Hollow PVDF (Polyvinylidene Fluoride) micro-nanofiber microstructure piezoelectric sensor and preparation method thereof
The hollow PVDF micro-nanofiber membrane was prepared by coaxial electrospinning method and the microstructure was constructed, which solved the problems of small sensor detection range and poor durability, achieved the improvement of high sensitivity and stability, and significantly improved the output voltage.
Patent Information
- Application Number
- CN202411190884.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-28
AI Technical Summary
The existing PVDF fiber membrane preparation methods are complex and unstable, resulting in limited sensor detection range, poor mechanical durability and stability, and lack of high sensitivity.
The hollow PVDF micro-nanofiber membrane was prepared by coaxial electrospinning method. By changing the fiber shape and building microstructures on the surface of the fiber membrane, the compressibility and piezoelectric properties of the fiber are improved, and the preparation process is simplified.
It significantly improves the piezoelectric output of PVDF nanofiber membrane, improves the sensitivity and stability of the sensor, achieves a wider detection range and better mechanical durability, and the output voltage reaches three times that of microstructure-free solid PVDF nanofibers.
Smart Images

Figure CN119053231A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of piezoelectric sensor preparation, and in particular to a hollow PVDF micro-nano fiber microstructure piezoelectric sensor and a preparation method thereof. Background Art
[0002] Currently, in the field of human-computer interaction and human activity monitoring, traditional detection equipment faces challenges such as large size, high cost, and lack of portability. Flexible sensors are thin-film electronic devices that can maintain high photoelectric efficiency, reliability, and integration even under conditions of bending, folding, twisting, compression, and stretching. Wearable electronic devices made of flexible electronic materials have attracted widespread attention due to their huge application potential and broad market opportunities.
[0003] Among the ideal materials for wearable electronic devices, piezoelectric materials stand out due to their high flexibility, light weight, biocompatibility and remarkable piezoelectric properties. In particular, polyvinylidene fluoride (PVDF) is widely used due to its portability, piezoelectricity and other remarkable properties, and has an extremely high piezoelectric coefficient. Electrospinning is a simple method to prepare high-β-phase crystalline PVDF nanofibers by in-situ mechanical stretching and poling during fiber processing.
[0004] At present, in order to increase the β-phase content of the prepared PVDF fiber membrane, the main methods include adding salt and adding nanofillers. However, the disadvantage of these methods is that the steps are complicated. Although the β-phase content can be increased, the addition of other materials exacerbates the instability of the electrospinning process, and it is not easy to form a complete fiber membrane without obvious defects. However, the prepared planar fiber membrane has a limited amount of compression when it is compressed by external force, which results in the detection range of the sensor being limited to a small range, and the mechanical durability and stability of the sensor are also relatively general. With the increasing application of flexible sensors, higher requirements are also placed on the performance of the sensor.
[0005] In the related research of the existing technology, changing the shape of PVDF fiber can further improve its piezoelectric properties, such as core-shell nanofibers, high porosity fibers, multi-channel nanofibers, etc. The output voltage or power has been significantly improved compared with solid fibers. In order to improve the comprehensive performance of flexible sensors, in addition to enhancing the material properties, constructing a microstructure in the functional layer of the sensor is also an effective method. The piezoelectric film with a microstructure has high compressibility and strong resistivity, which improves the piezoelectric properties of the nanofiber membrane. Changing the shape of the fiber and constructing a microstructure on the surface of the fiber membrane can improve the performance of the flexible sensor, but previous studies have almost discussed these two solutions separately, and research on the combination of the two is currently rare. Summary of the invention
[0006] The technical problem to be solved by the present invention is to provide a method for preparing a hollow PVDF micro-nanofiber microstructure piezoelectric sensor, so as to solve the problem that the existing preparation method has complicated steps, is unstable and is not easy to form a complete fiber membrane without obvious defects, thereby limiting the detection range of the sensor to a smaller range. A preparation method is provided that can improve the performance of the flexible sensor by changing the shape of the fiber and constructing a microstructure on the surface of the fiber membrane.
