Organic solvent-dispersed sol containing conductive tin oxide particles, and method for producing same

By dispersing modified particles of tin oxide and other metal oxides in an organic solvent, combining the proportion of different amines, the problem of poor dispersion of modified metal oxide particles in the prior art in organic solvents is solved, and high refractive is achieved Coating properties of rate and conductivity.

CN119053553AActive Publication Date: 2024-11-29NISSAN CHEM CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202480001990.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-04-03
Filing Date
2024-03-26
Publication Date
2024-11-29
Estimated Expiration
2044-03-26

AI Technical Summary

Technical Problem

The prior art is difficult to stabilize the dispersion of modified metal oxide particles with high conductivity and high refractive index in an organic solvent, and it is difficult to maintain transparency and good resistivity when the substrate is coated.

Method used

Using tin oxide having an average particle size of 4 to 50 nm as the core, at least one metal oxide of antimony oxide, tin oxide and silicon oxide as the coated particles, is used to combine with a modified metal oxide sol dispersed in an organic solvent. The ratio of amines with high water solubility and low water solubility achieves stable dispersion and coating properties of particles.

Benefits of technology

The stable dispersion of modified metal oxide particles in organic solvents is achieved, ensuring transparency and high resistivity during coating, and improving the performance of the coating film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005063410400000031
    Figure BDA0005063410400000031
  • Figure BDA0005063410400000032
    Figure BDA0005063410400000032
  • Figure BDA0005063410400000191
    Figure BDA0005063410400000191
Patent Text Reader

Abstract

Provided is a modified metal oxide particle sol having transparency, a high particle refractive index, and a good coating film resistivity value when a coating agent using modified metal oxide particles is applied to a substrate. The present invention is a sol containing modified metal oxide particles (iii) which have tin oxide particles (i) having an average primary particle diameter of 4-50 nm as cores, and which are dispersed in an organic solvent, and which are characterized in that: the modified metal oxide particles (iii) have tin oxide particles (i) having an average primary particle diameter of 4-50 nm as the cores; the core particles are coated with particles (ii) of at least one type of metal oxide selected from antimony oxide, tin oxide, and silicon oxide having an average primary particle diameter of 1-10 nm, the average primary particle diameter having a relationship of not less than (i) the core particles but not less than (ii) the coated particles, (the total mass of metal oxides other than tin oxide) / (the mass of tin oxide) being 0.005-1.0, and the average primary particle diameter being not less than (i) the average primary particle diameter being not less than (i) the average primary particle diameter being not less than (i) the average primary particle diameter being not less than (ii) the average primary particle diameter being not less than (i) the average primary particle diameter. The sol contains an amine (a) having a water solubility of 0.1 g / L or more and an amine (b) having a water solubility of less than 0.1 g / L.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an organic solvent-dispersed sol containing colloidal particles of conductive tin oxide (also referred to as modified oxide particles) and a method for producing the same. Background Art

[0002] It is known that high-purity tin oxide itself is insulating, but by doping with indium or antimony, it exhibits electronic conductivity. In addition, it is also known that tin oxide exhibits electronic conductivity due to oxygen defects. By utilizing the properties of these tin oxide particles as a transparent conductive coating agent, for example, it is disclosed that a transparent conductive film is obtained by coating it on a film (see Patent Document 1).

[0003] In addition, the following modified metal oxide sol is disclosed, wherein an aqueous sol containing tin oxide and a water-soluble amine having an average particle size of 4 to 50 nm is hydrothermally treated at a pressure of 0.1 to 40 MPa and a temperature of 100 to 350°C to produce an aqueous sol containing core particles, and then an aqueous sol of composite colloidal particles of antimony pentoxide and silicon dioxide having an average particle size of less than 5 nm or an aqueous sol of colloidal particles of antimony pentoxide containing a water-soluble amine and an average particle size of 1 to 10 nm is mixed as coating particles to coat the surface of the core particles with the coating particles (see Patent Document 2).

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Publication No. 35-6616

[0007] Patent Document 2: Japanese Patent Application Publication No. 2006-176392 Summary of the invention

[0008] Problems to be solved by the invention

[0009] The present invention provides an organic solvent sol, which comprises modified metal oxide particles (iii) having tin oxide (i) as a core and coated with metal oxide particles (ii) of at least one selected from antimony oxide, tin oxide and silicon oxide, wherein the modified metal oxide particles (iii) have high conductivity and high refractive index, and when the modified metal oxide particles (iii) are stably dispersed in an organic solvent, they can have transparency, particle refractive index and coating film resistivity when applied to a substrate as a coating agent.

[0010] Means for solving problems

[0011] According to the present invention, as a first aspect, there is provided a modified metal oxide sol comprising modified metal oxide particles (iii), the modified metal oxide particles being dispersed in an organic solvent, wherein the modified metal oxide particles (iii) have tin oxide particles (i) having an average primary particle size of 4 to 50 nm as cores and are coated with metal oxide particles (ii) having an average primary particle size of 1 to 10 nm and being at least one selected from antimony oxide, tin oxide and silicon oxide, wherein the average primary particle size has a relationship of core particles (i) ≧ coated particles (ii), (total mass of metal oxides other than tin oxide) / (mass of tin oxide) is 0.005 to 1.0, and the sol comprises an amine (a) having a water solubility of 0.1 g / liter or more and an amine (b) having a water solubility of less than 0.1 g / liter;

[0012] As a second aspect, there is provided the modified metal oxide sol according to the first aspect, wherein the average particle size measured by a dynamic light scattering method is 5 to 100 nm;

[0013] As a third aspect, there is provided the modified metal oxide sol according to the first aspect or the second aspect, wherein the tin oxide particles (i) as the core particles are hydrothermally treated tin oxide particles;

[0014] As a fourth aspect, there is provided the modified metal oxide sol according to any one of the first aspect to the third aspect, wherein the tin oxide particles (i) as the core particles have a crystallinity of 60% or more as determined by an X-ray diffraction method;

[0015] As a fifth aspect, there is provided the modified metal oxide sol according to any one of the first aspect to the fourth aspect, wherein the metal oxide particles (ii) as the coated particles are antimony oxide particles, or composite particles of tin oxide and silicon oxide in a mass ratio of 1:0.1 to 10.0;

[0016] As a sixth aspect, there is provided the modified metal oxide sol according to any one of the first aspect to the fifth aspect, wherein the modified metal oxide sol contains the amine (a) at a ratio of 20 to 3000 ppm;

[0017] As a seventh aspect, there is provided the modified metal oxide sol according to any one of the first aspect to the sixth aspect, wherein the modified metal oxide sol contains the amine (b) at a ratio of 1000 to 30000 ppm;

[0018] As an eighth aspect, there is provided the modified metal oxide sol according to any one of the first aspect to the seventh aspect, wherein the amine (a) is an amine comprising a primary amine, a secondary amine, or a combination thereof;

[0019] As a ninth aspect, there is provided the modified metal oxide sol according to any one of the first aspect to the eighth aspect, wherein the amine (b) is a tertiary amine;

[0020] As a tenth aspect, there is provided the modified metal oxide sol according to any one of the first aspect to the ninth aspect, wherein the amine (a) is at least one amine selected from the group consisting of n-propylamine, di-n-propylamine, isopropylamine, diisopropylamine, n-butylamine, isobutylamine, di-n-butylamine and diisobutylamine;

[0021] As an eleventh aspect, there is provided the modified metal oxide sol according to any one of the first aspect to the tenth aspect, wherein the amine (b) is at least one amine selected from tri-n-butylamine, tri-isobutylamine, tri-n-pentylamine and tri-isopentylamine;

[0022] As a twelfth aspect, there is provided the modified metal oxide sol according to any one of the first aspect to the eleventh aspect, wherein the mass ratio of amine (b) / amine (a) is 3.0 to 200;

[0023] As a thirteenth aspect, there is provided the modified metal oxide sol according to any one of the first aspect to the twelfth aspect, wherein the modified metal oxide particles (iii) are coated with at least one coating agent selected from the group consisting of formula (1) to formula (6):

[0024]

Chemistry 1

[0025] R 1 a si(R 2 ) 4-a (1)

[0026]

[0027] R 5 d Si(R 6 ) 4-d (3)

[0028]

Chemistry 2

[0029]

[0030] [In formula (1), R 1 Each is an alkyl group, a halogenated alkyl group, an alkenyl group, an aryl group, or an organic group having a polyether group, an epoxy group, a (meth)acryloyl group, a mercapto group, an amino group, a urea group, or a cyano group, and is bonded to the silicon atom through a Si-C bond, R 2 Each represents an alkoxy group, an acyloxy group, or a halogen group, and a represents an integer of 1 to 3.

[0031] In formula (2) and formula (3), R 3 and R 5Each is an alkyl group having 1 to 3 carbon atoms or an aryl group having 6 to 30 carbon atoms, and is bonded to the silicon atom through a Si-C bond, R 4 and R 6 Each represents an alkoxy group, an acyloxy group, or a halogen group, Y represents an alkylene group, an NH group, or an oxygen atom, b is an integer of 1 to 3, c is an integer of 0 or 1, and d is an integer of 1 to 3,

[0032] In formula (4) to formula (6), X1, X2 and X3 each represent an alkylene group having 2 to 20 carbon atoms, f, h and j each represent an integer of 1 to 100, e, g and i each represent an integer of 1 to 3, and Y1, Y2 and Y3 each represent a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, or a (meth)acryloyl group. ];

[0033] As a fourteenth aspect, there is provided the modified metal oxide sol according to any one of the first aspect to the thirteenth aspect, wherein the organic solvent is a solvent containing an alcohol, a ketone, an ester, an ether, an amide, a hydrocarbon, a cyano group-containing solvent, a halogen-containing solvent, a sulfonyl group-containing solvent, a carboxyl group-containing solvent, or a mixed solvent thereof;

[0034] As a fifteenth aspect, there is provided the modified metal oxide sol according to the fourteenth aspect, wherein the alcohol is a monohydric alcohol having 1 to 20 carbon atoms or a polyhydric alcohol having 1 to 20 carbon atoms;

[0035] As a sixteenth aspect, an antistatic composition is provided, comprising the modified metal oxide particles (iii) in the modified metal oxide sol according to any one of the first aspect to the fifteenth aspect.

[0036] As a seventeenth aspect, there is provided a composition for an electron transport material, comprising the modified metal oxide particles (iii) in the modified metal oxide sol according to any one of the first aspect to the fifteenth aspect;

[0037] As an eighteenth aspect, there is provided a method for producing an organic solvent sol of modified metal oxide particles according to any one of the first aspect to the fifteenth aspect, the method comprising the following steps (A) to (D):

[0038] (A) step: a step of preparing an aqueous sol containing an amine (a) having a water solubility of 0.1 g / liter or more and tin oxide particles (i) having an average primary particle size of 4 to 50 nm,

[0039] (B) step: preparing an aqueous sol containing an amine (a) having a water solubility of 0.1 g / liter or more and metal oxide particles (ii) having an average primary particle size of 1 to 10 nm and being at least one selected from antimony oxide, tin oxide and silicon oxide,

[0040] (C) a step of mixing the aqueous sol of tin oxide obtained in step (A) and the aqueous sol of modified metal oxide obtained in step (B) at a ratio of (total mass of metal oxides other than tin oxide) / (mass of tin oxide) of 0.005 to 1.0 to produce modified metal oxide particles (iii) having tin oxide particles (i) having an average primary particle size of 4 to 50 nm as cores and coated with at least one metal oxide particle (ii) having an average primary particle size of 1 to 10 nm selected from antimony oxide, tin oxide and silicon oxide, and adding an amine (b) having a water solubility of less than 0.1 g / liter,

[0041] Step (D): a step of replacing the aqueous medium solvent of the aqueous sol of the modified metal oxide particles (iii) obtained in step (C) with an alcohol having 1 to 5 carbon atoms;

[0042] As a nineteenth aspect, there is provided a method for producing an organic solvent sol of modified metal oxide particles (iii) according to the eighteenth aspect, wherein the step (A) is a step (A-1) of adding an amine (a) having a water solubility of 0.1 g / liter or more to an aqueous sol of tin oxide particles (i) having an average primary particle size of 4 to 50 nm, and then subjecting the sol to a hydrothermal treatment at a pressure of 0.1 to 40 MPa and a temperature of 100 to 350° C. for 0.01 to 100 hours;

[0043] As a twentieth aspect, there is provided the method for producing an organic solvent sol of modified metal oxide particles according to the eighteenth aspect or the nineteenth aspect, wherein step (E) and / or step (F) is added after step (D):

[0044] Step (E): adding at least one coating agent selected from the group consisting of formulae (1) to (6) to the organic solvent sol of the modified metal oxide particles (iii) to perform surface treatment on the modified metal oxide particles (iii);

[0045] Step (F): a step of replacing the alcohol solvent of the alcohol solvent sol having 1 to 5 carbon atoms of the modified metal oxide particles (iii) with an alcohol, ketone, ester, ether, amide, hydrocarbon, cyano group-containing solvent, halogen-containing solvent, sulfonyl group-containing solvent, carboxyl group-containing solvent, or a mixed solvent thereof other than those used in step (D).

[0046] Effects of the Invention

[0047] In the present invention, modified metal oxide particles (iii) are used, wherein the surface of tin oxide particles (i) serving as core particles is coated with at least one metal oxide particle selected from antimony oxide, tin oxide and silicon oxide (ii) as coating particles.

[0048] Both the core particles and the coated particles can use an aqueous sol in which colloidal metal oxide particles are stably dispersed in an aqueous medium. These aqueous sols can be mixed. For example, an aqueous sol containing the coated particles (ii) is added to an aqueous sol containing the core particles (i) to obtain an aqueous sol containing the modified metal oxide particles (iii). In order to stably disperse in an aqueous medium, these aqueous sols must contain an amine (a) having a water solubility of 0.1 g / liter or more. With respect to the two aqueous sols, namely the aqueous sol containing core particles (i) and the aqueous sol containing coated particles (ii), cation exchange is carried out before or after the two are mixed to remove a portion of them. With respect to the aqueous sol of the mixed modified metal oxide particles (iii), at the stage of then replacing the dispersion medium from the aqueous medium with an organic solvent to produce an organic solvent sol of the modified metal oxide particles (iii), the aqueous medium can be replaced with an organic solvent by the coexistence of an amine (a) having a water solubility of more than 0.1 g / liter and an amine (b) having a water solubility of less than 0.1 g / liter, thereby making it possible to produce an organic solvent sol of non-agglomerated modified metal oxide particles (iii).

[0049] In addition, the core particles (i) can also be subjected to a hydrothermal treatment. As for the hydrothermal treatment, for example, the treatment is carried out at a pressure of 0.1 to 40 MPa and a temperature of 100 to 350°C for 0.01 to 100 hours. It is hoped that the core particles will be stably dispersed in an aqueous medium, so an amine (a) with a water solubility of 0.1 g / liter or more is required.

[0050] In the present invention, the modified metal oxide particles (iii) are a sol dispersed in an organic solvent. In order to improve the dispersibility of the modified metal oxide particles (iii) in the organic solvent by replacing the aqueous medium with an organic solvent, it is necessary to contain an amine (b) having a water solubility of less than 0.1 g / L. DETAILED DESCRIPTION

[0051] The present invention provides a modified metal oxide sol, which comprises modified metal oxide particles (iii) dispersed in an organic solvent, wherein the modified metal oxide particles (iii) have tin oxide particles (i) having an average primary particle size of 4 to 50 nm as cores and are coated with metal oxide particles (ii) having an average primary particle size of 1 to 10 nm and being at least one selected from antimony oxide, tin oxide and silicon oxide, wherein the average primary particle size satisfies the relationship of core particles (i) ≧ coated particles (ii), (total mass of metal oxides other than tin oxide) / (mass of tin oxide) is 0.005 to 1.0, and the sol comprises an amine (a) having a water solubility of 0.1 g / liter or more and an amine (b) having a water solubility of less than 0.1 g / liter.

[0052] As a method for measuring the solubility of a chemical substance in water, a column elution method is used when the solubility is low, and a flask method is used when the solubility is high. For example, a measurement method specified in OECD Test Guide 105 (solubility in water) can be used.

[0053] The metal oxide other than tin oxide refers to a metal oxide whose metal component is other than tin.

[0054] The average primary particle size of the tin oxide particles (i) and the metal oxide particles (ii) can be measured by observation with a transmission electron microscope.

[0055] The sol containing the modified metal oxide particles (iii) can be measured by a dynamic light scattering method, and the average particle size by the dynamic light scattering method is preferably 5 to 100 nm, 10 to 60 nm, or 10 to 50 nm.

[0056] The tin oxide particles (i) having an average primary particle size of 4 to 50 nm used as a raw material in the present invention can be prepared as an aqueous sol containing the tin oxide particles (i).

