maximum pore size does not exceed 1.2μm, and the puncture strength is ≥50gf.
[0007] The ultra-high molecular weight polyolefin separator as described above, wherein the average molecular weight of the ultra-high molecular weight polyethylene is 1 million to 1.5 million.
[0008] The ultra-high molecular weight polyolefin separator as described above, wherein the thickness of the ultra-high molecular weight polyolefin separator is 7 μm to 15 μm.
[0009] The ultra-high molecular weight polyolefin membrane as described above, wherein the ionic conductivity of the ultra-high molecular weight polyolefin membrane is ≥1.8 mS / cm.
[0010] Another object of the present application is to provide a method for preparing an ultra-high molecular weight polyolefin diaphragm, characterized in that it comprises the following steps: a step of preparing micron- or submicron-sized sodium chloride particles: adding balls to sodium chloride for ball milling, sieving and drying after grinding, then adding white oil for further grinding, and then obtaining micron- or submicron-sized sodium chloride particles; a step of mixing raw materials: selecting ultra-high molecular weight polyethylene and the micron- or submicron-sized sodium chloride particles and mixing them in white oil, and fully stirring them with a stirrer to form a premixed raw material, wherein the average molecular weight of the ultra-high molecular weight polyethylene is ≥1 million, and the content of the white oil is greater than that of the ultra-high molecular weight polyethylene, and the The content of ultra-high molecular weight polyethylene is greater than the micron-level or submicron-level sodium chloride particles; an extrusion molding step: adding the premixed raw material into an extruder, followed by extrusion molding to form a cast sheet; an extraction step: firstly placing the cast sheet obtained by extrusion molding in a mixture of acetone and water for extraction, and then performing ultrasound to simultaneously clean the sodium chloride and part of the white oil in the pores, and then using pure water to clean the acetone remaining on the surface, wiping it dry and placing it in pure dichloromethane for re-extraction to form an extracted raw material; and a stretching step: then placing the extracted raw material obtained by extrusion molding in a handkerchief machine for stretching, and obtaining the ultra-high molecular weight polyolefin diaphragm after stretching.
[0011] The preparation method of the ultra-high molecular weight polyolefin diaphragm as described above, wherein, in the step of preparing the micron-sized or submicron-sized sodium chloride particles, zirconium beads mixed from at least three different sizes are added to ordinary industrial-grade sodium chloride, which are sieved and dried after grinding, and then white oil is added to continue grinding. The addition of white oil can ensure that the sodium chloride does not absorb water. After grinding, micron-sized or submicron-sized sodium chloride particles are obtained, wherein the ordinary industrial-grade sodium chloride is industrial salt with a sodium chloride purity of more than 99% and a particle size of 0.5 mm to 2 mm, and the maximum size diameter of the zirconium beads does not exceed 1 mm.
[0012] In the method for preparing the ultra-high molecular weight polyolefin diaphragm as described above, the diameter of the micron-sized or submicron-sized sodium chloride particles is between 0.1 μm and 1 μm.
[0013] The method for preparing an ultra-high molecular weight polyolefin diaphragm as described above, wherein, in the raw material mixing step, based on the total weight of the premixed raw materials, the weight proportion of the micron or submicron sodium chloride particles is 1wt% to 20wt%, the weight proportion of the ultra-high molecular weight polyethylene content is 1wt% to 29wt%, and the weight proportion of the white oil is 60wt% to 80wt%.
[0014] In the method for preparing the ultra-high molecular weight polyolefin separator as described above, the average molecular weight of the ultra-high molecular weight polyethylene is 1 million to 1.5 million.
[0015] The method for preparing an ultra-high molecular weight polyolefin diaphragm as described above, wherein, in the step of preparing the micron-sized or submicron-sized sodium chloride particles, the micron-sized or submicron-sized sodium chloride particles include spheres, quasi-spherical shapes or irregular spheres, and their particle size distribution is approximately normal distribution, wherein 80% of the sodium chloride particles are quasi-spherical.
[0016] The present application introduces micron or submicron sodium chloride particles during the membrane production process, controls the membrane to achieve a better median pore size and maximum pore size by limiting the content of the sodium chloride particles and their particle size distribution, and adopts a special process of first extraction and then stretching to make the pore size appropriate, neither too large nor too small, so that the obtained ultra-high molecular weight polyolefin membrane has both high safety performance and ionic conductivity. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 The present invention is a schematic block diagram of a process for preparing an ultra-high molecular weight polyolefin membrane according to an embodiment of the present invention. DETAILED DESCRIPTION
[0018] In order to further explain the technical means and effects adopted by the present application to achieve the predetermined invention purpose, the following, in combination with the accompanying drawings and specific embodiments, describes in detail an ultra-high molecular weight polyolefin diaphragm and a preparation method thereof proposed in the present application, as well as its specific implementation method, structure, characteristics and effects.