[0007] In order to solve the above technical problems, the present invention provides a method for preparing a hollow PVDF micro-nano fiber microstructure piezoelectric sensor, comprising the following steps:
[0008] S1: Pour PVDF and polyvinyl pyrrolidone powder into a mixture of dimethylacetamide and acetone, and fully heat and stir to obtain a PVDF / PVP mixed outer layer spinning solution; dissolve polyvinyl pyrrolidone powder in anhydrous ethanol and heat and stir to obtain an inner layer spinning solution;
[0009] S2: Printing a microstructure collector by stereolithography technology, and fixing the microstructure collector on the surface of the electrospinning flat collector;
[0010] S3: using the outer layer spinning solution and the inner layer spinning solution of step S1 as raw materials to prepare a PVDF / PVP composite fiber membrane through a coaxial electrospinning method;
[0011] S4: removing PVP from the PVDF / PVP composite fiber membrane of step S3 and drying it in a vacuum oven, thereby finally obtaining a PVDF micro-nano fiber membrane with a porous surface, a hollow inner layer and a microstructure on the fiber membrane surface;
[0012] S5: Covering electrodes on both sides of the PVDF micro-nano fiber membrane obtained in step S4, and then encapsulating it with PDMS and a curing agent to prepare a hollow PVDF micro-nano fiber microstructure piezoelectric sensor.
[0013] Compared with the prior art, the preparation method of a hollow PVDF micro-nano fiber microstructure piezoelectric sensor in the present application has the following advantages: The preparation method of a hollow PVDF micro-nano fiber microstructure piezoelectric sensor in the present invention increases the compressibility of the nanofiber membrane through multiple levels, thereby improving the piezoelectric output of the prepared PVDF nanofiber membrane, so that the sensitivity of the sensor can be improved. Through the coaxial electrospinning method, the concentration of the inner spinning solution is further regulated, and finally a nanofiber with a porous surface and a hollow interior is prepared, and a microstructure collector is also used to directly construct a microstructure on the surface of the fiber membrane. The synergistic effect of the multi-level microstructure further increases the compressibility of the fiber membrane and the sensitivity of the final sensor. The output voltage of the microstructured hollow PVDF nanofiber is about three times that of the solid PVDF nanofiber without a microstructure.
[0014] The present invention prepares a hollow PVDF fiber membrane containing a high β phase under the combined action of the electric field force stretching of electrospinning and the inner and outer spinning solutions, without the need for subsequent treatment, thereby simplifying the preparation process; and by utilizing the coaxial electrospinning method, the internal shape of the prepared fiber can be controlled by only changing the concentration of the inner spinning solution, and the prepared fiber morphology is intact without obvious defects, thereby further improving the stability of the final sensor.
[0015] In a possible implementation, in step S1, the polyvinyl pyrrolidone powder in the outer layer spinning solution is polyvinyl pyrrolidone K30; and the polyvinyl pyrrolidone powder in the inner layer spinning solution is polyvinyl pyrrolidone K90.
[0016] In the above embodiment, the selection of polyvinyl pyrrolidone K30 as a porogen is conducive to forming a porous surface structure after removal, and combined with the selection of K90 in the inner layer spinning solution, the performance of the final product is further improved.
[0017] In a possible embodiment, in step S1, the molecular weight of the PVDF is 300±50k, which is conducive to the stretching and orientation of the molecular chains to form bead-free round fibers; the mass ratio of the PVDF and polyvinyl pyrrolidone K30 is (1.7±0.2):(0.8±0.2); the mass ratio of dimethylacetamide and acetone is (1±0.1):(1±0.1).
[0018] In a possible implementation, in step S1, the concentration of polyvinyl pyrrolidone in the inner layer spinning solution is 5-15%, and the heating and stirring conditions are: stirring by magnetic stirring, and the stirring temperature is 60°C, the stirring time is 6-8h, and the rotation speed is 400-500rpm.
[0019] In the above embodiment, sufficient heating and stirring is beneficial to forming a stable spinning solution, so that the spinning effect is improved.
[0020] In a possible implementation, in step S2, the grid size of the microstructure collector is (2.2±0.4) mm, and the grid spacing is 0.1 mm.
[0021] In the above possible implementation manner, the present invention prepares a collector with a microstructure and assembles it on a flat collector, which can directly prepare a fiber membrane with a microstructure on the surface, greatly reducing the preparation steps and time.
[0022] In a possible implementation, in step S3, the method for preparing the PVDF / PVP composite fiber membrane includes:
[0023] The inner layer spinning solution and the outer layer spinning solution of step S1 are added into the syringe respectively, connected to the coaxial needle, and two micro-injection pumps are used to accurately control the flow rate of the inner and outer layer solutions, and the PVDF / PVP composite fiber membrane is prepared by coaxial electrospinning.