[0057] For example, it is possible to easily produce a sol of colloidal particles having a particle size of about 4 to 50 nm by using a method such as an ion exchange method, a peptization method, a hydrolysis method, a reaction method, or the like.

[0058] As an example of the above-mentioned ion exchange method, there can be cited a method of treating a stannate such as sodium stannate with a hydrogen-type cation exchange resin, or a method of treating a tin salt such as tin chloride or tin nitrate with a hydroxyl-type anion exchange resin. As an example of the above-mentioned degumming method, there can be cited a method of neutralizing a tin salt with an alkali or neutralizing stannic acid with hydrochloric acid to wash the obtained tin hydroxide gel, and then degumming with an acid or an alkali. As an example of the above-mentioned hydrolysis method, there can be cited a method of hydrolyzing a tin alkoxide, or a method of removing unnecessary acid after hydrolyzing an alkaline tin chloride salt under heating. As an example of the above-mentioned reaction method, there can be cited a method of reacting a metallic tin powder with an acid.

[0059] The aqueous sol containing the tin oxide particles (i) as a raw material can also be obtained by the reaction of metallic tin and hydrogen peroxide solution.

[0060] The metal tin can be used in the form of powder or granules. For example, a metal tin powder obtained by atomizing a melted ingot and spraying and solidifying it, or a flaky metal tin powder produced by cutting an ingot with a turntable, a file, or the like can be used.

[0061] As for hydrogen peroxide, a commercially available aqueous solution with a concentration of 35% by mass can be used at a desired concentration. For example, an organic acid aqueous solution such as oxalic acid with a concentration of 1 to 30% by mass or 5 to 20% by mass is prepared, and hydrogen peroxide and metallic tin are added to the organic acid aqueous solution simultaneously or alternately to obtain an aqueous solution of stannic acid. An organic acid aqueous solution such as oxalic acid is placed in a reaction vessel equipped with a stirrer, and hydrogen peroxide and metallic tin are added simultaneously or alternately from their respective addition ports under stirring. Since the slurry of the agglomerate containing tin oxide colloid is acidic, it is preferred to use a glass reaction device or a glass-lined (enamel) reaction device for the reaction device used in these steps.

[0062] Hydrogen peroxide solution and metal tin are added to an organic acid aqueous solution such as oxalic acid while maintaining a H2O2 / Sn molar ratio of 2 to 3. More specifically, the following method of adding in stages can be cited: 1 / 3 to 1 / 30 mass parts of each of hydrogen peroxide solution and metal tin to be added are taken with respect to the total mass parts of hydrogen peroxide solution and metal tin to be added, and a series of steps of adding hydrogen peroxide solution to an organic acid aqueous solution such as oxalic acid, then adding metal tin, and then reacting for 2 to 20 minutes are repeated 3 to 30 times.

[0063] Even if the H2O2 / Sn molar ratio slightly exceeds 3, the reaction can be carried out, but it is not preferred to exceed it significantly. When the H2O2 / Sn molar ratio is less than 2, oxidation becomes insufficient, so it is not preferred. As for the addition time of hydrogen peroxide water and metallic tin, it can be added for 0.4 to 10 hours, preferably 0.4 to 5 hours. When the addition time is less than 0.4 hours, the exothermic reaction is violent and cannot be controlled, and unreacted metallic tin is likely to remain, so it is not preferred. In addition, it can be more than 10 hours, but it is not economical, so it is not preferred.

[0064] The reaction of metallic tin and hydrogen peroxide in an aqueous solution of an organic acid such as oxalic acid is carried out at 30 to 95° C., preferably 40 to 85° C. The reaction of hydrogen peroxide with metallic tin is an oxidation reaction, and therefore becomes an exothermic reaction. In addition, a decomposition reaction of hydrogen peroxide also occurs at the same time, and this reaction is also an exothermic reaction, so attention must be paid to temperature control during the reaction, and cooling can be performed as required. The reaction temperature may be less than 30° C., and since it is an exothermic reaction, excessive cooling is required, and the reaction takes too much time, which is not economical. When the reaction temperature is above 95° C., coarse colloidal particles are generated, so it is not preferred.

[0065] The process is to remove excess electrolyte (mainly anions) from the obtained slurry of tin oxide colloid agglomerates and dissociate the tin oxide colloid particles to obtain a sol. By removing excess electrolyte, a sol in which tin oxide colloid particles are dispersed in a state close to primary particles can be obtained. The cleaning can be carried out by a method of agglomerating and precipitating the supernatant, an ultrafiltration method, an ion exchange method, etc. In the case of containing a large amount of electrolyte, a cleaning method of repeatedly ultrafiltration, then water injection, and then ultrafiltration again (ultrafiltration-water injection-ultrafiltration) is particularly preferred. The average primary particle size of the tin oxide composite colloid particles obtained by this process is 4 to 50 nm or 10 to 20 nm (nanometers).

[0066] The step of performing anion exchange on the tin oxide aqueous sol can be added. By this anion exchange treatment, a sol that is stable even at high concentration can be obtained. Commercially available anion exchange resins can be used for anion exchange, and the anion exchange resins are used after being prepared into a hydroxyl type. Anion exchange can be easily performed by passing the tin oxide aqueous sol through a column filled with anion exchange resin. The flow temperature is preferably 0 to 60°C, and the flow rate is preferably a space velocity SV1 to 10 hours.

[0067] Before and / or after the anion exchange treatment, an alkaline substance can be added to the tin oxide aqueous sol to improve stability. As the alkaline substance used, an organic base is preferred, for example, an amine (a) having a water solubility of 0.1 g / liter or more, 0.1 to 5000.0 g / liter, 0.1 to 3000.0 g / liter, 0.1 to 2000.0 g / liter, 0.5 to 2000.0 g / liter, 1.0 to 2000.0 g / liter, 10.0 to 2000.0 g / liter, or 100 to 1000.0 g / liter can be used.

[0068] Amine (a) can be added in a ratio of 20 to 3000 ppm, or 20 to 1000 ppm. Amine (a) can use an amine containing a primary amine, a secondary amine, or a combination thereof. For example, as amine (a), at least one amine selected from n-propylamine, di-n-propylamine, isopropylamine, diisopropylamine, n-butylamine, isobutylamine, di-n-butylamine, and diisobutylamine can be used.

[0069] The crystallinity of the tin oxide particles (i) used as the core particles in the present invention as determined by X-ray diffraction is preferably 60% or more, or 65% or more and 100% or less, and typically, 60 to 95% or 65 to 95% can be used. Preferably, it is 60% or more, and typically, it can be 60 to 99% or 60 to 95%.

[0070] In the present invention, the tin oxide aqueous sol having a SnO2 concentration of 1 to 50% by mass produced by the above method can be directly used, and hydrothermally treated tin oxide particles can be produced by hydrothermally treating the tin oxide particles under pressure at 100 to 350°C for 0.01 to 100 hours. For the hydrothermal treatment, for example, the tin oxide aqueous sol is placed in an autoclave and treated at a pressure of 0.1 to 40 MPa (megapascals) and a temperature of 100 to 350°C for 0.01 to 100 hours.

[0071] The medium of these tin oxide sols can be any one of water and hydrophilic organic solvents, and preferably the medium is an aqueous sol in which water is used as the medium. In addition, the pH of the sol can be a value that stabilizes the sol, and usually, it can be about 0.2 to 11.5. As long as the purpose of the present invention is achieved, the tin oxide sol can contain any components, such as alkaline substances, acidic substances, hydroxycarboxylic acids, etc. for stabilizing the sol. The concentration of the tin oxide sol used is about 0.5 to 50% by mass in terms of tin oxide, and the lower the concentration, the better, preferably 1 to 30% by mass.

[0072] As for the tin oxide sol, it is particularly preferred to use an alkaline sol stabilized with an organic base such as the above-mentioned amine, and the addition of the above-mentioned amine is preferably performed at 5 to 100° C., preferably at room temperature (20° C.) to 60° C. In addition, as for the mixing, the above-mentioned amine is added to the tin oxide sol under stirring, and it is necessary to mix it thoroughly, preferably for 0.5 to 3 hours.

[0073] As the coated particles (ii) used in the present invention, aqueous sols of coated particles can be used. As the coated particles (ii), antimony oxide particles (ii-1) alone or composite particles of tin oxide and silicon oxide (ii-2) with a mass ratio of tin oxide:silicon dioxide = 1:0.1 to 10.0 can be used.

[0074] The antimony pentoxide colloidal particles (ii-1) containing an alkylamine can be obtained by oxidation, acid decomposition, or the like. As an example of the acid decomposition method, an alkali metal antimonate is reacted with an inorganic acid and then degraded with an amine (Japanese Patent Publication No. 60-41536, Japanese Patent Publication No. 61-227918, Japanese Patent Publication No. 2001-123115), and as an example of the oxidation method, an antimony trioxide is oxidized with hydrogen peroxide in the presence of an amine and an alkali metal (Japanese Patent Publication No. 57-11848, Japanese Patent Publication No. 59-232921); and an amine and an alkali metal are added after oxidation of antimony trioxide with hydrogen peroxide. As for the above-mentioned amine, for example, an amine (a) having a water solubility of 0.1 g / liter or more can be used. The amine (a) can be added in a ratio of 20 to 3000 ppm or 20 to 1000 ppm. Amine (a) can use amines including primary amines, secondary amines or combinations thereof. For example, amine (a) can use at least one amine selected from n-propylamine, di-n-propylamine, isopropylamine, diisopropylamine, n-butylamine, isobutylamine, di-n-butylamine and diisobutylamine.

[0075] The alkylamine-containing antimony pentoxide colloidal particles (ii-1) are minute antimony pentoxide colloidal particles, and the particle size thereof, as observed by electron microscope, is about 1 to 20 nm in oligomer or primary particle size. As the amine component, an alkylamine salt such as diisopropylamine is preferred, and the molar ratio of amine to Sb2O5 is 0.02 to 4.00.

[0076] In the above-mentioned coating, silica particles containing an alkylamine may be further added to the antimony pentoxide colloidal particles containing an amine.

[0077] The composite colloid of antimony pentoxide and silicon dioxide that can be used as the coating sol can be obtained by the known method shown below (for example, Japanese Patent Publication No. 50-40119), that is, it can be obtained by mixing an alkali metal silicate aqueous solution or a silicic acid solution with an alkali metal antimonate aqueous solution and then removing cations using a cation exchange resin.

[0078] As the antimony raw material, potassium antimonate aqueous solution can be preferably used. As the silica raw material, sodium silicate, potassium silicate and active silicic acid obtained by cation exchange thereof can be used. The molar ratio of SiO2 / Sb2O5 is 0.55 to 55. As for the particle size, the oligomer or the average primary particle is less than 5 nm, preferably 1 to 5 nm, by electron microscope observation.

[0079] The tin oxide and silicon dioxide composite colloidal particles (ii-2) used in the coating sol of the present invention can be obtained by the method described below.

[0080] The method is as follows: an aqueous solution containing stannate and silicate in a SiO2 / SnO2 mass ratio of 0.1 to 10 is prepared, and the cations present in the obtained aqueous solution are removed. The total concentration of SnO2 and SiO2 contained in the sol is usually 40% by mass or less, preferably 2% by mass or more, and preferably 5 to 30% by mass.

[0081] The sol can exist stably without substantially containing an alkali component. However, it can also contain an alkali component and be stabilized. As for the alkali component, as amine (a), it can be added at a ratio of 20 to 3000 ppm, or 20 to 1000 ppm. Amine (a) can use an amine containing a primary amine, a secondary amine or a combination thereof. For example, as for amine (a), at least one amine selected from n-propylamine, di-n-propylamine, isopropylamine, diisopropylamine, n-butylamine, isobutylamine, di-n-butylamine and diisobutylamine can be used. These alkali components can be contained in an amount of about 30% by mass or less relative to the total amount of SnO2 and SiO2. In addition, two or more of these can be mixed and contained. By adding amine (a) at a ratio of 20 to 3000 ppm, the amine dissolved in the sol is adsorbed on the surface of the modified metal oxide particles, and the dispersion stability is improved.

[0082] The sol is a colorless, transparent or slightly colloidal liquid with a pH of 1 to 9. It is stable at room temperature for more than 3 months and at 60° C. for more than 1 month, and no precipitate is generated in the sol. In addition, the sol does not thicken or gel.

[0083] As examples of stannates and silicates used in the manufacture of the sol, sodium stannate (Na2SnO3·3H2O) and sodium silicate (water glass) are preferred. In addition, substances obtained by dissolving stannic acid, silicic acid, etc. in an aqueous solution of an alkali metal hydroxide can also be used. Examples include a method of preparing an aqueous solution by dissolving powders of stannates and silicates in water; a method of preparing an aqueous solution by mixing an aqueous stannate solution and an aqueous silicate solution; a method of preparing an aqueous solution by adding stannate powder and an aqueous silicate solution to water, etc. As an aqueous solution of stannate, a SnO2 concentration of about 0.1 to 30% by mass is preferred, but a concentration above this can also be used. As an aqueous solution of silicate, a SiO2 concentration of about 0.1 to 30% by mass is preferred, but a concentration above this can also be used.

[0084] The preparation of the aqueous solution can be carried out under stirring at room temperature (about 20°C) to 100°C, preferably at room temperature (about 20°C) to 60°C. The aqueous solution to be mixed is preferably 0.1 to 100 in terms of SiO2 / SnO2 mass ratio. Next, the cations present in the aqueous solution obtained here are removed to obtain an aqueous sol. As a method for decationization treatment, a method of contacting with a hydrogen-type ion exchanger or salting out can be used. The hydrogen-type cation exchanger used here is a commonly used hydrogen-type cation exchanger, and if convenient, a commercially available hydrogen-type cation exchange resin can be used.

[0085] When the concentration of the sol is low, the aqueous sol can be concentrated by a common concentration method, such as evaporation, ultrafiltration, etc., as required to increase the concentration of the sol. Ultrafiltration is particularly preferred. During the concentration, the temperature of the sol is preferably maintained at about 100° C. or less, particularly at about 60° C. or less. In addition, the lower limit is not particularly limited, but is preferably maintained at 10° C. or more, and more preferably maintained at 20° C. or more.

[0086] According to the present invention, the modified tin oxide colloidal particles (iii-1) whose surfaces are coated with amine-containing Sb2O5 colloidal particles (ii-1) are negatively charged in the sol. The above-mentioned tin oxide particles (i) are positively charged, and the Sb2O5 colloid is negatively charged. Therefore, it is believed that through mixing, the negatively charged Sb2O5 colloid (ii-1) is electrically attracted around the positively charged tin oxide colloidal particles (i), and then the Sb2O5 colloid is bonded to the surface of the positively charged colloidal particles through chemical bonding, and the positively charged particles are used as cores, and the negatively charged Sb2O5 covers its surface, thereby generating modified tin oxide colloidal particles (iii-1).

[0087] When tin oxide colloidal particles (i) having an average primary particle size of 4 to 50 nm as a core sol are mixed with amine-containing Sb2O5 colloids (ii-1) as a coating sol, if the metal oxide of the coating sol is less than 1 part by mass relative to 100 parts by mass of the metal oxide (SnO2) of the core sol, a stable sol cannot be obtained. This is considered to be because when the amount of Sb2O5 colloid is insufficient, the surface coating of the tin oxide colloidal particles used as the core of the composite colloidal particles becomes insufficient, and aggregation of the generated colloidal particles is likely to occur, making the generated sol unstable. Therefore, the amount of Sb2O5 colloidal particles to be mixed can be less than the amount that covers the entire surface of the tin oxide colloidal particles, but it is an amount greater than the minimum amount required to generate a stable sol of modified tin oxide particles. When Sb2O5 colloidal particles in an amount exceeding the amount used in the surface coating are used in the above mixing, the resulting sol is nothing more than a stable mixed sol of the Sb2O5 colloid sol and the generated modified tin oxide colloidal particles sol.

[0088] The tin oxide colloidal particles (i) are positively charged, and the composite colloid of tin oxide and silicon dioxide (ii-2) is negatively charged. Therefore, it is believed that by mixing, the negatively charged composite colloid of tin oxide and silicon dioxide (ii-2) is electrically attracted around the positively charged tin oxide colloidal particles (i), and then the composite colloid of tin oxide and silicon dioxide is bonded to the surface of the positively charged colloidal particles by chemical bonding, and the negatively charged composite colloid of tin oxide and silicon dioxide covers the surface of the positively charged particles as cores, thereby generating modified tin oxide colloidal particles (iii-2).