[0019] An ultra-high molecular weight polyolefin membrane according to an embodiment of the present application is characterized in that it comprises ultra-high molecular weight polyethylene, the average molecular weight of the ultra-high molecular weight polyethylene is ≥ 1 million, wherein the median pore size of the ultra-high molecular weight polyolefin membrane is 0.04 μm to 1 μm, the maximum pore size does not exceed 1.2 μm, and the puncture strength is ≥ 50 gf.
[0020] In some embodiments, the average molecular weight of the ultra-high molecular weight polyethylene is 1 million to 1.5 million. In some embodiments, in addition to ultra-high molecular weight polyethylene, the ultra-high molecular weight polyolefin membrane can also use high-density polyethylene, high molecular weight polyethylene or ultra-high molecular weight polyethylene grafted material. Under conditions other than ultra-high molecular weight polyethylene, based on the total weight of the ultra-high molecular weight polyolefin membrane, the ultra-high molecular weight polyethylene accounts for at least greater than 80wt%. In some embodiments, the median pore size of the ultra-high molecular weight polyolefin membrane is 0.04μm to 0.5μm, preferably 0.04μm, 0.05μm, 0.1μm, or 0.5μm. In some embodiments, the maximum pore size of the ultra-high molecular weight polyolefin membrane is 0.11μm to 1.2μm, preferably 0.11μm, 0.15μm, 0.25μm, or 1.2μm. In some embodiments, the puncture strength of the ultra-high molecular weight polyolefin separator is 50 gf to 150 gf, preferably 50 gf, 80 gf, 90 gf, or 150 gf.
[0021] In some embodiments, by limiting the thickness of the ultra-high molecular weight polyolefin separator to 15 μm, the median pore size to 100 nm, and the maximum pore size to 0.25 μm, the battery safety, that is, the thickness is guaranteed, and a higher ionic conductivity can be obtained, because the ion passing rate is directly determined by the pore size, and a larger pore size of 1 μm can obtain a higher ionic conductivity of ≥3 mS / cm. In other embodiments, the thickness of the ultra-high molecular weight polyolefin separator is 7 μm to 15 μm, preferably 7 μm, 9 μm, 12 μm, or 15 μm, and the ionic conductivity is ≥1.8 mS / cm, preferably 1.8 mS / cm, 2.1 mS / cm, 3 mS / cm, or 4.8 mS / cm.
[0022] See also Figure 1In another embodiment, the present application provides a method 1 for preparing an ultra-high molecular weight polyolefin diaphragm, characterized in that it comprises the following steps: a step S11 for preparing micron- or submicron-sized sodium chloride particles: adding balls to sodium chloride for ball milling, sieving and drying after grinding, then adding white oil for further grinding, and then obtaining micron- or submicron-sized sodium chloride particles; a raw material mixing step S12: selecting ultra-high molecular weight polyethylene and the micron- or submicron-sized sodium chloride particles and mixing them in white oil, and stirring them fully with a stirrer to form a premixed raw material, wherein the average molecular weight of the ultra-high molecular weight polyethylene is ≥1 million, and the content of the white oil is greater than that of the ultra-high molecular weight polyethylene, and the ultra-high molecular weight polyethylene is ≥1 million. The content of high molecular weight polyethylene is greater than the micron or submicron sodium chloride particles; an extrusion molding step S13: adding the premixed raw material into an extruder, followed by extrusion molding to form a cast sheet; an extraction step S14: firstly extracting the cast sheet obtained by extrusion molding in a mixture of acetone and water, then performing ultrasound to clean the sodium chloride and part of the white oil in the pores, then cleaning the residual acetone on the surface with pure water, wiping it dry and then placing it in pure dichloromethane for re-extraction to form an extracted raw material; and a stretching step S15: then placing the extracted raw material obtained by extrusion molding in a handkerchief machine for stretching, and obtaining the ultra-high molecular weight polyolefin diaphragm after stretching.