[0024] In a possible embodiment, in step S3, the size of the coaxial needle is 23 / 16G, the flow rate of the inner layer spinning solution is 0.55 ml / h, the flow rate of the outer layer spinning solution is 1.3 ml / h, the voltage applied for spinning is 18-22 KV, the spinning distance is 15 cm, and the spinning time is 2 hours.
[0025] In the above possible implementation manner, the present invention utilizes the coaxial electrospinning method, and the internal shape of the prepared fiber can be controlled by only changing the concentration of the inner spinning solution, and the prepared fiber morphology is intact without obvious defects;
[0026] In one possible embodiment, in step S4, the method of removing PVP is to remove the PVP in the fiber by immersing the PVDF / PVP composite fiber membrane in anhydrous ethanol and performing ultrasonic treatment, and the time of the ultrasonic treatment is more than 2 hours; the drying condition is to put the composite fiber membrane into a vacuum oven for drying at a temperature of 60°C for more than 6 hours, which is conducive to sufficient drying and forming hollow fibers with a full morphology.
[0027] In a possible implementation, in step S5, the electrode is copper foil, and the mass ratio of PDMS to curing agent is 10:1, and the packaging conditions are: after mixing PDMS and curing agent, pouring them on the piezoelectric film, and curing at 60° C. for 2 hours.
[0028] Another technical problem to be solved by the present invention is to provide a hollow PVDF micro-nano fiber microstructure piezoelectric sensor to solve the problems of small detection range and low sensitivity of conventional piezoelectric sensors.
[0029] In order to solve the above technical problems, the present invention provides a hollow PVDF micro-nano fiber microstructure piezoelectric sensor, and the piezoelectric sensor is prepared by the preparation method.
[0030] Compared with the prior art, the hollow PVDF micro-nano fiber microstructure piezoelectric sensor of the present invention has higher β phase and porosity, better mechanical durability and stability, fast response time and good recovery time, good dynamic performance, and has great potential in human activity monitoring and intelligent human-computer interaction. The hollow PVDF micro-nano fiber microstructure piezoelectric sensor of the present invention has good sensitivity, can detect signals under tiny pressure, and is suitable for signal detection and collection in multiple scenarios, with high universality. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 It is a flow chart of a method for preparing a hollow PVDF micro-nano fiber microstructure piezoelectric sensor in the present invention;
[0032] Figure 2 The crystal structure characterization and tensile performance test diagram of the fiber membrane prepared in Example 1;
[0033] Figure 3 The surface and cross-sectional morphology of nanofibers were observed by scanning electron microscopy (SEM);
[0034] Figure 4 The output voltage signal diagram of PVDF-0, PVDF-5, PVDF-10, and PVDF-15 without microstructures;
[0035] Figure 5 It is a physical picture of the microstructure collector, a physical picture of the microstructure fiber membrane and a basic representation picture of the microstructure size;
[0036] Figure 6 The cross-sectional size images of three groups of microstructured fiber membranes;
[0037] Figure 7 It is the sensitivity curve diagram of three groups of microstructure fiber membranes and PVDF-15 fiber membrane;
[0038] Figure 8 This is a 14,400-cycle endurance test diagram of the hollow PVDF micro-nano fiber microstructure piezoelectric sensor;
[0039] Fig. 9 The output voltage signal diagram of the sensor in different human activity monitoring;
[0040] Fig.10 Output voltage signal diagram for sensors monitoring various types of pulses and heartbeats of the human body;
[0041] Fig.11 is the image that the sensor uses for gesture recognition. DETAILED DESCRIPTION
[0042] First, those skilled in the art should understand that these implementations are only used to explain the technical principles of the embodiments of the present application, and are not intended to limit the protection scope of the embodiments of the present application. Those skilled in the art can make adjustments to them as needed to adapt to specific application scenarios.
[0043] In the description of the embodiments of the present application, it should be noted that, unless otherwise clearly specified and limited, the terms "connected" and "connection" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be directly connected or indirectly connected through an intermediate medium. For ordinary technicians in this field, the specific meanings of the above terms in the embodiments of the present application can be understood according to specific circumstances.