[0089] When tin oxide colloidal particles (i) having an average primary particle size of 4 to 50 nm as a core sol are mixed with a composite colloid of tin oxide and silicon dioxide (ii-2) as a coating sol, if the metal oxide of the coating sol is less than 1 mass part relative to 100 mass parts of the metal oxide (SnO2) of the core sol, a stable sol cannot be obtained. This is believed to be because when the amount of the composite colloid of tin oxide and silicon dioxide is insufficient, the surface coating of the colloidal particles of the composite using the tin oxide colloidal particles as the core becomes insufficient, and aggregation of the generated colloidal particles is likely to occur, making the generated sol unstable. Therefore, the amount of composite colloid particles of tin oxide and silicon dioxide to be mixed can be less than the amount covering the entire surface of the tin oxide or tin oxide-zirconium oxide composite colloid particles, but it is an amount greater than the minimum amount required to generate a stable sol of modified tin oxide colloidal particles. When the composite colloid particles of tin oxide and silicon dioxide in an amount exceeding the amount used for the surface coating are used for the above mixing, the obtained sol is nothing more than a stable mixed sol of the composite colloid sol of tin oxide and silicon dioxide and the sol of the generated modified tin oxide colloid particles.

[0090] Preferably, when the tin oxide colloidal particles are modified by the surface coating, the amount of the composite colloid of tin oxide and silicon dioxide used can be 50 parts by mass or less based on 100 parts by mass of the metal oxide (SnO2) in the core sol, calculated as the metal oxide in the coating sol.

[0091] The sol of the present invention is obtained by the following method, which includes the following steps (A) to (D):

[0092] (A) step: a step of preparing an aqueous sol containing an amine (a) having a water solubility of 0.1 g / liter or more and tin oxide particles (i) having an average primary particle size of 4 to 50 nm,

[0093] (B) step: preparing an aqueous sol containing an amine (a) having a water solubility of 0.1 g / liter or more and metal oxide particles (ii) having an average primary particle size of 1 to 10 nm and being at least one selected from antimony oxide, tin oxide and silicon oxide,

[0094] (C) a step of mixing the aqueous sol of tin oxide obtained in step (A) and the aqueous sol of modified metal oxide obtained in step (B) at a ratio of (total mass of metal oxides other than tin oxide) / (mass of tin oxide) of 0.005 to 1.0 to produce modified metal oxide particles (iii) having tin oxide particles (i) having an average primary particle size of 4 to 50 nm as cores and coated with at least one metal oxide particle (ii) having an average primary particle size of 1 to 10 nm selected from antimony oxide, tin oxide and silicon oxide, and adding an amine (b) having a water solubility of less than 0.1 g / liter,

[0095] Step (D): a step of replacing the aqueous medium solvent of the aqueous sol of the modified metal oxide particles (iii) obtained in step (C) with an alcohol having 1 to 5 carbon atoms.

[0096] In the present invention, as for the step (A), a step (A-1) can be used in which an amine (a) having a water solubility of 0.1 g / liter or more is added to an aqueous sol of tin oxide particles (i) having an average primary particle size of 4 to 50 nm, followed by a hydrothermal treatment at a pressure of 0.1 to 40 MPa and a temperature of 100 to 350° C. for 0.01 to 100 hours.

[0097] In the present invention, the mixing of the aqueous sol of the tin oxide particles (i) obtained in step (A) and the aqueous sol of the metal oxide particles (ii) selected from at least one of antimony oxide, tin oxide and silicon oxide obtained in step (B) in step (C) is preferably carried out so that the (total mass of metal oxides other than tin oxide) / (mass of tin oxide) in the modified metal oxide particles (iii) is 0.005 to 1.0, or 0.005 to 0.5, or 0.01 to 0.5, or 0.01 to 0.3, or 0.01 to 0.2, or 0.04 to 0.15.

[0098] The amine (b) having a water solubility of less than 0.1 g / liter used in step (C) includes amines having a water solubility of less than 0.1 g / liter, 0.00001 g / liter or more and less than 0.1 g / liter, 0.00002 g / liter or more and less than 0.1 g / liter, 0.00003 g / liter or more and less than 0.1 g / liter, 0.00005 g / liter or more and less than 0.1 g / liter, 0.0001 g / liter or more and less than 0.1 g / liter, The tertiary amine can be 0.1 g / liter, 0.001 g / liter or more and less than 0.1 g / liter, 0.01 g / liter or more and less than 0.1 g / liter, 0.00003 g / liter or more and 0.08 g / liter, 0.00003 g / liter or more and 0.05 g / liter, or 0.00003 g / liter or more and 0.03 g / liter, for example, at least one amine selected from tri-n-butylamine, tri-isobutylamine, tri-n-pentylamine and tri-isopentylamine.

[0099] The modified metal oxide sol may contain the amine (a) in a ratio of 20 to 3000 ppm or 20 to 1000 ppm.

[0100] The modified metal oxide sol may contain the amine (b) in a ratio of 1,000 to 30,000 ppm or 1,000 to 10,000 ppm.

[0101] It is believed that the amine (b) added in step (C) with a water solubility of less than 0.1 g / liter is partially adsorbed on the surface of the modified metal oxide particles (iii) in the aqueous sol of step (C). By the presence of the above-mentioned amine (b) when the dispersion medium of the sol is replaced by an organic solvent from an aqueous medium solvent in the subsequent step (D), the compatibility with the organic solvent is improved, and the modified metal oxide particles (iii) will not agglomerate and can be dispersed in the organic solvent. The above-mentioned amine (b) is made to migrate from the surface of the modified metal oxide particles (iii) to the organic solvent in the organic solvent. In the organic solvent-dispersed sol of the above-mentioned modified metal oxide particles (iii), amine (a) and amine (b) can be detected from the dispersion medium. By fully dispersing the modified metal oxide particles (iii) in the organic solvent, the sol exists stably, so that when the coating agent using them is applied to the substrate and cured, the modified metal oxide particles will not be biased on the substrate, thereby obtaining a high refractive index and good conductivity. The refractive index of such modified metal oxide particles is preferably in the range of 1.75 to 2.00.

[0102] Examples of the alcohol having 1 to 5 carbon atoms used in the step (D) include methanol, ethanol, n-propanol, isopropanol, n-butanol, and propylene glycol monomethyl ether.

[0103] In the modified metal oxide sol obtained in the present invention, the mass ratio of amine (b) / amine (a) is preferably 3.0-200, or 3.0-100, or 3.0-60.

[0104] In the present invention, after step (D), step (E) and / or step (F) may be added:

[0105] Step (E): adding at least one coating agent selected from the group consisting of formulae (1) to (6) to the organic solvent sol of the modified metal oxide particles (iii) to perform surface treatment on the modified metal oxide particles (iii);

[0106] Step (F): a step of replacing the alcohol solvent of the alcohol solvent sol having 1 to 5 carbon atoms of the modified metal oxide particles (iii) with an alcohol, ketone, ester, ether, amide, hydrocarbon, cyano group-containing solvent, halogen-containing solvent, sulfonyl group-containing solvent, carboxyl group-containing solvent, or a mixed solvent thereof other than those used in step (D).

[0107] In the coating agent of the above step (E), Formulas (1) to (3) are silane coupling agents, and Formulas (4) to (6) are phosphate ester compounds. As the coating agent, a silane coupling agent, a phosphate ester compound, or a combination thereof can be used.

[0108] For example, it is also possible to perform step (E) after step (D); perform step (F) after step (D); perform step (E) after step (D), and then perform step (F).

[0109] As the silane compound, the coating may be performed with a hydrolyzate of at least one silane compound selected from the group consisting of formula (1) to formula (3).

[0110] In formula (1), R 1 Each is an alkyl group, a halogenated alkyl group, an alkenyl group, an aryl group, or an organic group having a polyether group, an epoxy group, a (meth)acryloyl group, a mercapto group, an amino group, a urea group, or a cyano group, and is bonded to the silicon atom through a Si-C bond, R 2 Each represents an alkoxy group, an acyloxy group, or a halogen group, and a represents an integer of 1 to 3.

[0111] In formula (2) and formula (3), R 3 and R 5 Each is an alkyl group having 1 to 3 carbon atoms or an aryl group having 6 to 30 carbon atoms, and is bonded to the silicon atom through a Si-C bond, R 4 and R 6 Each represents an alkoxy group, an acyloxy group, or a halogen group, Y represents an alkylene group, an NH group, or an oxygen atom, b is an integer of 1 to 3, c is an integer of 0 or 1, and d is an integer of 1 to 3.

[0112] The alkyl group is an alkyl group having 1 to 18 carbon atoms, and examples thereof include methyl, ethyl, n-propyl, isopropyl, cyclopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, cyclobutyl, 1-methyl-cyclopropyl, 2-methyl-cyclopropyl, n-pentyl, 1-methyl-n-butyl, 2-methyl-n-butyl, 3-methyl-n-butyl, 1,1-dimethyl-n-propyl, 1,2-dimethyl-n-propyl, 2,2-dimethyl-n-propyl, 1-ethyl-n-propyl, cyclopentyl, 1-methylcyclobutyl, 2-methylcyclobutyl, 3-methylcyclobutyl, butyl, 1,2-dimethylcyclopropyl, 2,3-dimethylcyclopropyl, 1-ethylcyclopropyl, 2-ethylcyclopropyl, n-hexyl, 1-methyl-n-pentyl, 2-methyl-n-pentyl, 3-methyl-n-pentyl, 4-methyl-n-pentyl, 1,1-dimethyl-n-butyl, 1,2-dimethyl-n-butyl, 1,3-dimethyl-n-butyl, 2,2-dimethyl-n-butyl, 2,3-dimethyl-n-butyl, 3,3-dimethyl-n-butyl, 1-ethyl-n-butyl, 2-ethyl-n-butyl, 1,1,2-trimethyl-n-propyl, 1, 2,2-trimethyl-n-propyl, 1-ethyl-1-methyl-n-propyl, 1-ethyl-2-methyl-n-propyl, cyclohexyl, 1-methylcyclopentyl, 2-methylcyclopentyl, 3-methylcyclopentyl, 1-ethylcyclobutyl, 2-ethylcyclobutyl, 3-ethylcyclobutyl, 1,2-dimethylcyclobutyl, 1,3-dimethylcyclobutyl, 2,2-dimethylcyclobutyl, 2,3-dimethylcyclobutyl, 2,4-dimethylcyclobutyl, 3,3-dimethylcyclobutyl, 1-n-propylcyclopropyl, 2-n-propylcyclopropyl, 1-isopropylcyclopropyl, 2-isopropylcyclopropyl, 1,2,2-trimethylcyclopropyl, 1,2,3-trimethylcyclopropyl, 2,2,3-trimethylcyclopropyl, 1-ethyl-2-methylcyclopropyl, 2-ethyl-1-methylcyclopropyl, 2-ethyl-2-methylcyclopropyl and 2-ethyl-3-methylcyclopropyl, hexyl, heptyl, octyl, nonyl, decyl, undecyl, dodecyl, tridecyl, tetradecyl, pentadecyl, hexadecyl, heptadecyl, octadecyl and the like, but are not limited to these.

[0113] In addition, examples of the alkylene group include alkylene groups derived from the above-mentioned alkyl groups.

[0114] The aryl group is an aryl group having 6 to 30 carbon atoms, and examples thereof include phenyl, naphthyl, anthracenyl, and pyrenyl.

[0115] Examples of the alkenyl group include an alkenyl group having 2 to 10 carbon atoms, such as vinyl, 1-propenyl, 2-propenyl, 1-methyl-1-vinyl, 1-butenyl, 2-butenyl, 3-butenyl, 2-methyl-1-propenyl, 2-methyl-2-propenyl, 1-ethylvinyl, 1-methyl-1-propenyl, 1-methyl-2-propenyl, 1-pentenyl, 2-pentenyl, 3-pentenyl, 4-pentenyl, 1-n-propylvinyl, 1-methyl-1-butenyl, 1-methyl-2-butenyl, 1-methyl-3-butenyl, 2-ethyl-2-propenyl, 2-methyl-1-butenyl, 2-methyl-2-butenyl, 2-methyl-3-butenyl, The invention also includes, but is not limited to, 1-butylene, 3-methyl-1-butenyl, 3-methyl-2-butenyl, 3-methyl-3-butenyl, 1,1-dimethyl-2-propenyl, 1-isopropylvinyl, 1,2-dimethyl-1-propenyl, 1,2-dimethyl-2-propenyl, 1-cyclopentenyl, 2-cyclopentenyl, 3-cyclopentenyl, 1-hexenyl, 2-hexenyl, 3-hexenyl, 4-hexenyl, 5-hexenyl, 1-methyl-1-pentenyl, 1-methyl-2-pentenyl, 1-methyl-3-pentenyl, 1-methyl-4-pentenyl, 1-n-butylvinyl, 2-methyl-1-pentenyl, and 2-methyl-2-pentenyl.

[0116] As for the above-mentioned alkoxy group, alkoxy groups having 1 to 10 carbon atoms can be listed, for example, methoxy group, ethoxy group, n-propoxy group, isopropoxy group, n-butoxy group, isobutoxy group, sec-butoxy group, tert-butoxy group, n-pentoxy group, 1-methyl-n-butoxy group, 2-methyl-n-butoxy group, 3-methyl-n-butoxy group, 1,1-dimethyl-n-propoxy group, 1,2-dimethyl-n-propoxy group, 2,2-dimethyl-n-propoxy group, 1-ethyl-n-propoxy group, n-hexyloxy group and the like can be listed, but it is not limited to these.

[0117] The acyloxy group is an acyloxy group having 2 to 10 carbon atoms, and examples thereof include, but are not limited to, a methylcarbonyloxy group, an ethylcarbonyloxy group, an n-propylcarbonyloxy group, an isopropylcarbonyloxy group, an n-butylcarbonyloxy group, an isobutylcarbonyloxy group, a sec-butylcarbonyloxy group, a tert-butylcarbonyloxy group, an n-pentylcarbonyloxy group, a 1-methyl-n-butylcarbonyloxy group, a 2-methyl-n-butylcarbonyloxy group, a 3-methyl-n-butylcarbonyloxy group, a 1,1-dimethyl-n-propylcarbonyloxy group, a 1,2-dimethyl-n-propylcarbonyloxy group, a 2,2-dimethyl-n-propylcarbonyloxy group, a 1-ethyl-n-propylcarbonyloxy group, an n-hexylcarbonyloxy group, a 1-methyl-n-pentylcarbonyloxy group, and a 2-methyl-n-pentylcarbonyloxy group.

[0118] Examples of the halogen group include fluorine, chlorine, bromine, and iodine.

[0119] Examples of the organic group having a polyether group include a polyether propyl group having an alkoxy group. For example, (CH3O)3SiC3H6(OC2H4)nOCH3 may be mentioned. n may be used in the range of 1 to 100, or 1 to 10.

[0120] Examples of the organic group having an epoxy group include a 2-(3,4-epoxycyclohexyl)ethyl group and a 3-glycidoxypropyl group.

[0121] The (meth)acryloyl group refers to both an acryloyl group and a methacryloyl group. Examples of the organic group having a (meth)acryloyl group include a 3-methacryloyloxypropyl group and a 3-acryloyloxypropyl group.

[0122] Examples of the organic group having a mercapto group include a 3-mercaptopropyl group.

[0123] Examples of the organic group having an amino group include 2-aminoethyl, 3-aminopropyl, N-2-(aminoethyl)-3-aminopropyl, N-(1,3-dimethylbutylene)aminopropyl, N-phenyl-3-aminopropyl, and N-(vinylbenzyl)-2-aminoethyl-3-aminopropyl.

[0124] As an organic group which has a ureido group, a 3-ureidopropyl group is mentioned, for example.

[0125] Examples of the organic group having a cyano group include a 3-cyanopropyl group.

[0126] The compounds of the above formula (2) and formula (3) are preferably compounds capable of forming trimethylsilyl groups on the surface of silica particles. Examples of these compounds are as follows.

[0127]

Chemistry 3

[0128]

[0129] In the above formula, R 12 is an alkoxy group, and examples thereof include a methoxy group and an ethoxy group. As the silane compound, for example, a silane compound manufactured by Shin-Etsu Chemical Co., Ltd. can be used.

[0130] The process is as follows: on the surface of the modified metal oxide particles (iii), a hydroxyl group, for example, a silanol group in the case of silica particles, reacts with the above-mentioned silane compound, and the surface of the silica particles is coated with the above-mentioned silane compound through a siloxane bond. The reaction temperature can be carried out at a temperature ranging from 20°C to the boiling point of the dispersion medium, for example, in the range of 20°C to 100°C. The reaction time can be carried out for about 0.1 to 6 hours.

[0131] The coating amount of the silane compound on the surface of the modified metal oxide particle (iii) can be set to 0.1 atoms / nm corresponding to the number of silicon atoms in the silane compound. 2 ~6.0 / nm 2 A silane compound in a coating amount of 1000 Å to 1000 Å is added to the sol of the modified metal oxide particles (iii) to coat the surfaces of the silica particles.