[0023] In some embodiments, in the step S11 of preparing the micron or submicron sodium chloride particles, zirconium beads of three sizes, large, medium and small, are mixed and added to ordinary industrial-grade sodium chloride. After grinding for 4 hours, the beads are opened and sieved, and then dried for 1 hour after sieving. Then white oil is added and grinding is continued. The addition of white oil can ensure that the sodium chloride does not absorb water. After grinding for 4 hours, uniform micron or submicron sodium chloride particles are obtained. The ordinary industrial-grade sodium chloride is industrial salt with a sodium chloride purity of more than 99% and a particle size of 0.5mm to 2mm (millimeter). The diameter of the small-sized zirconium beads is 0.2mm, the diameter of the medium-sized zirconium beads is 0.5mm, and the diameter of the large-sized zirconium beads is 1mm. Therefore, the maximum size diameter of the zirconium beads described in the embodiment does not exceed 1mm.
[0024] However, it is not limited to this. In other embodiments, the zirconium beads can be replaced with other grinding equipment, and ordinary industrial-grade sodium chloride can be ground so that the maximum particle size of the sodium chloride particles reaches 1μm (micrometer) and can be applied to the present invention. In the micron-level or submicron-level sodium chloride particle preparation step S11, the micron-level or submicron-level sodium chloride particles include spherical, quasi-spherical or irregular spherical shapes, and their particle size distribution is similar to a normal distribution, wherein 80% of the sodium chloride particles are quasi-spherical. It is understandable that the shape and particle size distribution of such sodium chloride particles will be conducive to forming the size distribution and shape of the pore size of the ultra-high molecular weight polyolefin diaphragm.
[0025] In some embodiments, in the raw material mixing step S12, ultra-high molecular weight polyethylene is selected and mixed with the previously prepared micron or submicron sodium chloride particles in white oil, and is fully stirred with a mixer to form a premixed raw material, wherein the average molecular weight of the ultra-high molecular weight polyethylene is 1 million to 1.5 million, and based on the total weight of the premixed raw material, the micron or submicron sodium chloride particles account for 10wt%, the ultra-high molecular weight polyethylene accounts for 20wt%, and the white oil accounts for 70wt%, and the diameter of the micron or submicron sodium chloride particles is between 0.1μm and 1μm. However, it is not limited thereto. In other embodiments, based on the total weight of the premixed raw materials, the micron or submicron sodium chloride particles preferably account for 1wt% to 20wt%, more preferably in the range between any two values of 1wt%, 10wt%, and 20wt%, the ultra-high molecular weight polyethylene accounts for 1wt% to 29wt%, more preferably in the range between any two values of 1wt%, 16wt%, 18wt%, 19.8wt%, and 29wt%, the white oil accounts for 60wt% to 80wt%, more preferably 60wt%, 64wt%, 72wt%. In the range between any two values of %, 79.2wt%, and 80wt%, preferably, the micron or submicron sodium chloride particles account for 1wt%, the ultra-high molecular weight polyethylene accounts for 19.8wt%, and the white oil accounts for 79.2wt%, preferably, the micron or submicron sodium chloride particles account for 10wt%, the ultra-high molecular weight polyethylene accounts for 18wt%, and the white oil accounts for 72wt%, preferably, the micron or submicron sodium chloride particles account for 20wt%, the ultra-high molecular weight polyethylene accounts for 16wt%, and the white oil accounts for 64wt%.
[0026] In this embodiment, in the extrusion molding step S13, a mixture of 10% micron or submicron sodium chloride particles, 20% ultra-high molecular weight polyethylene, and 70% white oil is added to the extruder and extruded to form a uniform casting. In the extraction step S14, the casting obtained by extrusion molding is first placed in a blend of acetone and water for extraction, and then ultrasonically cleaned to remove the sodium chloride and part of the white oil in the pores, and then the residual acetone on the surface is cleaned with pure water, and after drying, it is placed in pure dichloromethane for re-extraction.
[0027] It is worth mentioning that this embodiment adopts a special process of first extracting and then stretching, wherein the first extraction step is to remove pore-forming agents such as white oil and sodium chloride, at which time the pores will shrink, and then the temperature recovery stretching can ensure that the pores are expanded to an appropriate size, not too large or too small. On the contrary, if the process of first stretching and then extracting is adopted, due to the presence of pore-forming agents, the size of the pores in the stretching process is relatively fixed after the initial casting, and there is only a small expansion in the stretching process, so this process cannot really effectively expand the pores.
[0028] In the invention, some parameters are designed to conduct experiments, and the experimental process and results are summarized as follows.