[0044] The present invention provides a method for preparing a hollow PVDF micro-nano fiber microstructure piezoelectric sensor, the preparation process is as follows: Figure 1 As shown, the following steps are included:
[0045] S1: Pour PVDF and polyvinyl pyrrolidone powder into a mixture of dimethylacetamide and acetone, and heat and stir to obtain a PVDF / PVP mixed outer layer spinning solution; dissolve polyvinyl pyrrolidone powder in anhydrous ethanol and heat and stir to obtain an inner layer spinning solution;
[0046] S2: Printing a microstructure collector by stereolithography technology, and fixing the microstructure collector on the surface of the electrospinning flat collector;
[0047] S3: using the outer layer spinning solution and the inner layer spinning solution of step S1 as raw materials, preparing a PVDF / PVP composite fiber membrane by coaxial electrospinning;
[0048] S4: removing PVP from the PVDF / PVP composite fiber membrane of step S3 and drying the membrane to obtain a PVDF micro-nano fiber membrane with a porous surface, a hollow inner layer and a microstructure on the fiber membrane surface;
[0049] S5: Covering electrodes on both sides of the PVDF micro-nano fiber membrane obtained in step S4, and then encapsulating it with PDMS and a curing agent to prepare a hollow PVDF micro-nano fiber microstructure piezoelectric sensor.
[0050] As a preferred solution, in step S1, the polyvinyl pyrrolidone powder in the outer layer spinning solution is polyvinyl pyrrolidone K30; and the polyvinyl pyrrolidone powder in the inner layer spinning solution is polyvinyl pyrrolidone K90.
[0051] As a preferred solution, in step S1, the molecular weight of the PVDF is 300±50k; the mass ratio of the PVDF to polyvinylpyrrolidone K30 is (1.7±0.2):(0.8±0.2); and the mass ratio of dimethylacetamide to acetone is (1±0.1):(1±0.1).
[0052] As a preferred solution, in step S1, the concentration of polyvinyl pyrrolidone in the inner layer spinning solution is 5-15%, and the heating and stirring conditions are: stirring by magnetic stirring, and the stirring temperature is 60°C, the stirring time is 6-8h, and the rotation speed is 400-500rpm.
[0053] As a preferred solution, in step S2, the grid size of the microstructure collector is (2.2±0.4) mm, and the grid spacing is 0.1 mm.
[0054] As a preferred solution, in step S3, the method for preparing the PVDF / PVP composite fiber membrane comprises:
[0055] The inner layer spinning solution and the outer layer spinning solution of step S1 are added into the syringe respectively, connected to the coaxial needle, and two micro-injection pumps are used to accurately control the flow rate of the inner and outer layer solutions to prepare the PVDF / PVP composite fiber membrane by spinning.
[0056] As a preferred solution, in step S3, the size of the coaxial needle is 23 / 16G, the flow rate of the inner layer spinning solution is 0.55 ml / h, the flow rate of the outer layer spinning solution is 1.3 ml / h, the voltage applied for spinning is 18-22 KV, the spinning distance is 15 cm, and the spinning time is 2 hours.
[0057] As a preferred scheme, in step S4, the method of removing PVP is to remove PVP by immersing the PVDF / PVP composite fiber membrane in anhydrous ethanol and then subjecting it to ultrasonic treatment, and the time of the ultrasonic treatment is more than 2 hours; the drying condition is to place the composite fiber membrane in a vacuum oven for drying at a temperature of 60°C for more than 6 hours.
[0058] As a preferred solution, in step S5, the electrode is copper foil, and the mass ratio of PDMS to curing agent is 10:1, and the packaging conditions are: after mixing PDMS and curing agent, pouring them on the piezoelectric film, and curing at 60°C for 2h.
[0059] The present invention also provides a hollow PVDF micro-nano fiber microstructure piezoelectric sensor, which is prepared by the preparation method.
[0060] The following provides an embodiment that combines specific experimental data and operating methods, and uses the inner layer spinning solution as a controlled variable for experimental comparison. Of course, the present invention does not only include the following embodiments of experimental conditions. The experimental parameters, experimental time and experimental conditions within the scope of the above technical solution of the present invention should be included in the protection scope of the present invention. The following embodiment further describes the above technical solution of the present invention by controlling the changes in some data, and provides the results of testing the finished product:
[0061] Embodiment 1:
[0062] In Example 1, the step S1 includes 3 groups of inner layer spinning solution cases with different concentrations, and the step S2 includes 3 groups of micro-lattice cases with different sizes, so as to facilitate further comparison in the subsequent test stage:
[0063] S1: 1.7 g PVDF powder and 0.8 g PVP were weighed into a screw-capped bottle at room temperature, and a mixed solution of DMAC and acetone in a volume ratio of 1:1 (10 mL in total) was added into the bottle and placed on a magnetic stirrer. After stirring at 60 °C for 6 h, a uniform and stable outer spinning solution was obtained.