[0132] The hydrolysis of the silane compound requires water. When the aqueous medium solvent is replaced with an organic solvent, the water remaining in the solvent can be used. For example, water present in an amount of 0.01 to 1% by mass can be used. In addition, the hydrolysis can be carried out using a catalyst or without a catalyst.

[0133] As the above-mentioned phosphoric acid ester compound, as phosphoric acid ester, at least one phosphoric acid ester compound selected from the group consisting of formula (4) to formula (6) can be cited.

[0134] In formulas (4) to (6), X1, X2 and X3 each represent an alkylene group having 2 to 20 carbon atoms, f, h and j each represent an integer from 1 to 100, e, g and i each represent an integer from 1 to 3, and Y1, Y2 and Y3 each represent a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms or a (meth)acryloyl group.

[0135] As the phosphate ester, polyoxyethylene alkyl ether phosphate can be preferably used. For example, the phosphate ester can be a phosphate ester in which the terminal alkyl group (Y1) in the above formula (4) represents an alkyl group having 6 to 10 or 12 to 15 carbon atoms. As for the products thereof, for example, Phosphanol RA-600 and RS-610 manufactured by Toho Chemical Industry Co., Ltd. can be used.

[0136] Examples of the alkylene group having 2 to 20 carbon atoms include those derived from the above-mentioned alkyl groups, and examples of the alkenyl group having 2 to 20 carbon atoms and the aryl group having 6 to 30 carbon atoms include those exemplified above.

[0137] The coating amount of the phosphoric acid ester compound on the surface of the modified metal oxide particle (iii) can be set to 0.1 atoms / nm corresponding to the number of phosphorus atoms in the phosphoric acid ester compound. 2 ~6.0 / nm 2 The phosphoric acid ester compound is added to the sol of the modified metal oxide particles (iii) in a coating amount to coat the surfaces of the modified metal oxide particles.

[0138] In the present invention, the following step (F) may be added after the step (D).

[0139] Step (F): a step of replacing the alcohol solvent of the alcohol solvent sol having 1 to 5 carbon atoms of the modified metal oxide particles (iii) obtained in step (D) with an alcohol, ketone, ester, ether, amide, hydrocarbon, cyano group-containing solvent, halogen-containing solvent, sulfonyl group-containing solvent, carboxyl group-containing solvent, or a mixed solvent thereof other than those used in step (D).

[0140] Alcohols other than those used in step (D) that can be used in step (F) are monohydric alcohols having 1 to 20 carbon atoms or 1 to 10 carbon atoms, or polyhydric alcohols having 1 to 20 carbon atoms or 1 to 10 carbon atoms. Examples of the monohydric alcohol include methanol, ethanol, n-propanol, isopropanol, n-butanol, propylene glycol monomethyl ether, isobutanol, n-pentanol, ethylene glycol monomethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, 1-octanol, 1-nonanol, 1-decanol, benzyl alcohol, 2-phenoxyethanol, 2-benzyloxyethanol, and tetrahydrofurfuryl alcohol. Examples of the polyhydric alcohol include ethylene glycol, propylene glycol, diethylene glycol, triethylene glycol, dipropylene glycol, tripropylene glycol, 1,3-butanediol, and 2,3-butanediol.

[0141] As the ketone, an aliphatic ketone can be preferably used as a ketone having 1 to 20 carbon atoms or 1 to 10 carbon atoms. Examples thereof include acetone, methyl ethyl ketone, diethyl ketone, methyl propyl ketone, methyl isobutyl ketone, methyl amyl ketone, cyclohexanone, methylcyclopentanone, isophorone, 4-hydroxy-4-methyl-2-pentanone, methyl n-propyl ketone, methyl n-butyl ketone, methyl n-amyl ketone, 2-heptanone, and acetylacetone.

[0142] As the ester, an aliphatic ester having 1 to 20 carbon atoms or 1 to 10 carbon atoms can be preferably used. For example, methyl formate, ethyl formate, propyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl acrylate, ethyl acrylate, propyl acrylate, dimethyl maleate, diethyl maleate, dipropyl maleate, dimethyl adipate, diethyl adipate, dipropyl adipate, propylene glycol monomethyl ether acetate, methyl benzoate, ethyl benzoate, butyl benzoate, dimethyl phthalate, dibutyl maleate, diethyl oxalate, dibutyl oxalate, hexyl acetate, benzyl acetate, Diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether acetate, diethyl maleate, diethyl fumarate, dipropylene glycol methyl ether acetate, 1,3-butylene glycol diacetate, propylene glycol diacetate, 1,6-hexanediol diacetate, triacetin, γ-butyrolactone, ethylene carbonate, propylene carbonate, methyl cellosolve acetate, ethyl cellosolve acetate, diethyl cellosolve acetate, phenyl cellosolve acetate, n-butyl acetate, isobutyl acetate, methyl lactate, ethyl lactate, methyl glycolate, ethyl glycolate, Butyl glycolate, methoxymethyl acetate, methoxyethyl acetate, methoxybutyl acetate, ethoxymethyl acetate, ethoxyethyl acetate, methyl-3-hydroxypropionate, ethyl-3-hydroxypropionate, methyl-3-methoxypropionate, ethyl-3-methoxypropionate, methyl-3-ethoxypropionate, ethyl-3-ethoxypropionate, methyl-2-hydroxypropionate, ethyl-2-hydroxypropionate, propyl-2-hydroxypropionate, methyl-2-methoxypropionate, ethyl-2-methoxypropionate, Ethyl-2-ethoxypropionate, methyl-2-ethoxypropionate, methyl-2-hydroxy-2-methylpropionate, ethyl-2-hydroxy-2-methylpropionate, methyl-2-methoxy-2-methylpropionate, ethyl-2-ethoxy-2-methylpropionate, 2-hydroxyethyl propionate, 2-hydroxy-2-methylethyl propionate, hydroxyethyl acetate, methyl 2-hydroxy-3-methylbutyrate, ethyl pyruvate, methyl ethyl carbitol, diethyl carbitol, diethylene glycol methyl ethyl ether, diethylene glycol diethyl ether, and the like.

[0143] As the ether, an ether having 1 to 20 carbon atoms or 1 to 10 carbon atoms, an aliphatic ether can be preferably used. For example, dimethyl ether, ethyl methyl ether, diethyl ether, tetrahydrofuran, 1,4-dioxane, anisole, 4-methoxytoluene, diethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol dimethyl ether, diethylene glycol monophenyl ether, triethylene glycol monomethyl ether, dipropylene glycol monomethyl ether, diethylene glycol butyl methyl ether, triethylene glycol dimethyl ether, tripropylene glycol monomethyl ether, 2-(2-isobutoxyethoxy)ethanol, benzyl ethyl ether, etc. can be mentioned.

[0144] As the amide, as the amide having 1 to 20 carbon atoms or 1 to 10 carbon atoms, dimethylacetamide, dimethylformamide, N-methylpyrrolidone, N-ethylpyrrolidone, N,N-dimethylisobutyramide, 1,3-dimethyl-2-imidazolidinone, N-methylformamide, N-methylformanilide, and N-methylacetamide can be listed.

[0145] Examples of hydrocarbons include paraffinic hydrocarbons, cycloparaffinic hydrocarbons, aromatic hydrocarbons, and mixtures thereof having 6 to 18 carbon atoms or 6 to 40 carbon atoms. Examples of normal paraffins include normal hexane, normal heptane, normal octane, normal nonane, normal decane, etc., examples of isoparaffins include isooctane, isononane, isodecane, etc., and examples of aromatic hydrocarbons include toluene, xylene, tetralin, cyclohexylbenzene, decylbenzene, etc.

[0146] Examples of the cyano group-containing solvent include acetonitrile and 3-methoxypropionitrile.

[0147] Examples of the halogen-containing solvent include chloroform and chlorobenzene.

[0148] Examples of the sulfonyl group-containing solvent include dimethyl sulfoxide and the like.

[0149] Examples of the carboxyl group-containing solvent include formic acid, acetic acid, acrylic acid, methacrylic acid, oleic acid, linoleic acid, linolenic acid, lactic acid, and caproic acid.

[0150] In the present invention, in step (D), the surface of the modified metal oxide particle (iii) can be coated with a silane compound.

[0151] In the present invention, a film-forming composition comprising the organic solvent sol of the modified metal oxide particles (iii) and an organic resin is obtained.

[0152] As for the organic resin, a film-forming composition is obtained by selectively mixing a thermosetting or photocurable resin. In addition, a curing agent such as an amine curing agent, an acid anhydride curing agent, a radical generator curing agent (thermal radical generator, photo radical generator), or an acid generator curing agent (thermal acid generator or photoacid generator) can be contained to form a cured product.

[0153] In the present composition, a film-forming composition comprising an organic resin and a curing agent is applied or filled on a substrate, and a cured product can be formed by heating, light irradiation or a combination thereof. As for the organic resin (curable resin), resins having functional groups such as epoxy groups or (meth) acryloyl groups, and isocyanate resins can be cited. For example, photocurable multifunctional acrylates can be preferably used.

[0154] Examples of the polyfunctional acrylate include polyfunctional acrylates having bifunctional, trifunctional, tetrafunctional, or higher functional groups in the molecule, such as neopentyl glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, and dipentaerythritol hexa(meth)acrylate.

[0155] These multifunctional acrylates can also be described below.

[0156]

Chemistry 4

[0157]

[0158]

Chemistry 5

[0159]

[0160]

Chemistry 6

[0161]

[0162]

Chemistry 7

[0163]

[0164] The film-forming composition of the present invention may contain a surfactant (leveling agent).

[0165] As the surfactant (leveling agent), anionic surfactants, cationic surfactants, amphoteric surfactants, nonionic surfactants, and silicone surfactants can be used. The surfactant (leveling agent) can be added in the range of 0.01 to 5 phr or 0.01 to 1 phr relative to the organic resin.

[0166] Examples of the anionic surfactant used in the present invention include sodium and potassium salts of fatty acids, alkylbenzene sulfonates, higher alcohol sulfate ester salts, polyoxyethylene alkyl ether sulfates, α-sulfofatty acid esters, α-olefin sulfonates, monoalkyl phosphate ester salts, and alkane sulfonates.

[0167] For example, as the alkylbenzene sulfonate, there are sodium salts, potassium salts and lithium salts, such as sodium C10-C16 alkylbenzene sulfonate, C10-C16 alkylbenzene sulfonic acid, sodium alkylnaphthalene sulfonate and the like.

[0168] Examples of higher alcohol sulfuric acid ester salts include sodium dodecyl sulfate (sodium lauryl sulfate) having 12 carbon atoms, triethanolamine lauryl sulfate, and triethanolammonium lauryl sulfate.

[0169] As for the polyoxyethylene alkyl ether sulfates, there are polyoxyethylene styrene phenyl ether sodium sulfate, polyoxyethylene styrene phenyl ether ammonium sulfate, polyoxyethylene decyl ether sodium sulfate, polyoxyethylene decyl ether ammonium sulfate, polyoxyethylene lauryl ether sodium sulfate, polyoxyethylene lauryl ether ammonium sulfate, polyoxyethylene tridecyl ether sodium sulfate, polyoxyethylene oleyl cetyl ether sodium sulfate and the like.

[0170] As the α-olefin sulfonate, there are sodium α-olefin sulfonate and the like.

[0171] Examples of the alkanesulfonate include sodium 2-ethylhexyl sulfate and the like.

[0172] Examples of the cationic surfactant used in the present invention include alkyltrimethylammonium salts, dialkyldimethylammonium salts, alkyldimethylbenzylammonium salts, and amine salt-based agents.

[0173] Alkyl trimethyl ammonium salts are quaternary ammonium salts having chloride ions and bromide ions as counter ions, and examples thereof include dodecyl trimethyl ammonium chloride, cetyl trimethyl ammonium chloride, coconut oil alkyl trimethyl ammonium chloride, and alkyl (C16-18) trimethyl ammonium chloride.

[0174] The dialkyldimethylammonium salt has two lipophilic main chains and two methyl groups. Examples thereof include di(hydrogenated tallow)dimethylammonium chloride. Examples thereof include didecyldimethylammonium chloride, dicocoalkyldimethylammonium chloride, dihydrogenated tallowalkyldimethylammonium chloride, and dialkyl(C14-18)dimethylammonium chloride.

[0175] The alkyl dimethyl benzyl ammonium salt is a quaternary ammonium salt having one lipophilic main chain, two methyl groups, and a benzyl group, and examples thereof include benzalkonium chloride. For example, alkyl (C8-18) dimethyl benzyl ammonium chloride is included.

[0176] The amine salt-based agent is a product in which the hydrogen atoms of ammonia are substituted with one or more hydrocarbon groups, and an example thereof is N-methylbishydroxyethylamine fatty acid ester hydrochloride.

[0177] As the amphoteric surfactant used in the present invention, there can be mentioned N-alkyl-β-alanine type alkylamino fatty acid salts, alkyl carboxy betaine type alkyl betaine, N, N-dimethyl dodecylamine oxide type alkyl amine oxide. Examples of these include lauryl betaine, stearyl betaine, 2-alkyl-N-carboxymethyl-N-hydroxyethyl imidazolinium betaine, and lauryl dimethyl amine oxide.

[0178] The nonionic surfactant used in the present invention is selected from polyoxyethylene alkyl ethers, polyoxyethylene alkylphenol ethers, alkyl glucosides, polyoxyethylene fatty acid esters, sucrose fatty acid esters, sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, and fatty acid alkanolamides. For example, as polyoxyethylene alkyl ethers, polyoxyethylene dodecyl ether (polyoxyethylene lauryl ether), polyoxyethylene lauryl ether, polyoxyethylene tridecyl ether, polyoxyethylene tridecyl ether, polyoxyethylene myristyl ether, polyoxyethylene cetyl ether, polyoxyethylene oleyl ether, polyoxyethylene stearyl ether, polyoxyethylene behenyl ether, polyoxyethylene-2-ethylhexyl ether, polyoxyethylene isodecyl ether, etc. can be cited.

[0179] Examples of the polyoxyethylene alkylphenol ethers include polyoxyethylene styrenated phenyl ether, polyoxyethylene nonylphenyl ether, polyoxyethylene distyrenated phenyl ether, and polyoxyethylene tribenzylphenyl ether.

[0180] Examples of the alkyl glucoside include decyl glucoside and lauryl glucoside.

[0181] Examples of the polyoxyethylene fatty acid esters include polyoxyethylene monolaurate, polyoxyethylene monostearate, polyoxyethylene monooleate, polyethylene glycol distearate, polyethylene glycol dioleate, and polypropylene glycol dioleate.

[0182] Examples of the sorbitan fatty acid esters include sorbitan monocaprylate, sorbitan monolaurate, sorbitan monomyristate, sorbitan monopalmitate, sorbitan monostearate, sorbitan distearate, sorbitan tristearate, sorbitan monooleate, sorbitan trioleate, sorbitan monosesquiolate, and ethylene oxide adducts thereof.

[0183] Examples of the polyoxyethylene sorbitan fatty acid esters include polyoxyethylene sorbitan monolaurate, polyoxyethylene sorbitan monopalmitate, polyoxyethylene sorbitan monostearate, polyoxyethylene sorbitan tristearate, polyoxyethylene sorbitan monooleate, polyoxyethylene sorbitan trioleate, and polyoxyethylene sorbitan triisostearate.

[0184] Examples of fatty acid alkanolamides include coconut oil fatty acid diethanolamide, tallow fatty acid diethanolamide, lauric acid diethanolamide, and oleic acid diethanolamide.

[0185] Furthermore, polyoxyalkyl ethers or polyoxyalkyl glycols such as polyoxyethylene polyoxypropylene glycol and polyoxyethylene fatty acid esters, polyoxyethylene hydrogenated castor oil ether, sorbitan fatty acid ester alkyl ether, alkyl polyglucosides, sorbitan monooleate, and sucrose fatty acid esters may be mentioned.