[0029] Example 1
[0030] The fast-charging diaphragm of this embodiment, the particle size of the micron-level or submicron-level sodium chloride is 100nm, and the preparation steps of the fast-charging diaphragm are as follows: ultra-high molecular weight polyethylene powder and white oil are mixed at a mass ratio of 2:8, and then further mixed with sodium chloride particles to form a premixed raw material, the weight proportion of the sodium chloride particles in the premixed raw material is 1%, and the rest is ultra-high molecular weight polyethylene powder and white oil mixed at a mass ratio of 2:8, melt-mixed by a twin-screw extruder, cooled, extracted, and stretched to form the ultra-high molecular weight polyolefin diaphragm. The stretching condition is 10*10.
[0031] Example 2
[0032] The fast-charging diaphragm of this embodiment is the same as that of Embodiment 1 except that the weight percentage of the sodium chloride content is 5%.
[0033] Example 3
[0034] The fast-charging diaphragm of this embodiment has a particle size of 100nm for the micron- or submicron-sized sodium chloride. The preparation steps of the fast-charging diaphragm are as follows: After the ultra-high molecular weight polyethylene powder and white oil are mixed at a mass ratio of 2:8, they are further mixed with sodium chloride particles to form a premixed raw material. The weight proportion of the sodium chloride particles in the premixed raw material is 10%, and the rest is ultra-high molecular weight polyethylene powder and white oil mixed at a mass ratio of 2:8. They are melt-mixed by a twin-screw extruder, cooled, extracted, and stretched to form the ultra-high molecular weight polyolefin diaphragm. The stretching condition is 6.5*6.5.
[0035] Example 4
[0036] The fast-charging diaphragm of this embodiment is the same as that of Embodiment 3 except that the weight percentage of the sodium chloride content is 20%.
[0037] Comparative Example 1
[0038] Ultra-high molecular weight polyethylene powder and white oil are melt-mixed in a mass ratio of 3:7 through a twin-screw extruder, and then cooled, stretched and extracted to form a polyethylene-based film.
[0039] Comparative Example 2
[0040] After ultra-high molecular weight polyethylene powder and white oil are mixed in a mass ratio of 2:8, they are further mixed with sodium chloride particles to form a premixed raw material, in which the weight proportion of sodium chloride particles in the premixed raw material is 10%, and the rest is ultra-high molecular weight polyethylene powder and white oil mixed in a mass ratio of 2:8. The premixed raw material is melt-mixed through a twin-screw extruder, and is cooled, stretched, and extracted to form a polyethylene-based film.
[0041] Comparative Example 3
[0042] Ultra-high molecular weight polyethylene powder and white oil are melt-mixed in a mass ratio of 3:7 through a twin-screw extruder, and then cooled, extracted, and stretched to form a polyethylene-based film.
[0043]
[0044]
[0045] The above experimental results are summarized as shown in Table 1. From the results in Table 1, it can be seen that in Examples 1, 2, 3, and 4, the content of sodium chloride mainly affects the size of the median pore size and the uniformity of the pore size distribution. It can be seen from Example 4 that when the sodium chloride content is 20%, the maximum pore size is above 1000nm, and the safety performance cannot be guaranteed. After the solid content increases and the stretching ratio is 10*10, the thickness tends to decrease; Comparative Examples 1 and 2 adopt a general stretching process, that is, stretching first and then extracting, but this process has a smaller pore size and a smaller ionic conductivity than before, and the battery cannot be fast charged. Comparative Example 3 adopts extraction first and then stretching, and the pore size distribution is uneven and the strength is not very high.
[0046] In summary, in order to improve the safety performance of the current common lithium battery wet-process diaphragms, the present invention proposes an ultra-high molecular weight polyolefin fast-charging diaphragm, which is prepared by a specific process using a sodium chloride raw material with a limited particle size range, different diaphragm preparation processes, different extraction times, specific extractants and detailed steps to obtain a fast-charging diaphragm with a larger median pore size of 0.04μm to 1μm. This fast-charging diaphragm has a higher ionic conductivity and can provide higher safety performance. Therefore, this case can actually solve the problem that the diaphragm in the prior art cannot have both fast charging and high safety at the same time.
[0047] The above description is only an embodiment of the present application and does not constitute any form of limitation to the present application. Although the present application has been disclosed as above with specific embodiments, it is not intended to limit the present application. Any technician familiar with the profession can make slight changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present application. However, any simple modification, equivalent changes and modifications made to the above embodiments based on the technical essence of the present application without departing from the content of the technical solution of the present application are still within the scope of the technical solution of the present application.