[0064] PVP K90 powder was added to a screw-mouth bottle at room temperature, anhydrous ethanol was added to the bottle and placed on a magnetic stirrer, and stirred at 60° C. for 6 h to prepare inner layer spinning solutions with concentrations of 5%, 10%, and 15%, respectively.
[0065] S2: A collection plate with a microstructure was prepared using SLA. The sizes of the microgrids were 1.8 mm × 1.8 mm, 2.2 mm × 2.2 mm, and 2.6 mm × 2.6 mm, respectively. The size between each group of grids was 0.1 mm. The prepared microstructured small blocks were assembled onto the flat collector of electrospinning.
[0066] S3: Add the inner and outer spinning solutions into the syringe respectively and connect the syringe to a 23 / 16G coaxial needle, and ground the needle. Connect the collecting plate to the positive pole of the high-voltage power supply and set the voltage to 18-22kV. The distance between the needle and the collecting plate is 15cm. Two micro-injection pumps are used to accurately control the flow rate. The flow rate of the inner spinning solution is controlled at 0.55ml / h, and the flow rate of the outer spinning solution is controlled at 1.3ml / h. The fiber collection time is 2h. A 21G uniaxial needle is used for spinning as a control group. The spinning solution flow rate is 1.5ml / h, the applied voltage is 17KV, the spinning distance is 15cm, and the fiber collection time is 2h.
[0067] S4: After the prepared PVDF / PVP composite fiber membrane is naturally dried, it is transferred to anhydrous ethanol for ultrasonic treatment for 2 hours to remove the PVP inside the fiber, and then transferred to a vacuum oven and dried at 60°C for 6 hours to finally obtain a hollow PVDF micro-nano fiber membrane with a microstructure.
[0068] S5: Copper foils were attached to both sides of the piezoelectric film as electrodes, 20 g of PDMS liquid and 2 g of curing agent were weighed and placed in a beaker and stirred for 5 min, then poured onto the piezoelectric film and cured at 60°C for 2 h. After the PDMS was cured, it was cut into appropriate sizes, and finally a hollow PVDF micro-nano fiber microstructure piezoelectric sensor was obtained.
[0069] Embodiment 2-3:
[0070] Embodiment 2-3 is similar to embodiment 1, except that, in step S1, the concentration of the inner layer spinning solution is different, namely 10% and 15%, and the fibers prepared in embodiments 1-3 are named PVDF-5, PVDF-10, and PVDF-15 according to the concentration of the inner layer spinning solution;
[0071] Comparative Example 1:
[0072] Comparative Example 1 is also similar to Example 1, except that in step S1, the concentration of the inner layer spinning solution is different, which is 0%, that is, anhydrous ethanol. The fiber obtained in Comparative Example 1 is named PVDF-0.
[0073] The following relevant tests were performed on the above-mentioned Examples 1-3 and Comparative Example 1 of the present invention:
[0074] like Figure 2 As shown, the fiber prepared in the above embodiment was subjected to crystal structure characterization and tensile performance testing. Figure 2As shown in Figure a, the melting temperatures of four groups of fiber membranes (PVDF-0, PVDF-5, PVDF-10, and PVDF-15) prepared in Examples 1-3 and Comparative Example 1 were measured by differential scanning calorimetry (DSC). It can be seen that the melting temperatures of all hollow PVDF micro-nano fibers are higher than those of the solid fiber PVDF-0 in Comparative Example 1. Figure 2 As shown in Figures 2b and 2c, the content of β phase in the fiber was obtained by X-ray diffraction analysis and Fourier transform infrared spectroscopy analysis, and as the inner layer PVP solution was gradually introduced, the non-polar α phase originally contained gradually decreased. The crystallinity and β phase content of the four groups of fiber membranes measured are shown in Figure 2c. Figure 2 As shown in Figure d, the crystallinity of the three groups of hollow PVDF is slightly lower than that of solid fiber PVDF-0, but the β-phase content is significantly improved. When the inner layer spinning solution concentration is 15%, the β-phase content reaches a maximum of 91.31%. Figure 2 As shown in Figure e, the porosity of the four groups of fiber membranes was measured using the n-butanol method. It can be seen that the porosity of the three groups of hollow PVDF fibers is higher than that of the solid fiber PVDF-0, and the porosity of PVDF-15 is the highest, reaching 88.94. Figure 2 As shown in FIG. 5 , four groups of fiber membranes were subjected to uniaxial tensile performance tests, and the tensile strains of the three groups of hollow PVDF fibers were all higher than that of the solid fiber PVDF-0, among which PVDF-15 reached a maximum of 56.9%. The above test results fully demonstrate that the prepared hollow PVDF fiber has a high β-phase content and excellent strain performance, and also prove that the spinning solution prepared by the present invention through a special preparation method solves the problems existing in the background technology after practical application.