[0186] Silicone surfactants can be used. Silicone surfactants are compounds having repeating units containing siloxane bonds in the main chain. The weight average molecular weight of the silicone surfactant can be used in the range of 500 to 50,000. They may be modified silicone surfactants, and structures in which organic groups are introduced into the side chains and / or ends of polysiloxanes can be listed. Examples of the organic group include amino groups, epoxy groups, alicyclic epoxy groups, methanol groups, mercapto groups, carboxyl groups, aliphatic ester groups, aliphatic amide groups, and polyether groups. Examples of the silicone surfactant include Toray Silicone DC3PA, Toray Silicone SH7PA, Toray Silicone DC11PA, Toray Silicone SH21PA, Toray Silicone SH28PA, Toray Silicone SH29PA, Toray Silicone SH30PA, and Toray Silicone SH8400 (all manufactured by Dow Corning Toray Co., Ltd.), Silwet L-77, L-7280, L-7001, L-7002, L-7200, L-7210, L-7220, L-7230, L7500, L-7600, L-7602, L-7604, L-7605, L-7622, ​​L-7657, L-8500, and L-8610 (all manufactured by Momentive Performance Materials Co., Ltd.), KP-341, KF-6001, KF-6002 (all manufactured by Shin-Etsu Silicone Co., Ltd.), BYK307, BYK323, BYK330 (all manufactured by BYK-Chemie), etc. For example, as a polyether-modified silicone, trade name L-7001 (manufactured by DOWSIL) can be preferably used.

[0187] In the present invention, a film-forming composition comprising the organic solvent sol and an organic resin is obtained. The film-forming composition can be prepared by removing the organic solvent from the organic solvent sol to obtain a film-forming composition comprising modified metal oxide particles (iii) and an organic resin.

[0188] In the case of a thermosetting film-forming composition, a thermosetting agent may be added in a range of 0.01 to 50 phr or 0.01 to 10 phr relative to the resin containing a functional group such as an epoxy group or a (meth)acryloyl group. For example, the thermosetting agent may be contained in a ratio of 0.5 to 1.5 equivalents, preferably 0.8 to 1.2 equivalents relative to the functional group such as an epoxy group or a (meth)acryloyl group. The equivalent of the thermosetting agent relative to the curable resin is expressed as an equivalent ratio of the thermosetting agent relative to the functional group.

[0189] Examples of the thermosetting agent include phenolic resins, amine curing agents, polyamide resins, imidazoles, polythiol, acid anhydrides, thermal radical generators, thermal acid generators, etc. Radical generator curing agents, acid anhydride curing agents, and amine curing agents are particularly preferred.

[0190] Even if these thermosetting agents are solid, they can be used by dissolving them in a solvent. However, evaporation of the solvent causes a decrease in density of the cured product and formation of pores, which results in a decrease in strength and water resistance. It is preferred that the curing agent itself is liquid at room temperature and pressure.

[0191] Examples of the phenol resin include phenol novolac resin and cresol novolac resin.

[0192] Examples of the amine curing agent include piperidine, N,N-dimethylpiperazine, triethylenediamine, 2,4,6-tris(dimethylaminomethyl)phenol, benzyldimethylamine, 2-(dimethylaminomethyl)phenol, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, diethylaminopropylamine, N-aminoethylpiperazine, di(1-methyl-2-aminocyclohexyl)methane, menthene diamine, isophoronediamine, diaminodicyclohexylmethane, 1,3-diaminomethylcyclohexane, xylenediamine, m-phenylenediamine, diaminodiphenylmethane, diaminodiphenylsulfone, 3,3'-diethyl-4,4'-diaminodiphenylmethane, and diethyltoluenediamine. Among these, liquid diethylenetriamine, triethylenetetramine, tetraethylenepentamine, diethylaminopropylamine, N-aminoethylpiperazine, di(1-methyl-2-aminocyclohexyl)methane, menthene diamine, isophoronediamine, diaminodicyclohexylmethane, 3,3′-diethyl-4,4′-diaminodiphenylmethane, diethyltoluenediamine and the like can be preferably used.

[0193] The polyamide resin is a polyamide amine produced by condensation of a dimer acid and a polyamine and having a primary amine and a secondary amine in the molecule.

[0194] Examples of the imidazoles include 2-methylimidazole, 2-ethyl-4-methylimidazole, 1-cyanoethyl-2-undecylimidazolium trimellitate, and epoxyimidazole adducts.

[0195] Polythiol is, for example, a substance having a thiol group at the end of a polypropylene glycol chain or a substance having a thiol group at the end of a polyethylene glycol chain, and is preferably in a liquid state.

[0196] As the acid anhydride curing agent, the acid anhydride of a compound having a plurality of carboxyl groups in one molecule is preferred. As these acid anhydride curing agents, phthalic anhydride, trimellitic anhydride, pyromellitic anhydride, benzophenone tetracarboxylic anhydride, ethylene glycol ditrimellitate, glycerol trimellitate, maleic anhydride, tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, endomethylene tetrahydrophthalic anhydride, methyl endomethylene tetrahydrophthalic anhydride, methylbutenyl tetrahydrophthalic anhydride, dodecenyl succinic anhydride, hexahydrophthalic anhydride, methylhexahydrophthalic anhydride, succinic anhydride, methylcyclohexene dicarboxylic anhydride, chlorendic anhydride, etc. can be listed.

[0197] Examples of the thermal acid generator include sulfonium salts and phosphonium salts, and sulfonium salts are preferably used. For example, the following compounds can be exemplified.

[0198]

Chemistry 8

[0199]

[0200] Examples of R include an alkyl group having 1 to 12 carbon atoms and an aryl group having 6 to 20 carbon atoms, and an alkyl group having 1 to 12 carbon atoms is particularly preferred.

[0201] Among these, methyltetrahydrophthalic anhydride, methyl-5-norbornene-2,3-dicarboxylic anhydride (methylnadic anhydride, methylnadic anhydride), hydrogenated methylnadic anhydride, methylbutenyltetrahydrophthalic anhydride, dodecenylsuccinic anhydride, methylhexahydrophthalic anhydride, and a mixture of methylhexahydrophthalic anhydride and hexahydrophthalic anhydride, which are liquid at room temperature and pressure, are preferred. The viscosity of these liquid anhydrides is about 10 to 1000 mPa·s when measured at 25°C.

[0202] Examples of thermal radical generators include 2,2'-azobis(isobutyronitrile), 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobis(2-methylpropionic acid) dimethyl ester, 2,2'-azobis(2-methylpropionamidine) dihydrochloride, 2,2'-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride, tert-butyl hydroperoxide, cumene hydroperoxide, di-tert-butyl peroxide, dicumyl peroxide, benzoyl peroxide, etc. These can be obtained from Tokyo Chemical Industry Co., Ltd.

[0203] In addition, when obtaining the above-mentioned cured product, a curing aid can be appropriately used in combination. As the curing aid, organic phosphorus compounds such as triphenylphosphine and tributylphosphine, quaternary phosphonium salts such as ethyltriphenylphosphonium bromide and diethyl methyltriphenylphosphonium phosphate, 1,8-diazabicyclo (5,4,0) undec-7-ene, 1,8-diazabicyclo (5,4,0) undec-7-ene and octanoic acid salts, zinc octanoate, tetrabutylammonium bromide and other quaternary ammonium salts can be listed. These curing aids can be contained in a ratio of 0.001 to 0.1 parts by mass relative to 1 part by mass of the curing agent.

[0204] As for the composition, a resin, a curing agent and a curing aid as required are mixed to obtain a thermosetting varnish. The mixing can be carried out in a reaction vessel using a stirring blade or a kneader. The mixing is carried out by a heating mixing method at a temperature of 60 to 100° C. for 0.5 to 1 hour.

[0205] The obtained curable film-forming composition is a thermosetting coating composition, for example, having an appropriate viscosity for use as a liquid sealing material. The liquid thermosetting film-forming composition can be prepared to have any viscosity, and in order to be used as a transparent sealing material for LEDs, etc. by casting, pouring, dispenser, printing, etc., it can be partially sealed at any part thereof. The liquid thermosetting composition is directly installed on an LED, etc. in a liquid state by the above-mentioned method, and then dried and cured to obtain an epoxy resin cured body.

[0206] A cured product is obtained by applying a thermosetting film-forming composition (thermosetting coating composition) to a substrate and heating the substrate at a temperature of 80 to 200°C.

[0207] In the case of the above-mentioned film-forming composition, in the case of a photocurable resin composition, a photocuring agent (photoradical generator, photoacid generator) can be added in the range of 0.01 to 50 phr or 0.01 to 10 phr relative to the resin containing functional groups such as epoxy groups or (meth) acryloyl groups. For example, the photocuring agent (photoradical generator, photoacid generator) can be contained in a ratio of 0.5 to 1.5 equivalents, preferably 0.8 to 1.2 equivalents relative to the functional groups such as epoxy groups or (meth) acryloyl groups. The equivalent of the photocuring agent relative to the curable resin is represented by the equivalent ratio of the photocuring agent relative to the functional group.

[0208] The photoradical generator is not particularly limited as long as it generates radicals directly or indirectly by light irradiation.

[0209] As the photoradical generator, as the photoradical polymerization initiator, for example, imidazole compounds, diazo compounds, bisimidazole compounds, N-arylglycine compounds, organic azide compounds, titanocene compounds, aluminate compounds, organic peroxides, N-alkoxypyridinium salt compounds, and thioxanthone compounds can be listed. As the azide compound, p-azidobenzaldehyde, p-azidoacetophenone, p-azidobenzoic acid, p-azidobenzylideneacetophenone, 4,4'-diazidechalcone, 4,4'-diazidediphenylsulfide, and 2,6-bis(4'-azidobenzylidene)-4-methylcyclohexanone can be listed. As the diazo compound, 1-diazo-2,5-diethoxy-4-p-tolylmercaptobenzene fluoroborate, 1-diazo-4-N,N-dimethylaminobenzene chloride, and 1-diazo-4-N,N-diethylaminobenzene fluoroborate can be listed. Examples of the bisimidazole compound include 2,2'-bis(o-chlorophenyl)-4,5,4',5'-tetrakis(3,4,5-trimethoxyphenyl)1,2'-bisimidazole and 2,2'-bis(o-chlorophenyl)4,5,4',5'-tetraphenyl-1,2'-bisimidazole. Examples of the titanocene compound include dicyclopentadienyl-titanium-dichloride, dicyclopentadienyl-titanium-bisphenyl, dicyclopentadienyl-titanium-bis(2,3,4,5,6-pentafluorophenyl), dicyclopentadienyl-titanium-bis(2,3,5,6-tetrafluorophenyl), dicyclopentadienyl-titanium-bis(2,4,6-trifluorophenyl), dicyclopentadienyl-titanium-bis(2,6-di ... Dicyclopentadienyl-titanium-bis(2,4-difluorophenyl), bis(methylcyclopentadienyl)-titanium-bis(2,3,4,5,6-pentafluorophenyl), bis(methylcyclopentadienyl)-titanium-bis(2,3,5,6-tetrafluorophenyl), bis(methylcyclopentadienyl)-titanium-bis(2,6-difluorophenyl), and dicyclopentadienyl-titanium-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)-phenyl), etc.

[0210] Examples of the photoradical generator include 1,3-di(tert-butyldioxycarbonyl)benzophenone, 3,3',4,4'-tetra(tert-butyldioxycarbonyl)benzophenone, 3-phenyl-5-isoxazolone, 2-mercaptobenzimidazole, 2,2-dimethoxy-1,2-diphenylethane-1-one, 1-hydroxy-cyclohexyl-phenyl-ketone, and 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone.

[0211] As these photoradical polymerization agents, for example, they can be obtained as Irgacure TPO manufactured by BASF (the component is 2,4,6-trimethylbenzoyldiphenylphosphine oxide) (c1-1-1), Omnirad819 manufactured by IGM RESINS (the component is bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide) (c1-1-2), and Irgacure 184 manufactured by IGM RESINS (the component is 1-hydroxycyclohexyl phenyl ketone) (c1-1-3).

[0212]

Chemistry 1

[0213]

[0214] The photoacid generator is not particularly limited as long as it generates acid directly or indirectly by light irradiation. Specific examples of the photoacid generator include triazine compounds, acetophenone derivative compounds, disulfone compounds, diazomethane compounds, sulfonic acid derivative compounds, onium salts such as iodonium salts, sulfonium salts, phosphonium salts, and selenonium salts, metallocene complexes, and iron arene complexes.

[0215] As for the onium salt used as the above-mentioned photoacid generator, examples of the iodonium salt include diphenyliodonium chloride, diphenyliodonium trifluoromethanesulfonate, diphenyliodonium methanesulfonate, diphenyliodonium toluenesulfonate, diphenyliodonium bromide, diphenyliodonium tetrafluoroborate, diphenyliodonium hexafluoroantimonate, diphenyliodonium hexafluoroarsenate, bis(p-tert-butylphenyl)iodonium hexafluorophosphate, bis(p-tert-butylphenyl)iodonium methanesulfonate, bis(p-tert-butylphenyl)iodonium toluenesulfonate, bis(p-tert-butylphenyl)iodonium trifluoromethanesulfonate, bis(p-tert-butylphenyl)iodonium )iodonium tetrafluoroborate, bis(p-tert-butylphenyl)iodonium chloride, bis(p-chlorophenyl)iodonium chloride, bis(p-chlorophenyl)iodonium tetrafluoroborate, further bis(alkylphenyl)iodonium salts such as bis(4-tert-butylphenyl)iodonium hexafluorophosphate, alkoxycarbonylalkoxy-trialkylaryliodonium salts (for example, 4-[(1-ethoxycarbonyl-ethoxy)phenyl]-(2,4,6-trimethylphenyl)-iodonium hexafluorophosphate, etc.), bis(alkoxyaryl)iodonium salts (for example, bis(alkoxyphenyl)iodonium salts such as (4-methoxyphenyl)phenyliodonium hexafluoroantimonate).

[0216] Examples of the sulfonium salt include triphenylsulfonium chloride, triphenylsulfonium bromide, tri(p-methoxyphenyl)sulfonium tetrafluoroborate, tri(p-methoxyphenyl)sulfonium hexafluorophosphate, tri(p-ethoxyphenyl)sulfonium tetrafluoroborate, triphenylsulfonium trifluoromethanesulfonate, triphenylsulfonium hexafluoroantimonate, and triphenylsulfonium hexafluorophosphate; and sulfonium salts such as (4-phenylthiophenyl)diphenylsulfonium hexafluoroantimonate, (4-phenylthiophenyl)diphenylsulfonium hexafluorophosphate, bis[4-(diphenylsulfonyl)phenyl]sulfide-bis-hexafluoroantimonate, bis[4-(diphenylsulfonyl)phenyl]sulfide-bis-hexafluorophosphate, and (4-methoxyphenyl)diphenylsulfonium hexafluoroantimonate.

[0217] Examples of the phosphonium salt include triphenylphosphonium chloride, triphenylphosphonium bromide, tri(p-methoxyphenyl)phosphonium tetrafluoroborate, tri(p-methoxyphenyl)phosphonium hexafluorophosphate, tri(p-ethoxyphenyl)phosphonium tetrafluoroborate, 4-chlorobenzenediazonium hexafluorophosphate, and benzyltriphenylphosphonium hexafluoroantimonate.

[0218] Examples thereof include selenonium salts such as triphenylselenium hexafluorophosphate and metallocene complexes such as (η5 or η6-isopropylbenzene)(η5-cyclopentadienyl)iron(II) hexafluorophosphate.

[0219] In addition, the following compounds can also be used as the photoacid generator.

[0220]

Chemistry 10

[0221]

[0222]

Chemistry 11

[0223]

[0224]

Chemistry 12

[0225]

[0226]

Chemistry 13

[0227]

[0228]

Chemistry 14

[0229]

[0230]

Chemistry 15

[0231]

[0232]

Chemistry 16

[0233]

[0234]

Chemistry 17

[0235]

[0236]

Chemistry 18

[0237]

[0238] As the photoacid generator, sulfonium salt compounds and iodonium salt compounds are preferred. As their anion species, CF3SO3 can be listed. - 、C4F9SO3 - 、C8F 17 SO3 - , camphorsulfonic acid anion, toluenesulfonic acid anion, BF4 - PF6 - 、AsF6 - and SbF6 - etc. Anionic species such as phosphorus hexafluoride and antimony hexafluoride which exhibit strong acidity are particularly preferred.

[0239] The film-forming composition of the present invention may contain conventional additives as required. As such additives, for example, pigments, colorants, thickeners, sensitizers, defoamers, coating improvers, lubricants, stabilizers (antioxidants, heat stabilizers, light stabilizers, etc.), plasticizers, dissolution promoters, fillers, antistatic agents, etc., may be cited. These additives may be used alone or in combination of two or more.

[0240] Examples of the coating method of the film-forming composition of the present invention include flow coating, spin coating, spray coating, screen printing, casting, bar coating, curtain coating, roll coating, gravure coating, dipping, and slit coating.

[0241] In the present invention, the photo-coating composition (film-forming composition) can be applied on a substrate and cured by light irradiation. In addition, heating can be performed before or after light irradiation.

[0242] The thickness of the coating film can be selected from a range of about 0.01 μm to 10 mm depending on the use of the cured product. For example, when used in a photoresist, it can be set to about 0.05 to 10 μm (especially 0.1 to 5 μm); when used in a printed wiring substrate, it can be set to about 5 μm to 5 mm (especially 100 μm to 1 mm); when used in an optical film, it can be set to about 0.1 to 100 μm (especially 0.3 to 50 μm).