Claims
1. An ultra-high molecular weight polyolefin diaphragm, characterized in that: It comprises ultra-high molecular weight polyethylene, the average molecular weight of the ultra-high molecular weight polyethylene is ≥ 1 million, wherein the median pore size of the ultra-high molecular weight polyolefin diaphragm is 0.04 μm to 1 μm, the maximum pore size does not exceed 1.2 μm, and the puncture strength is ≥ 50 gf.
2. The ultra-high molecular weight polyolefin membrane according to claim 1, characterized in that: The average molecular weight of the ultra-high molecular weight polyethylene is 1 million to 1.5 million.
3. The ultra-high molecular weight polyolefin membrane according to claim 1, characterized in that: The thickness of the ultra-high molecular weight polyolefin separator is 7 μm to 15 μm.
4. The ultra-high molecular weight polyolefin membrane according to claim 1, characterized in that: The ionic conductivity of the ultra-high molecular weight polyolefin membrane is ≥1.8 mS / cm.
5. A method for preparing an ultra-high molecular weight polyolefin diaphragm, characterized in that: The following steps are involved: The steps of preparing micron or submicron sodium chloride particles are as follows: adding ball beads to sodium chloride for ball milling, sieving and drying after grinding, then adding white oil for further grinding, and then obtaining micron or submicron sodium chloride particles; A raw material mixing step: selecting ultra-high molecular weight polyethylene and the micron-sized or submicron-sized sodium chloride particles and mixing them in white oil, and fully stirring them with a stirrer to form a premixed raw material, wherein the average molecular weight of the ultra-high molecular weight polyethylene is ≥ 1 million, and the content of the white oil is greater than that of the ultra-high molecular weight polyethylene, and the content of the ultra-high molecular weight polyethylene is greater than that of the micron-sized or submicron-sized sodium chloride particles; An extrusion molding step: adding the premixed raw material into an extruder, followed by extrusion molding to form a cast sheet; An extraction step: the cast sheet obtained by extrusion molding is first placed in a mixture of acetone and water for extraction, and then subjected to ultrasound to clean the sodium chloride and part of the white oil in the pores, and then the residual acetone on the surface is cleaned with pure water, and then dried and placed in pure dichloromethane for re-extraction to form an extracted raw material; as well as A stretching step: the extracted raw material obtained by extrusion molding is then placed in a handkerchief machine for stretching, and the ultra-high molecular weight polyolefin diaphragm is obtained after stretching.
6. The method for preparing an ultra-high molecular weight polyolefin membrane according to claim 5, characterized in that: In the step of preparing the micron- or submicron-sized sodium chloride particles, zirconium beads mixed with at least three different sizes are added to ordinary industrial-grade sodium chloride, which are ground, sieved and dried, and then white oil is added to continue grinding. After grinding, micron- or submicron-sized sodium chloride particles are obtained, wherein the ordinary industrial-grade sodium chloride is industrial salt with a sodium chloride purity of more than 99% and a particle size of 0.5 mm to 2 mm, and the maximum diameter of the zirconium beads does not exceed 1 mm.
7. The method for preparing an ultra-high molecular weight polyolefin membrane according to claim 5, characterized in that: The diameter of the micron-sized or submicron-sized sodium chloride particles is between 0.1 μm and 1 μm.
8. The method for preparing an ultra-high molecular weight polyolefin membrane according to claim 5, characterized in that: In the raw material mixing step, based on the total weight of the premixed raw materials, the weight proportion of the micron or submicron sodium chloride particles is 1wt% to 20wt%, the weight proportion of the ultra-high molecular weight polyethylene is 1wt% to 29wt%, and the weight proportion of the white oil is 60wt% to 80wt%.
9. The method for preparing an ultra-high molecular weight polyolefin diaphragm according to claim 5, characterized in that: The average molecular weight of the ultra-high molecular weight polyethylene is 1 million to 1.5 million.
10. The method for preparing an ultra-high molecular weight polyolefin diaphragm according to claim 5, characterized in that: In the step of preparing the micron or submicron sodium chloride particles, the micron or submicron sodium chloride particles include spheres, quasi-spherical shapes or irregular spheres, and their particle size distribution is similar to a normal distribution, wherein 80% of the sodium chloride particles are quasi-spherical.
Citation Information
Patent Citations
Method for preparing porous film by adopting high molecular weight polyolefin and product and application thereof
CN102153776A
Battery diaphragm with three cellular structures and adopted pore-forming agents and extraction agents
CN106299197A
Preparation method of lithium ion battery diaphragm
CN111129398A
Polyethylene diaphragm for lithium ion battery and preparation method of polyethylene diaphragm
CN113451706A
Embedded solid electrolyte diaphragm as well as preparation method and application thereof