[0075] like Figure 3 As shown in the figure, the surface and cross-sectional morphology of the nanofibers were observed by scanning electron microscopy (SEM). It can be seen that as the concentration of the inner layer PVP solution increases, the fiber gradually changes from internal porous to hollow structure, the surface becomes more and more rough and porous, and the average diameter of the fiber increases. The main reason for this phenomenon is that as the concentration of the inner layer solution increases, the inner layer solution gradually diffuses outward. When the concentration of the inner layer solution is 15%, the fiber presents a completely hollow structure with good morphology.
[0076] like Figure 4 As shown, Figure 4PVDF-0, PVDF-5, PVDF-10, and PVDF-15 are PVDF micro-nano fiber membranes prepared by removing step S2 and step S4 from examples 1-3 and comparative example 1; four groups of fiber membranes (PVDF-0, PVD F-5, PVDF-10, and PVDF-15) without microstructures prepared by removing step S2 from examples 1-3 and comparative example 1 were tested, and the packaged sensors were tested for piezoelectric performance. The piezoelectric outputs of the three groups of fibers with hollow structures under the impact of the 5N, 2Hz exciter were higher than those of the solid fiber PVDF-0, and the output voltage generated by PVDF-15 was up to 7.4V, while the maximum voltage of PVDF-0 was only 3.4V. And under the same frequency (2Hz) and different external forces (1N, 3N, 5N, 7.5N, 10N, 15N), PVDF-15 has higher sensitivity and detection range than PVD F-0. This indicates that micro-nano fibers with hollow structures can generate piezoelectric output higher than that of solid fibers, and the piezoelectric output increases with the increase of the hollowness. Since the performance of the prepared PVDF-15 (Example 3 without step S2) is better than that of the other materials, PVDF-15 is used in the subsequent experiments in the following tests.
[0077] like Figure 5 As shown, in order to further enhance the piezoelectric properties of the sensor, the present invention further constructs three microstructures of different scales on the surface of the above-mentioned PVDF-15 fiber membrane. In the step S2, the sizes of the micro grids are 1.8mm×1.8mm, 2.2mm×2.2mm, and 2.6mm×2.6mm, respectively, and the size between each group of grids is 0.1mm. They are named M1.8, M2.2, and M2.6, respectively. Further testing is carried out in the following test. Compared with the above-mentioned PVDF-15 of the present invention, the microstructure treatment of step S2 of the present invention is added.
[0078] like Figure 6 As shown, the cross-sectional dimensions of the three groups of microstructure fiber membranes prepared in the above embodiments of the present invention were scanned using a confocal laser microscope (CLSM). It can be seen that the maximum surface undulation difference of the microstructure of M2.6 is 250 microns, while that of the other two groups is only 120 microns and 180 microns.
[0079] like Figure 7As shown, the piezoelectric output of three groups of fiber membranes with microstructures under the same frequency (2Hz) and different external forces (1N, 3N, 5N, 7.5N, 10N, 15N) was tested and plotted into a sensitivity curve. As shown in the figure, after the microstructure is introduced, the output voltage of the nanofiber membrane is improved, and the maximum output voltage can reach 10.1V, which is about 1.6 times higher than PVDF-15 (6.2V) without step S2 treatment. Compared with PVDF-0 (3.4V) without step S2 treatment, it is improved by about 3 times. This also further proves that the further introduction of the microstructure of step S2 in the present invention can effectively improve the sensitivity of the sensor, and the synergistic effect of the configuration of the spinning solution and the concentration ratio configuration of the present invention further improves the sensitivity; compared with the other two microstructure sensors, M2.6 has a larger surface fluctuation and greater compression. In the range of 3-5N, the maximum sensitivity of M2.6 is 2.7V / N (1.08V / KPa), which is more than twice that of PVDF-15 without microstructure.