[0243] When a transparent film is obtained, the visible light transmittance of the film can be 80% or more, or 90% or more, typically 90 to 96%.

[0244] When using a photoacid generator, the irradiation or exposure light may be, for example, gamma rays, X-rays, ultraviolet rays, visible rays, etc., and usually, it is mostly visible light or ultraviolet rays, especially ultraviolet rays. The wavelength of the light is, for example, 150 to 800 nm, preferably 150 to 600 nm, and more preferably about 150 to 400 nm. The irradiation light amount varies depending on the thickness of the coating film, and can be, for example, 2 to 20,000 mJ / cm 2 , preferably 5 to 5000 mJ / cm 2 As a light source, it can be selected according to the type of exposure light. For example, in the case of ultraviolet rays, a low-pressure mercury lamp, a high-pressure mercury lamp, an ultra-high-pressure mercury lamp, a deuterium lamp, a halogen lamp, a laser (helium-cadmium laser, excimer laser, etc.) can be used. By such light irradiation, the curing reaction of the above-mentioned composition proceeds.

[0245] When a thermal acid generator is used, heating of the coating film after light irradiation using a photoacid generator as required is performed, for example, at 60 to 350° C., preferably at about 100 to 300° C. The heating time can be selected from a range of 3 seconds or more (for example, about 3 seconds to 5 hours), for example, 5 seconds to 2 hours, preferably about 20 seconds to 30 minutes, and usually about 1 minute to 3 hours (for example, 5 minutes to 2.5 hours).

[0246] Furthermore, in the case of forming a pattern or an image (for example, in the case of manufacturing a printed wiring board, etc.), the coating film formed on the substrate can be subjected to pattern exposure, and the pattern exposure can be performed by scanning with a laser or by irradiating light through a photomask. The non-irradiated area (unexposed portion) generated by such pattern exposure is developed (or dissolved) with a developer, thereby forming a pattern or an image.

[0247] As the developer, an aqueous alkaline solution or an organic solvent can be used.

[0248] Examples of the aqueous alkali solution include aqueous solutions of alkali metal hydroxides such as potassium hydroxide, sodium hydroxide, potassium carbonate, and sodium carbonate; aqueous solutions of quaternary ammonium hydroxides such as tetramethylammonium hydroxide, tetraethylammonium hydroxide, and choline; and aqueous solutions of amines such as ethanolamine, propylamine, and ethylenediamine.

[0249] The alkaline developer is generally an aqueous solution of 10% by mass or less, preferably 0.1 to 3.0% by mass. Furthermore, alcohols and surfactants may be added to the developer, preferably 0.05 to 10 parts by mass, each based on 100 parts by mass of the developer.

[0250] Among them, a 0.1 to 2.38 mass % aqueous solution of tetramethylammonium hydroxide can be used.

[0251] In addition, as the organic solvent of the developer, a general organic solvent can be used, for example, acetone, acetonitrile, toluene, dimethylformamide, methanol, ethanol, isopropanol, propylene glycol methyl ether, propylene glycol ethyl ether, propylene glycol propyl ether, propylene glycol butyl ether, propylene glycol methyl ether acetate, propylene glycol ethyl ether acetate, propylene glycol propyl ether acetate, propylene glycol butyl ether acetate, ethyl lactate, cyclohexanone, etc. These can be used alone or as a mixture of two or more. In particular, propylene glycol methyl ether, propylene glycol methyl ether acetate, ethyl lactate, etc. can be preferably used.

[0252] In the present invention, in order to improve the adhesion to the substrate after development, a adhesion promoter may be added. As for these adhesion promoters, chlorosilanes such as trimethylchlorosilane, dimethylvinylchlorosilane, methyldiphenylchlorosilane, and chloromethyldimethylchlorosilane, alkoxysilanes such as trimethylmethoxysilane, dimethyldiethoxysilane, methyldimethoxysilane, dimethylvinylethoxysilane, diphenyldimethoxysilane, and phenyltriethoxysilane, hexamethyldisilazane, N,N'-bis(trimethylsilyl)urea, dimethyltrimethylsilylamine, trimethylsilylimidazole, and vinyltrimethoxysilane may be cited. Silanes such as chlorosilane, 3-chloropropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-(N-piperidyl)propyltrimethoxysilane, benzotriazole, benzimidazole, indazole, imidazole, 2-mercaptobenzimidazole, 2-mercaptobenzothiazole, 2-mercaptobenzoxazole, urea, thiouracil, mercaptoimidazole, mercaptopyrimidine, urea such as 1,1-dimethylurea, 1,3-dimethylurea, or thiourea compounds. One or more of the above-mentioned adhesion promoters can be used in combination. The amount of these adhesion promoters added is usually 18% by mass or less in the solid content, preferably 0.0008 to 9% by mass, and more preferably 0.04 to 9% by mass.

[0253] In the present invention, sensitizers can be included. As sensitizers that can be used, anthracene, phenothiazine, perylene, thioxanthone, benzophenone thioxanthone etc. can be listed. And then, as sensitizing pigments, thiopyranium salt pigments, merocyanine pigments, quinoline pigments, styrylquinoline pigments, coumarin ketone pigments, thioxanthene pigments, xanthene pigments, oxo alcohol (Oxonol) pigments, cyanine pigments, rhodamine pigments, pyrylium salt pigments etc. can be exemplified. Particularly preferably, anthracene sensitizers are used, and by using a cationic curing catalyst (radioactive cationic polymerization initiator), sensitivity is greatly improved, and also free radical polymerization initiation function is also provided, and for the mixed type using the cationic curing system of the present invention and the free radical curing system, catalyst species can be simply obtained. As a specific anthracene compound, dibutoxyanthracene, dipropoxyanthraquinone etc. are effective. The sensitizer is used in an amount of 0.01 to 20% by mass, preferably 0.01 to 10% by mass, based on the solid content.

[0254] The composition of the present invention can be photocured or thermally cured using a photoradical generator, a thermal radical generator, a photoacid generator, or a thermal acid generator. When a photoacid generator or a thermal acid generator is used, for example, a commonly used epoxy curing agent (e.g., amine, anhydride) is not used or even if it is used, its content is extremely small, so the storage stability of the present composition is improved.

[0255] It has been found that the composition can be used in a photocationic polymerizable manner. Compared with the liquid epoxy compounds (e.g., alicyclic epoxy compounds having an epoxycyclohexyl ring) of existing products, it has a high curing speed. Due to the high curing speed, it is also possible to reduce the amount of acid generator added and use a weak acid acid generator. As for the reduction of the acid generator, acid active species sometimes remain after UV irradiation, which is important in preventing metal corrosion. Due to the high curing speed, thick film curing is possible.

[0256] Curing using UV irradiation can be applied to heat-sensitive materials (devices).

[0257] In the present invention, an antistatic composition comprising the modified metal oxide particles (iii) in the modified metal oxide sol can be produced.

[0258] In addition, in the present invention, a composition for an electron transport material comprising the modified metal oxide particles (iii) in the modified metal oxide sol can be produced.

[0259] For the resin varnish serving as the binder component, when a coating agent having a compounding amount of 300 phr of the modified metal oxide particles (iii) from the above-mentioned modified metal oxide sol is applied on a substrate so that the film after drying becomes a film thickness of 1.0 μm, a voltage of 1000 V is applied, and a surface resistance value of 10 to 500 GΩ / □ is displayed.

[0260] Example

[0261] The physical properties of the sol (dispersion liquid) were determined by the following measurement methods.

[0262] [Average primary particle size]

[0263] The particles were photographed using a transmission electron microscope (trade name: JEM-F200, manufactured by JEOL Ltd.), and the average value of the primary particle diameters of equivalent circles of 500 arbitrary particles was defined as the average primary particle diameter.

[0264] [Average particle size based on dynamic light scattering (dynamic light scattering particle size)]

[0265] The sol is diluted with a dispersion solvent, and the parameters of the solvent are measured using a dynamic light scattering measurement device: Zetasizer manufactured by Malvern Instruments Ltd.

[0266] [stability]

[0267] After the dispersion was stored at 50°C for 1 week, samples whose dynamic light scattering (DLS) particle size was less than 1.2 times that before the storage test were marked as unchanged and were labeled "○", and samples whose dynamic light scattering (DLS) particle size changed by 1.2 times or more compared to before the storage test were marked as "×".

[0268] [Determination of amine amount]

[0269] The amount of amine in the sol obtained in Examples and Comparative Examples was measured according to the following procedures 1) to 3).

[0270] 1) Preparation of standard samples for calibration lines

[0271] Standard samples of isopropylamine and diisopropylamine were prepared by diluting with 3 mM nitric acid so that the concentrations of isopropylamine and diisopropylamine became 10 ppm, 100 ppm, and 1000 ppm, respectively.

[0272] A standard sample of tri-n-pentylamine was prepared by diluting the sample with 3 mM nitric acid containing 20 mass % of acetonitrile so that the tri-n-pentylamine concentration became 100 ppm, 1000 ppm, and 1 mass %.

[0273] 2) Preparation of samples for quantitative determination of amine content in sols obtained in Examples and Comparative Examples

[0274] The sol obtained in the embodiment and the comparative example is diluted with pure water so that the concentration of the colloidal particles becomes 3% by mass. After adding 0.2 mL of 1M nitric acid to 8.5 g of the diluted sol, the amine adsorbed on the particle surface is peeled off from the particle surface by standing at room temperature for 24 hours. Next, the obtained solution is centrifuged using a centrifugal ultrafiltration filter unit with a molecular weight cutoff of 10,000 Da to recover the filtrate. The recovered filtrate is diluted 10 times with pure water to prepare a sample for quantifying the amount of amine in the sol obtained in the embodiment and the comparative example.

[0275] 3) Calculation of the Amount of Amine in the Sols Obtained in Examples and Comparative Examples

[0276] The samples prepared in 1) and 2) were measured using an ion chromatograph (Metrohm Japan Co., Ltd., Metrohm Compact IC 761). A calibration line was prepared by plotting the peak integrated intensity of the standard samples of isopropylamine, diisopropylamine, and tri-n-pentylamine prepared in 1) against the respective amine concentrations. The amount of amine contained in the sample prepared in 2) was calculated using the prepared calibration line.

[0277] [Determination of crystallinity]

[0278] The crystallinity of the modified metal oxide particles in the sols obtained in Examples and Comparative Examples was measured by the following procedures 1) to 3).

[0279] 1) X-ray diffraction measurement of modified metal oxide particles in sols obtained in Examples and Comparative Examples

[0280] The modified metal oxide particle-dispersed sol obtained in the example was vacuum dried at 60°C for 1 hour. The obtained dry powder was put into a mortar and crushed with a pestle. The crushed particles were mixed with tungsten powder (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., containing 99.9% by mass or more of tungsten) at a mass ratio of 50:50. The X-ray diffraction of the mixed powder was measured using an X-ray diffraction device (manufactured by Rigaku Corporation, trade name MiniFlex600).

[0281] 2) X-ray diffraction determination of tin (IV) oxide standard sample

[0282] Tin (IV) oxide powder (manufactured by Kanto Chemical Co., Ltd., containing 99.0% by mass or more of SnO2) and tungsten powder (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., containing 99.9% by mass or more of tungsten) were mixed in a mass ratio of 50:50. The X-ray diffraction of the mixed powder was measured using an X-ray diffraction device (manufactured by Rigaku Co., Ltd., trade name MiniFlex600).

[0283] 3) Calculation of crystallinity

[0284] The sum A of the peak integrated intensities of tin (IV) oxide (110), (101), (200), (211) and (220) contained in the modified metal oxide particles measured in 1) was calculated. S1 And the peak integrated intensity A of tungsten (110) W1 Next, the sum A of the peak integrated intensities of tin (IV) oxide (110), (101), (200), (211), and (220) measured in 2) is calculated. S2 , and the peak integrated intensity A of tungsten (110) W2 The crystallinity of the modified metal oxide particles obtained in Examples and Comparative Examples was calculated by the following calculation formula.

[0285] Crystallinity = (A S1 / A W1 ) / (A S2 / A W2 )

[0286] [Measurement of refractive index]

[0287] The refractive index of the modified metal oxide in the sol obtained in the examples and comparative examples was measured by the following procedures 1) to 3).

[0288] 1) Preparation of modified metal oxide methanol dispersed sol and varnish

[0289] 20.00 g of 3-glycidoxypropyltrimethoxysilane (produced by Momentive, trade name SILQUEST A-187T) was weighed in a polyethylene container, and 18.57 g of methanol and 4.57 g of 0.01 N hydrochloric acid aqueous solution were added thereto, and stirred at room temperature for 5 hours. 6.00 g of a methanol solution of 2,4-pentanedionate aluminum (Al(acac)3) (10% by mass Al(acac)3) prepared in advance was added as a curing agent, and stirred for 10 minutes to prepare a partial hydrolyzate of 3-glycidoxypropyltrimethoxysilane (concentration: 43% by mass).

[0290] The prepared partial hydrolyzate of 3-glycidoxypropyltrimethoxysilane, the modified metal oxide dispersed sol, water, methanol, and 0.25 g of a methanol solution (10% by mass of L-7604) of a leveling agent (DOWSIL trade name L-7604) were weighed into a brown bottle so that the total amount was 25.00 g, the final solvent composition was water / the total amount of solvents other than water = 1 / 4 in terms of mass ratio, and the amount of the modified metal oxide in the methanol dispersed sol was 50 phr, 100 phr, and 150 phr, and the mixture was stirred at room temperature for 30 minutes to prepare a modified metal oxide methanol dispersed sol compounded varnish (solid content concentration of 10.0% by mass, modified metal oxide compounding amount: 50 phr, 100 phr, 150 phr).

[0291] 2) Preparation of particle complex membrane

[0292] About 0.5 mL of the modified metal oxide methanol dispersion sol obtained in 1) was dripped onto a UV-O3 treated Si substrate and coated using a spin coater (Mikasa (KK) manufactured, trade name Opticoat MS-B100) so that the film thickness after coating was 1.0 μm. Then, the film was baked on a hot plate at 80° C. for 5 minutes and heat treated in an oven at 120° C. for 1 hour to prepare a particle-coated film (particle content: 50 phr, 100 phr, 150 phr).

[0293] 3) Refractive index measurement of particle-coated films and calculation of refractive index of particles

[0294] The refractive index of the particle-coated film (particle content: 50 phr, 100 phr, 150 phr) obtained in 2) was measured using an ellipsometer (manufactured by JA Woollam Japan (KK) under the trade name of multi-incident angle spectroscopic ellipsometer VASE). In addition, the refractive index of a film containing no particles, which was prepared in the same manner using only a partial hydrolyzate of 3-glycidoxypropyltrimethoxysilane, was also measured. The refractive index of the measured co-coated film was plotted against the particle content, and the refractive index of the particles was obtained by extrapolating the content of the particles to 100% by mass.

[0295] [Measurement of resistivity value]

[0296] The resistivity values ​​of the films in which the particles obtained in Examples and Comparative Examples were blended were measured in accordance with the following procedures 1) to 3).

[0297] 1) Preparation of modified metal oxide dispersion sol and varnish

[0298] 37.50 g of 3-glycidoxypropyltrimethoxysilane (produced by Momentive, trade name SILQUEST A-187T) was weighed in a polyethylene container, 8.57 g of a 0.01 N hydrochloric acid aqueous solution was added thereto, and the mixture was stirred at room temperature for 24 hours. 4.61 g of the obtained solution was weighed in a polyethylene container, 0.23 g of aluminum 2,4-pentanedionate (Al(acac)3) was added as a curing agent, and 0.50 g of a methanol solution (10 mass % L-7604) of a leveling agent (DOWSIL trade name L-7604) was added. Next, the modified metal oxide dispersion sol obtained in the examples and comparative examples, water and methanol were added so that the final solvent composition became water / total of solvents other than water = 1 / 4 in terms of mass ratio and the modified metal oxide content became 300 phr, and the mixture was stirred at room temperature for 24 hours to prepare a modified metal oxide dispersion sol varnish (solid content concentration of 15.0% by mass, modified metal oxide content of 300 phr).

[0299] 2) Preparation of particle complex membrane

[0300] About 1 mL of the modified metal oxide dispersion sol-coated varnish obtained in 1) was dropped onto a UV-O3 treated quartz substrate, and coated using a benchtop wire bar coater (manufactured by MST Co., Ltd., trade name PM-9050MC) so that the film thickness after drying was 1.0 μm. Then, the film was baked on a hot plate at 80° C. for 15 minutes and heat treated in an oven at 120° C. for 2 hours to prepare a particle-coated film.

[0301] 3) Determination of resistivity of particle-coated films

[0302] The surface resistance of the particle-blended film (particle blending amount: 300 phr) obtained in 2) was measured using a resistivity meter (trade name: Hiresta-UP MCP-HT450, manufactured by Mitsubishi Chemical Corporation) at a voltage of 1000 V and a time of 10 seconds. The unit is expressed in Ω / □ (Ohm per square).

[0303] [Qualitative and quantitative determination of tin oxide and other metal oxides]

[0304] The qualitative and quantitative determination of tin oxide and other metal oxides contained in the particles obtained in Examples and Comparative Examples was carried out by the following procedures 1) to 3).

[0305] 1) Fluorescence X-ray analysis of standard samples

[0306] Tin (IV) oxide powder (manufactured by Kanto Chemical Co., Ltd., containing more than 99.0% by mass of SnO2), antimony (V) oxide powder (Sigma-Aldrich, containing more than 99.9% by mass of Sb2O5), and silicon dioxide powder (made by Nissan Chemical Co., Ltd., trade name ST-XS, vacuum dried at 60°C for 1 hour, the obtained dry powder was put into a mortar and ground with a pestle) were mixed in a mass ratio of SnO2 / Sb2O5 / SiO2 = 1 / 1 / 1. The obtained powder was measured using a fluorescent X-ray analyzer (manufactured by Rigaku Co., Ltd., trade name Supermini200). The peak integrated intensity A from tin (IV) oxide was calculated. Sn1 , the peak integrated intensity A from antimony oxide (V) Sb1 and the peak integrated intensity A from silica Si1 .

[0307] 2) Fluorescent X-ray Analysis of Modified Metal Oxides in Sols Obtained in Examples and Comparative Examples

[0308] The modified metal oxide-dispersed sol obtained in the examples and comparative examples was vacuum dried at 60°C for 1 hour. The obtained dry powder was put into a mortar and pulverized with a pestle. The pulverized particles were measured using a fluorescent X-ray analyzer (manufactured by Rigaku Corporation, trade name Supermini200).

[0309] 3) Qualitative and quantitative determination of tin oxide and other metal oxides

[0310] If the peak wavelength of the fluorescent X-ray measured in 2) is the same as the peak wavelength of the standard sample measured in 1), it is determined that the metal oxide originating from the peak wavelength is contained. Next, the peak integrated intensity A derived from tin (IV) oxide of the fluorescent X-ray measured in 2) is calculated. Sn2 , the peak integrated intensity A from antimony oxide (V) Sb2 and the peak integrated intensity A from silica Si2 Tin oxide and other metal oxides contained in the modified metal oxides obtained in Examples and Comparative Examples were quantitatively determined by the following calculation formula.

[0311] Tin oxide content = (A Sn2 / A Sn1 ) / A 合计

[0312] Antimony oxide (V) content = (A Sb2 / A Sb1 ) / A 合计

[0313] Silicon dioxide content = (ASi2 / A Si1 ) / A 合计

[0314] wherein, A 合计 = (A Sn2 / A Sn1 ) + (A Sb2 / A Sb1 ) + (A Si2 / A Si1 )

[0315] (Reference Example 1) Preparation of Tin Oxide Composite Oxide Colloidal Particles (i) as the Core

[0316] Dissolve 37.5 kg of oxalic acid ((COOH)2·2H2O) in 363 kg of pure water, heat it to 70 °C with stirring, and add 170 kg of 35% hydrogen peroxide solution and 75 kg of metallic tin. The addition of hydrogen peroxide solution and metallic tin is carried out alternately. Initially, add 10 kg of 35% hydrogen peroxide solution, and then add 5 kg of metallic tin. After the reaction ends (5 - 10 minutes), repeat this operation. After adding all the amounts, further add 10 kg of 35% hydrogen peroxide solution. The addition takes 3 hours. After the addition is completed, further heat at 95 °C for 1 hour to complete the reaction.

[0317] Add 231 kg of 35% hydrogen peroxide solution and 52 kg of pure water to 629 kg of the obtained sol, and dilute it to be 10% by mass in terms of SnO2 and with the molar ratio of H2O2 / (COOH)2 being 8.0 relative to the oxalic acid at the time of feeding, and carry out aging at 95 °C for 5 hours. By this operation, the oxalic acid contained is decomposed into carbon dioxide and water by reaction with hydrogen peroxide. After cooling the obtained tin oxide slurry to about 40 °C, add 2.7 kg of isopropylamine (water solubility 1000 g / L, cited from the data recorded in Chemical Book. It can be referred to the website of the following URL. https: / / www.chemicalbook.com / ProductList_En.aspx?kwd = isopropylamine), peptize it, then pass the solution through and circulate it in a catalyst tower filled with about 15 L of a platinum-based catalyst (N - 220, manufactured by Süd - Chemie Catalyst Co., Ltd.) to decompose the excess hydrogen peroxide. Carry out circulation for 5 hours at a liquid passing speed of about 30 L / minute. Further, pass the solution through a column filled with an anion exchange resin and then concentrate it by the ultrafiltration membrane method. The obtained sol is a water-dispersed sol of tin oxide colloidal particles (i), with a pH of 11.0 and a SnO2 concentration of 10.0% by mass. By observation using a transmission electron microscope, the primary particle size is 10 - 15 nm.

[0318] (Reference Example 2) Preparation of Silica-Tin Oxide Composite Oxide Colloidal Particles (ii-2) as Coating

[0319] 77.2 g of JIS No. 3 sodium silicate (29.8% by mass in terms of SiO2) was dissolved in 668.8 g of pure water, and then 20.9 g of sodium stannate NaSnO3·H2O (55.1% by mass in terms of SnO2) was dissolved. The obtained aqueous solution was passed through a column filled with a hydrogen-type cation exchange resin. Next, 7.2 g of diisopropylamine (water solubility 100 g / L, quoted from the data recorded in Chemical Book. The website of the following URL can be referred to. https: / / www.chemicalbook.com / ProductList_En.aspx?kwd=108-18-9) was added to the obtained water-dispersed sol. The obtained sol was a water-dispersed sol of silica-tin oxide composite oxide colloidal particles (ii-2), with a pH of 8.0 and a total metal oxide concentration (SnO2 and SnO2) of 2.5% by mass. The primary particle size was 1 to 4 nm as observed by a transmission electron microscope.

[0320] (Reference Example 3) Preparation of antimony pentoxide colloidal particles (ii-1) as a coating

[0321] 12.5 kg of antimony trioxide (99.5% by mass as Sb2O3), 66.0 kg of pure water and 12.5 kg of potassium hydroxide (95% by mass as KOH) were added to a 100 L container, and 8.4 kg of 35% hydrogen peroxide was slowly added under stirring. 17.6 kg of the obtained aqueous solution of potassium antimonate was diluted to 2.2% by mass and passed through a column filled with a hydrogen-type cation exchange resin. 0.25 kg of diisopropylamine was added to the solution of antimonic acid after ion exchange under stirring. The obtained sol was a water-dispersed sol of antimony pentoxide colloidal particles (ii-1) with a pH of 10.8 and a Sb2O5 concentration of 1.5% by mass. The primary particle size was 1 to 10 nm as observed by a transmission electron microscope.

[0322] (Production Example 1) Preparation of Tin Oxide Colloidal Particles (iii-2-1) Coated with Silicon Dioxide-Tin Oxide Composite Oxide

[0323] The water-dispersed sol of the alkaline tin oxide colloidal particles (i) prepared in Reference Example 1 was continuously subjected to a hydrothermal treatment at a treatment temperature of 310° C., a treatment pressure of 20 MPa, and an average flow rate of 0.6 L / min. Next, 400 g of the water-dispersed sol of the silica-tin oxide composite oxide colloidal particles (ii-2) prepared in Reference Example 2 (total metal oxide concentration (SnO2 and SnO2) of 10 g, 10% by mass relative to the core particles) was added to 1000 g of the water-dispersed sol of the alkaline tin oxide colloidal particles obtained (100 g in terms of SnO2) under stirring, and then aged at 95° C. for 2 hours to obtain a water-dispersed sol of the tin oxide colloidal particles (iii-2-1) coated with the silica-tin oxide composite oxide. Next, the obtained water-dispersed sol was passed through a column filled with a hydrogen-type cation exchange resin. To the obtained water-dispersed sol, 3.5 g of tri-n-pentylamine (water solubility is 0.02 g / L, quoted from the data recorded on the homepage of Ambeed. The website can be referred to at the following URL: https: / / www.ambeed.com / products / 621-77-2.html) was added, and concentrated by ultrafiltration. The obtained sol is a water-dispersed sol of tin oxide colloidal particles (iii-2-1) coated with a silica-tin oxide composite oxide, with a pH of 5.5, a total metal oxide (SnO2 and SiO2) concentration of 30.5% by mass, an average particle size (dynamic light scattering particle size) of 19 nm by dynamic light scattering (DLS), and (total mass of metal oxides other than tin oxide) / (mass of tin oxide) = 0.065.

[0324] (Production Example 2) Preparation of Tin Oxide Colloidal Particles (iii-2-2) Coated with Silicon Dioxide-Tin Oxide Composite Oxide

[0325] A sol was prepared in the same manner as in Production Example 1, except that the amount of the water-dispersed sol of silica-tin oxide composite oxide colloidal particles added was changed to 800 g (the total metal oxide concentration (SnO2 and SnO2) was 20 g, 20% by mass relative to the core particles). The obtained sol was a water-dispersed sol of tin oxide colloidal particles (iii-2-2) coated with silica-tin oxide composite oxide, and had a pH of 5.5, a total metal oxide (SnO2 and SiO2) concentration of 30.5% by mass, an average particle size (dynamic light scattering particle size) obtained by dynamic light scattering (DLS) of 25 nm, and (total mass of metal oxides other than tin oxide) / (mass of tin oxide)=0.125.

[0326] (Production Example 3) Preparation of Tin Oxide Colloidal Particles (iii-1-1) Coated with Antimony Pentoxide Colloidal Particles

[0327] The water-dispersed sol of the alkaline tin oxide colloidal particles (i) prepared in Reference Example 1 was continuously subjected to a hydrothermal treatment at a treatment temperature of 310° C., a treatment pressure of 20 MPa, and an average flow rate of 0.6 L / min. Next, 400 g of the water-dispersed sol of the antimony pentoxide colloidal particles (ii-1) prepared in Reference Example 3 (6.0 g in terms of Sb2O5, 5.0% by mass relative to the core particles) was added to 1200 g of the water-dispersed sol of the alkaline tin oxide colloidal particles obtained (120 g in terms of SnO2) under stirring, and then aged at 95° C. for 2 hours to obtain a water-dispersed sol of the tin oxide colloidal particles (iii-1-1) coated with the antimony pentoxide colloidal particles. Next, the obtained water-dispersed sol was passed through a column filled with a hydrogen-type cation exchange resin. 3.8 g of tri-n-pentylamine was added to the obtained water-dispersed sol, and the sol was concentrated by an ultrafiltration membrane method. The obtained sol is a water-dispersed sol of tin oxide colloidal particles (iii-1-1) coated with antimony pentoxide colloidal particles, with a pH of 4.2, a total metal oxide (SnO2 and Sb2O5) concentration of 20.5 mass%, an average particle size (dynamic light scattering particle size) of 20 nm using the dynamic light scattering method (DLS), and (total mass of metal oxides other than tin oxide) / (mass of tin oxide) = 0.05.

[0328] (Production Example 4) Preparation of Tin Oxide Colloidal Particles (iii-2-3) Coated with Silicon Dioxide-Tin Oxide Composite Oxide

[0329] A sol was prepared in the same manner as in Preparation Example 1 except that the hydrothermal treatment temperature was changed to 240° C. and the treatment pressure was changed to 7.0 MPa. The obtained sol was a water-dispersed sol of tin oxide colloidal particles (iii-2-3) coated with a silica-tin oxide composite oxide, with a pH of 5.5, a total metal oxide (SnO2 and SiO2) concentration of 30.5% by mass, an average particle size (dynamic light scattering particle size) obtained by a dynamic light scattering method (DLS) of 23 nm, and (total mass of metal oxides other than tin oxide) / (mass of tin oxide)=0.125.

[0330] (Production Example 5) Preparation of Tin Oxide Colloidal Particles (iii-2-4) Coated with Silicon Dioxide-Tin Oxide Composite Oxide

[0331] A sol was prepared in the same manner as in Preparation Example 1 except that the hydrothermal treatment temperature was changed to 150° C. and the treatment pressure was changed to 1.0 MPa. The obtained sol was a water-dispersed sol of tin oxide colloidal particles (iii-2-4) coated with a silica-tin oxide composite oxide, with a pH of 5.5, a total metal oxide (SnO2 and SiO2) concentration of 30.5% by mass, an average particle size (dynamic light scattering particle size) obtained by a dynamic light scattering method (DLS) of 21 nm, and (total mass of metal oxides other than tin oxide) / (mass of tin oxide)=0.125.

[0332] (Production Example 6) Preparation of Tin Oxide Colloidal Particles (iii-2-5) Coated with Silica-Tin Oxide Composite Oxide

[0333] A sol was prepared in the same manner as in Preparation Example 1 except that the hydrothermal treatment was not performed in Preparation Example 1. The obtained sol was a water-dispersed sol of tin oxide colloidal particles (iii-2-5) coated with a silicon dioxide-tin oxide composite oxide, with a pH of 5.5, a total metal oxide (SnO2 and SiO2) concentration of 30.5% by mass, an average particle size (dynamic light scattering particle size) obtained by a dynamic light scattering method (DLS) of 20 nm, and (total mass of metal oxides other than tin oxide) / (mass of tin oxide)=0.125.

[0334] (Comparative Production Example 1) Preparation of Tin Oxide Colloidal Particles (iii-3) Coated with Silicon Dioxide-Tin Oxide Composite Oxide

[0335] A sol was prepared in the same manner as in Preparation Example 1 except that tri-n-pentylamine was not added. The obtained sol was a water-dispersed sol of tin oxide colloidal particles (iii-3) coated with a silica-tin oxide composite oxide, with a pH of 4.2, a total metal oxide (SnO2 and SiO2) concentration of 20.5% by mass, an average particle size (dynamic light scattering particle size) obtained by a dynamic light scattering method (DLS) of 28 nm, and (total mass of metal oxides other than tin oxide) / (mass of tin oxide)=0.125.

[0336] (Example 1)

[0337] 100 g of the water-dispersed sol of tin oxide colloidal particles (iii-2-1) coated with silica-tin oxide composite oxide obtained in Production Example 1 was replaced with methanol using a rotary evaporator to obtain a methanol-dispersed sol of tin oxide colloidal particles (iii-2-1) coated with silica-tin oxide composite oxide. The pH of the obtained sol was 4.7 (diluted with water of the same mass as methanol), the total metal oxide (SnO2 and SiO2) concentration was 20.5% by mass, the average particle size based on the dynamic light scattering method (DLS) (dynamic light scattering method particle size) was 16 nm, the stability test result of the sol was "0", the residual tri-n-pentylamine in the methanol dispersed sol of the particle (iii-2-1) was 3900 ppm, the diisopropylamine was 180 ppm, and the isopropylamine was 24 ppm. The crystallinity of the core particle (i) was 92%, the refractive index of the particle (iii-2-1) was 1.91, and the resistivity of the particle (iii-2-1) in the coating was 1.1×10 11 Ω / □. The mass ratio of amine (b) / amine (a) is 19.1.

[0338] (Example 2)

[0339] 100 g of the water-dispersed sol of tin oxide colloidal particles (iii-2-2) coated with silica-tin oxide composite oxide obtained in Production Example 2 was replaced with methanol using a rotary evaporator to obtain a methanol-dispersed sol of tin oxide colloidal particles (iii-2-2) coated with silica-tin oxide composite oxide. The pH of the obtained sol was 4.8 (diluted with water of the same mass as methanol), the total metal oxide (SnO2 and SiO2) concentration was 20.5% by mass, the average particle size based on the dynamic light scattering method (DLS) (dynamic light scattering method particle size) was 21 nm, the stability test result of the sol was "0", the residual tri-n-pentylamine in the methanol dispersed sol of the particle (iii-2-2) was 4200 ppm, the diisopropylamine was 190 ppm, and the isopropylamine was 22 ppm. The crystallinity of the core particle (i) was 91%, the refractive index of the particle (iii-2-2) was 1.87, and the resistivity of the particle (iii-2-2) in the coating was 1.9×10 11 Ω / □. The mass ratio of amine (b) / amine (a) is 19.8.