[0080] like Figure 8 As shown, the durability test of the microstructure sensor prepared in Example 3 shows that after 14,400 cycles of impact, the output voltage value of the sensor only slightly decreases, and the sensor can still maintain a stable piezoelectric output signal. The durability test shows that the sensor prepared by the present invention has good mechanical durability and stability, and solves the problems existing in the background technology.
[0081] like Fig. 9 As shown, in order to verify the feasibility of the prepared sensor in human activity monitoring, the sensor prepared in Example 3 was attached to various parts of the human body for signal detection. Fig. 9 a) Elbows Fig. 9 b) and knee joint ( Fig. 9 c), the sensor has obvious signal changes at the same bending angle but different bending frequencies. Taking knee joint monitoring as an example, the output signal of the volunteer in three motion states of walking, jogging and sprinting is shown in 7c. Based on the measured number of voltage cycles and voltage peaks, the running frequency during exercise can be calculated, and the exercise state of the volunteer can also be judged. Connect the sensor to the finger for activity monitoring, such as Fig. 9 d. When the finger is bent at different angles (30°, 60°, 90°) and the activity frequency is the same, the sensor shows obvious signal changes. From the enlarged images after the finger is bent and released, it can be seen that the sensor has a fast response time (60.4ms) and a good recovery time (157.6ms).
[0082] like Fig.10As shown, we also used the sensor prepared in Example 3 to detect the pulse and heartbeat of different parts of the volunteers' body, including the temporal artery, brachial artery, carotid artery, posterior tibial artery, radial artery and heart. The waveforms of various parts of the human body have obvious characteristic peaks, which proves that our sensor is capable of receiving these weak signals from the human body.
[0083] like Fig.11 As shown, the sensor of the present invention can also be used for human gesture recognition and synchronous control of the movement of the robot palm ( Fig.11 b) The circuit schematic diagram designed to control the robot is as follows Fig.11 As shown in a: The system consists of five microstructured hollow PVDF nanofiber flexible sensors, an operational amplifier, an Arduino development board and a robotic palm. When the fingers are bent, the electrical signals generated by the sensors are amplified and filtered by the operational amplifier, and the output analog signals are converted into digital signals through pulse width modulation, thereby controlling the bending of the corresponding fingers of the robotic palm; Fig.11 As shown in (c), the operator can make the same gestures as the volunteer (“Victory”, “OK”, and “I Love You”) at the same time. Therefore, the prepared sensor has good dynamic performance and has great potential in human activity monitoring and intelligent human-computer interaction.
[0084] The above-mentioned Examples 1-3 and Comparative Example 1 further prove that the present invention provides a hollow PVDF micro-nano fiber microstructure piezoelectric sensor and a preparation method thereof. The sensitivity of the piezoelectric sensor prepared by the preparation method of the present invention is greatly improved compared with conventional technical means, and the response time is short and has a good recovery time, which solves the problems existing in the background technology. The prepared sensor has excellent mechanical durability and stability, and has high commercial value and promotion value.
[0085] In the description of the embodiments of the present application, it should be noted that in the description of the present application, terms such as "inside" and "outside" indicating directions or positional relationships are based on the directions or positional relationships shown in the drawings. This is only for the convenience of description, and does not indicate or imply that the device or component must have a specific orientation, be constructed and operated in a specific orientation. Therefore, it cannot be understood as a limitation on the present application.
[0086] In the description of the present application, the description with reference to the terms "one embodiment", "some embodiments", "in the present embodiment", "specific example", or "some examples" etc. means that the specific features, mechanisms, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present application. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, mechanisms, materials or characteristics described may be combined in a suitable manner in any one or more embodiments or examples. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, unless they are contradictory.
[0087] The above is only a specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application shall be based on the protection scope of the claims.
Claims
1. A method for preparing a hollow PVDF micro-nano fiber microstructure piezoelectric sensor, characterized in that: The following steps are involved: S1: Pour PVDF and polyvinyl pyrrolidone powder into a mixture of dimethylacetamide and acetone, and heat and stir to obtain a PVDF / PVP mixed outer layer spinning solution; dissolve polyvinyl pyrrolidone powder in anhydrous ethanol and heat and stir to obtain an inner layer spinning solution; S2: Printing a microstructure collector by stereolithography technology, and fixing the microstructure collector on the surface of the electrospinning flat collector; S3: using the outer layer spinning solution and the inner layer spinning solution of step S1 as raw materials, preparing a PVDF / PVP composite fiber membrane by coaxial electrospinning; S4: removing PVP from the PVDF / PVP composite fiber membrane of step S3 and drying the membrane to obtain a PVDF micro-nano fiber membrane with a porous surface, a hollow inner layer and a microstructure on the fiber membrane surface; S5: Covering electrodes on both sides of the PVDF micro-nano fiber membrane obtained in step S4, and then encapsulating it with PDMS and a curing agent to prepare a hollow PVDF micro-nano fiber microstructure piezoelectric sensor.
2. The method for preparing the hollow PVDF micro-nano fiber microstructure piezoelectric sensor according to claim 1, characterized in that: In the step S1, the polyvinyl pyrrolidone powder in the outer layer spinning solution is polyvinyl pyrrolidone K30; and the polyvinyl pyrrolidone powder in the inner layer spinning solution is polyvinyl pyrrolidone K90.
3. The method for preparing the hollow PVDF micro-nano fiber microstructure piezoelectric sensor according to claim 2, characterized in that: In the step S1, the molecular weight of the PVDF is 300±50k; the mass ratio of the PVDF to polyvinylpyrrolidone K30 is (1.7±0.2):(0.8±0.2); and the mass ratio of dimethylacetamide to acetone is (1±0.1):(1±0.1).
4. The method for preparing the hollow PVDF micro-nano fiber microstructure piezoelectric sensor according to claim 1, characterized in that: In the step S1, the concentration of polyvinyl pyrrolidone in the inner layer spinning solution is 5-15%, and the heating and stirring conditions are: stirring by magnetic stirring, and the stirring temperature is 60° C., the stirring time is 6-8 hours, and the rotation speed is 400-500 rpm.
5. The method for preparing the hollow PVDF micro-nano fiber microstructure piezoelectric sensor according to claim 1, characterized in that: In step S2, the grid size of the microstructure collector is (2.2±0.4) mm, and the grid spacing is 0.1 mm.
6. The method for preparing the hollow PVDF micro-nano fiber microstructure piezoelectric sensor according to claim 1, characterized in that: In step S3, the method for preparing the PVDF / PVP composite fiber membrane comprises: The inner layer spinning solution and the outer layer spinning solution of step S1 are added into the syringe respectively, connected to the coaxial needle, and two micro-injection pumps are used to accurately control the flow rate of the inner and outer layer solutions to prepare the PVDF / PVP composite fiber membrane by spinning.
7. The method for preparing the hollow PVDF micro-nano fiber microstructure piezoelectric sensor according to claim 6, characterized in that: In step S3, the size of the coaxial needle is 23 / 16G, the flow rate of the inner layer spinning solution is 0.55 ml / h, the flow rate of the outer layer spinning solution is 1.3 ml / h, the voltage applied for spinning is 18-22 KV, the spinning distance is 15 cm, and the spinning time is 2 hours.
8. The method for preparing the hollow PVDF micro-nano fiber microstructure piezoelectric sensor according to claim 1, characterized in that: In step S4, the method of removing PVP is to remove PVP by immersing the PVDF / PVP composite fiber membrane in anhydrous ethanol and then subjecting it to ultrasonic treatment, and the ultrasonic treatment time is more than 2 hours; the drying condition is to place the composite fiber membrane in a vacuum oven for drying at a temperature of 60°C for more than 6 hours.
9. The method for preparing the hollow PVDF micro-nano fiber microstructure piezoelectric sensor according to claim 1, characterized in that: In the step S5, the electrode is copper foil, and the mass ratio of PDMS to curing agent is 10:
1. The packaging conditions are: after mixing PDMS and curing agent, pouring them on the piezoelectric film, and curing at 60° C. for 2 hours.
10. A hollow PVDF micro-nano fiber microstructure piezoelectric sensor, characterized in that: The piezoelectric sensor is prepared by the preparation method described in any one of claims 1-9.
Citation Information
Patent Citations
Perovskite composite nanofiber membrane as well as preparation method and application thereof
CN110230108A
Super-hydrophobic nanofiber, fibrous membrane and preparation method and application thereof
CN110777533A
Flexible sensing composite fiber membrane with multistage microstructure as well as preparation method and application of flexible sensing composite fiber membrane
CN116240678A
PVP (Polyvinyl Pyrrolidone) / PVA (Polyvinyl Acetate)-Nin composite nanofiber membrane, preparation method and fingerprint showing method
CN118441412A
Method for fabrication of porous fibrous microstructure with various 3-dimensional structures
US20150126633A1
Cited By
Signal amplification device and preparation method thereof
CN122248959A