[0340] (Example 3)

[0341] 100 g of the water-dispersed sol of the tin oxide colloidal particles (iii-1-1) coated with the silica-tin oxide composite oxide obtained in Production Example 3 was replaced with methanol using a rotary evaporator to obtain a methanol-dispersed sol of the tin oxide colloidal particles (iii-1-1) coated with the silica-tin oxide composite oxide. The obtained sol had a pH of 5.2 (diluted with water of the same mass as methanol), a total metal oxide (SnO2 and Sb2O5) concentration of 30.5% by mass, an average particle size (dynamic light scattering particle size) by dynamic light scattering (DLS) of 16 nm, a sol stability test result of "0", 1500 ppm of tri-n-pentylamine and 40 ppm of diisopropylamine remaining in the methanol-dispersed sol of the particles (iii-1-1), a crystallinity of the core particles (i) of 92%, a refractive index of the particles (iii-1-1) of 1.93, and a resistivity of the coating film of the particles (iii-1-1) of 6.1×10 10 Ω / □. The mass ratio of amine (b) / amine (a) is 37.5.

[0342] (Example 4)

[0343] 100 g of the water-dispersed sol of tin oxide colloidal particles (iii-2-3) coated with silica-tin oxide composite oxide obtained in Production Example 4 was replaced with methanol using a rotary evaporator to obtain a methanol-dispersed sol of tin oxide colloidal particles (iii-2-3) coated with silica-tin oxide composite oxide. The pH of the obtained sol was 5.1 (diluted with water of the same mass as methanol), the total metal oxide (SnO2 and SiO2) concentration was 30.5% by mass, the average particle size based on the dynamic light scattering method (DLS) (dynamic light scattering method particle size) was 19 nm, the stability test result of the sol was "0", the residual tri-n-pentylamine in the methanol dispersed sol of particles (iii-2-3) was 3900 ppm, diisopropylamine was 180 ppm, and isopropylamine was 41 ppm. The crystallinity of the core particle (i) was 85%, the refractive index of the particle (iii-2-3) was 1.85, and the resistivity of the particle (iii-2-3) in the coating was 4.3×10 11 Ω / □. The mass ratio of amine (b) / amine (a) is 17.6.

[0344] (Example 5)

[0345] 100 g of the water-dispersed sol of tin oxide colloidal particles (iii-2-4) coated with silica-tin oxide composite oxide obtained in Production Example 5 was replaced with methanol using a rotary evaporator to obtain a methanol-dispersed sol of tin oxide colloidal particles (iii-2-4) coated with silica-tin oxide composite oxide. The pH of the obtained sol was 5.2 (diluted with water of the same mass as methanol), the total metal oxide (SnO2 and SiO2) concentration was 30.5% by mass, the average particle size based on the dynamic light scattering method (DLS) (dynamic light scattering method particle size) was 19 nm, the stability test result of the sol was "0", the residual tri-n-pentylamine in the methanol dispersed sol of particles (iii-2-4) was 4000 ppm, diisopropylamine was 160 ppm, and isopropylamine was 93 ppm. The crystallinity of the core particle (i) was 77%, the refractive index of the particle (iii-2-4) was 1.83, and the resistivity of the particle (iii-2-4) in the coating was 8.3×10 11 Ω / □. The mass ratio of amine (b) / amine (a) is 15.8.

[0346] (Example 6)

[0347] 100 g of the water-dispersed sol of tin oxide colloidal particles (iii-2-5) coated with silica-tin oxide composite oxide obtained in Production Example 6 was replaced with methanol using a rotary evaporator to obtain a methanol-dispersed sol of tin oxide colloidal particles (iii-2-5) coated with silica-tin oxide composite oxide. The pH of the obtained sol was 4.7 (diluted with water of the same mass as methanol), the total metal oxide (SnO2 and SiO2) concentration was 30.5% by mass, the average particle size based on the dynamic light scattering method (DLS) (dynamic light scattering method particle size) was 21 nm, the stability test result of the sol was "0", the residual tri-n-pentylamine in the methanol dispersed sol of particles (iii-2-5) was 3500 ppm, diisopropylamine was 140 ppm, and isopropylamine was 160 ppm. The crystallinity of the core particle (i) was 68%, the refractive index of the particle (iii-2-5) was 1.81, and the resistivity of the particle (iii-2-5) in the coating was 1.2×10 12 Ω / □. The mass ratio of amine (b) / amine (a) is 11.7.

[0348] (Example 7)

[0349] 100 g of the water-dispersed sol of tin oxide colloidal particles (iii-2-2) coated with silica-tin oxide composite oxide obtained in Production Example 2 was replaced with ethanol using a rotary evaporator to obtain an ethanol-dispersed sol of tin oxide colloidal particles (iii-2-2) coated with silica-tin oxide composite oxide. The pH of the obtained sol was 5.0 (diluted with water of the same mass as ethanol), the total metal oxide (SnO2 and SiO2) concentration was 20.5% by mass, the average particle size based on the dynamic light scattering method (DLS) (dynamic light scattering method particle size) was 22 nm, the stability test result of the sol was "0", the residual tri-n-pentylamine in the ethanol dispersion sol of the particle (iii-2-2) was 4400 ppm, the diisopropylamine was 180 ppm, and the isopropylamine was 19 ppm. The crystallinity of the core particle (i) was 91%, the refractive index of the particle (iii-2-2) was 1.87, and the resistivity of the particle (iii-2-2) in the coating was 2.6×10 11 Ω / □. The mass ratio of amine (b) / amine (a) is 22.1.

[0350] (Example 8)

[0351] 100 g of the water-dispersed sol of tin oxide colloidal particles (iii-2-2) coated with a silica-tin oxide composite oxide obtained in Production Example 2 was replaced with 2-propanol using a rotary evaporator to obtain a 2-propanol-dispersed sol of tin oxide colloidal particles (iii-2-2) coated with a silica-tin oxide composite oxide. The pH of the obtained sol was 5.2 (diluted with water of the same mass as 2-propanol), the total metal oxide (SnO2 and SiO2) concentration was 15.0% by mass, the average particle size based on the dynamic light scattering method (DLS) (dynamic light scattering method particle size) was 22 nm, the stability test result of the sol was "0", the residual tri-n-pentylamine in the 2-propanol dispersed sol of the particle (iii-2-2) was 4800 ppm, the diisopropylamine was 170 ppm, and the isopropylamine was 19 ppm. The crystallinity of the core particle (i) was 92%, the refractive index of the particle (iii-2-2) was 1.87, and the resistivity of the particle (iii-2-2) in the coating was 2.3×10 11 Ω / □. The mass ratio of amine (b) / amine (a) is 25.4.

[0352] (Example 9)

[0353] 14.6 g of the water-dispersed sol of the tin oxide colloidal particles (iii-1-1) coated with antimony pentoxide colloidal particles obtained in Production Example 3 was replaced with ethanol using a rotary evaporator to obtain 20.0 g of an ethanol-dispersed sol of the tin oxide colloidal particles (iii-1-1) coated with antimony pentoxide colloidal particles having a total metal oxide (SnO2 and SiO2) concentration of 15.0% by mass. 1.00 g of polyoxyethylene alkyl ether phosphate (RS-710 manufactured by Toho Chemical Industry Co., Ltd.) diluted with ethanol to a mass ratio of 30% was added to the obtained sol under stirring as a surface modifier, and the particles were surface-modified by heating under reflux at 90°C for 5 hours. 12.0 g of propylene glycol monomethyl ether was added to the obtained surface-modified ethanol-dispersed sol, and ethanol was evaporated using a rotary evaporator to obtain 15.0 g of a propylene glycol monomethyl ether-dispersed sol of the tin oxide colloidal particles (iii-1-1) coated with antimony pentoxide colloidal particles. The pH of the obtained sol was 4.7 (diluted with water of the same mass as methanol), the total metal oxide (SnO2 and SiO2) concentration was 20.0% by mass, the average particle size based on the dynamic light scattering method (DLS) (dynamic light scattering method particle size) was 25 nm, the stability test result of the sol was "0", the residual tri-n-pentylamine in the propylene glycol monomethyl ether dispersed sol of the particle (iii-1-1) was 4900 ppm, the diisopropylamine was 240 ppm, and the isopropylamine was 25 ppm. The crystallinity of the core particle (i) was 92%, the refractive index of the particle (iii-1-1) was 1.91, and the resistivity of the particle (iii-1-1) was 8.0×10 11 Ω / □. The mass ratio of amine (b) / amine (a) is 18.5.

[0354] (Comparative Example 1)

[0355] 100 g of the water-dispersed sol of tin oxide colloidal particles (iii-3) coated with a silica-tin oxide composite oxide obtained in Comparative Production Example 1 was replaced with methanol using a rotary evaporator. As a result, the sol thickened and gelled during the replacement.

[0356] (Comparative Example 2)

[0357] A sol was prepared in the same manner as in Reference Example 1, except that isopropylamine was not added when preparing the tin oxide composite oxide colloidal particles (i) serving as the core in Reference Example 1. The tin oxide slurry was not debonded, and a water-dispersed sol could not be obtained.

[0358] Industrial Applicability

[0359] The modified metal oxide particles of the present invention have high conductivity and high refractive index, and they are stably dispersed in an organic solvent, thereby providing the above-mentioned sol which can have transparency, high particle refractive index and good coating resistivity value when applied to a substrate as a coating agent.

Claims

1. A modified metal oxide sol comprising modified metal oxide particles (iii), the modified metal oxide particles being dispersed in an organic solvent, wherein the modified metal oxide particles (iii) have tin oxide particles (i) having an average primary particle size of 4 to 50 nm as cores and are coated with metal oxide particles (ii) having an average primary particle size of 1 to 10 nm and being selected from antimony oxide, tin oxide and silicon oxide, wherein: The average primary particle size has a relationship of core particles (i) ≧ coated particles (ii), (total mass of metal oxides other than tin oxide) / (mass of tin oxide) is 0.005 to 1.0, and the sol contains an amine (a) having a water solubility of 0.1 g / liter or more and an amine (b) having a water solubility of less than 0.1 g / liter.

2. The modified metal oxide sol according to claim 1, wherein The average particle size determined by dynamic light scattering is 5 to 100 nm.

3. The modified metal oxide sol according to claim 1, wherein The tin oxide particles (i) as core particles are hydrothermally treated tin oxide particles.

4. The modified metal oxide sol according to claim 1, wherein The tin oxide particles (i) as core particles have a crystallinity of 60% or more as determined by X-ray diffraction.

5. The modified metal oxide sol according to claim 1, wherein The metal oxide particles (ii) as the coated particles are antimony oxide particles or composite particles in which tin oxide and silicon oxide are in a mass ratio of 1:0.1 to 10.

0.

6. The modified metal oxide sol according to claim 1, wherein The modified metal oxide sol contains the amine (a) in a ratio of 20 to 3000 ppm.

7. The modified metal oxide sol according to claim 1, wherein The modified metal oxide sol contains the amine (b) in a ratio of 1,000 to 30,000 ppm.

8. The modified metal oxide sol according to claim 1, wherein The amine (a) is an amine including a primary amine, a secondary amine, or a combination thereof.

9. The modified metal oxide sol according to claim 1, wherein The amine (b) is a tertiary amine.

10. The modified metal oxide sol according to claim 1, wherein The amine (a) is at least one amine selected from the group consisting of n-propylamine, di-n-propylamine, isopropylamine, diisopropylamine, n-butylamine, isobutylamine, di-n-butylamine and diisobutylamine.

11. The modified metal oxide sol according to claim 1, wherein The amine (b) is at least one amine selected from the group consisting of tri-n-butylamine, tri-isobutylamine, tri-n-pentylamine and tri-isopentylamine.

12. The modified metal oxide sol according to claim 1, wherein The mass ratio of amine (b) / amine (a) is 3.0-200.

13. The modified metal oxide sol according to claim 1, wherein The modified metal oxide particles (iii) are coated with at least one coating agent selected from the group consisting of formula (1) to formula (6): 【Chemistry 2】 R 1 a Si(R 2 ) 4-a (1) R 5 d Si(R 6 )4-d(3) 【Chemistry 3】 In formula (1), R 1 Each is an alkyl group, a halogenated alkyl group, an alkenyl group, an aryl group, or an organic group having a polyether group, an epoxy group, a (meth)acryloyl group, a mercapto group, an amino group, a urea group, or a cyano group, and is bonded to the silicon atom through a Si-C bond, R 2 Each represents an alkoxy group, an acyloxy group, or a halogen group, and a represents an integer of 1 to 3. In formula (2) and formula (3), R 3 and R 5 Each is an alkyl group having 1 to 3 carbon atoms or an aryl group having 6 to 30 carbon atoms, and is bonded to the silicon atom through a Si-C bond, R 4 and R 6 Each represents an alkoxy group, an acyloxy group, or a halogen group, Y represents an alkylene group, an NH group, or an oxygen atom, b is an integer of 1 to 3, c is an integer of 0 or 1, and d is an integer of 1 to 3, In formulas (4) to (6), X1, X2 and X3 each represent an alkylene group having 2 to 20 carbon atoms, f, h and j each represent an integer from 1 to 100, e, g and i each represent an integer from 1 to 3, and Y1, Y2 and Y3 each represent a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms or a (meth)acryloyl group.

14. The modified metal oxide sol according to claim 1, wherein The organic solvent is a solvent containing alcohol, ketone, ester, ether, amide, hydrocarbon, a cyano group-containing solvent, a halogen-containing solvent, a sulfonyl group-containing solvent, a carboxyl group-containing solvent, or a mixed solvent thereof.

15. The modified metal oxide sol according to claim 14, wherein The alcohol is a monohydric alcohol having 1 to 20 carbon atoms or a polyhydric alcohol having 1 to 20 carbon atoms. 16 . An antistatic composition comprising the modified metal oxide particles (iii) in the modified metal oxide sol according to claim 1 . 17 . A composition for an electron transport material, comprising the modified metal oxide particles (iii) in the modified metal oxide sol according to claim 1 .

18. The method for producing an organic solvent sol of modified metal oxide particles according to any one of claims 1 to 15, comprising the following steps (A) to (D): (A) step: a step of preparing an aqueous sol containing an amine (a) having a water solubility of 0.1 g / liter or more and tin oxide particles (i) having an average primary particle size of 4 to 50 nm, (B) step: preparing an aqueous sol containing an amine (a) having a water solubility of 0.1 g / liter or more and metal oxide particles (ii) having an average primary particle size of 1 to 10 nm and being at least one selected from antimony oxide, tin oxide and silicon oxide, (C) a step of mixing the aqueous sol of tin oxide obtained in step (A) and the aqueous sol of modified metal oxide obtained in step (B) at a ratio of (total mass of metal oxides other than tin oxide) / (mass of tin oxide) of 0.005 to 1.0 to produce modified metal oxide particles (iii) having tin oxide particles (i) having an average primary particle size of 4 to 50 nm as cores and coated with at least one metal oxide particle (ii) having an average primary particle size of 1 to 10 nm selected from antimony oxide, tin oxide and silicon oxide, and adding an amine (b) having a water solubility of less than 0.1 g / liter, Step (D): a step of replacing the aqueous medium solvent of the aqueous sol of the modified metal oxide particles (iii) obtained in step (C) with an alcohol having 1 to 5 carbon atoms.

19. The method for producing an organic solvent sol of modified metal oxide particles (iii) according to claim 18, wherein: Step (A) is a step (A-1) of adding an amine (a) having a water solubility of 0.1 g / L or more to an aqueous sol of tin oxide particles (i) having an average primary particle size of 4 to 50 nm, followed by a hydrothermal treatment at a pressure of 0.1 to 40 MPa and a temperature of 100 to 350° C. for 0.01 to 100 hours.

20. The method for producing an organic solvent sol of modified metal oxide particles according to claim 18, wherein: After step (D), step (E) and / or step (F) are added: Step (E): adding at least one coating agent selected from the group consisting of formulae (1) to (6) to the organic solvent sol of the modified metal oxide particles (iii) to perform surface treatment on the modified metal oxide particles (iii); Step (F): a step of replacing the alcohol solvent of the alcohol solvent sol having 1 to 5 carbon atoms of the modified metal oxide particles (iii) with an alcohol, ketone, ester, ether, amide, hydrocarbon, cyano group-containing solvent, halogen-containing solvent, sulfonyl group-containing solvent, carboxyl group-containing solvent, or a mixed solvent thereof other than those used in step (D).

Citation Information

Patent Citations

  • Silane surface-treated metal oxide fine particles and production method for same

    CN102781821A

  • Silica-coated metal-doped tin oxide material and preparation method thereof, and dispersion body and preparation method thereof

    CN105457572A

  • Inorganic oxide microparticles having amphiphilic organic silane compound bonded thereto, organic solvent dispersion thereof, and composition for film formation

    CN109071258A

  • Preparation method of Sn-based negative pole piece of lithium ion battery

    CN112086631A

  • Coating composition and optical material

    JP2005015756A