Copper foil, and copper-clad laminate and flexible printed wiring board using same

By improving the area ratio of the cube orientation of the copper foil and optimizing the crystal structure, the problem of insufficient flexural resistance of the flexible printed circuit board during sliding bending is solved, and higher bending resistance is achieved, and it is suitable for new mobile devices.

CN119053723APending Publication Date: 2024-11-29JX NIPPON MINING & METALS CORP
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202380034882.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-07-14
Filing Date
2023-06-01
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing flexible printed circuit boards require insufficient sliding bending resistance in foldable, wearable and curly devices and cannot meet the requirements of future technical trends.

Method used

By increasing the area ratio of the cube orientation of the copper foil {001}<100> to more than 92%, and combining high-temperature annealing technology, the crystal structure and impurity distribution of the copper foil are optimized to significantly improve its sliding bending resistance.

Benefits of technology

The sliding bending resistance of copper foil has been significantly improved, and the integrity and performance of the circuit can be maintained under more stringent bending conditions, which is suitable for the needs of new mobile devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005090896790000091
    Figure BDA0005090896790000091
  • Figure BDA0005090896790000101
    Figure BDA0005090896790000101
Patent Text Reader

Abstract

The invention provides a copper foil with high sliding bending resistance, and a copper-clad laminate and a flexible printed wiring board using the same. The invention relates to a cubic orientation {001} lt; 100 gt; a copper foil having an area ratio of 92% or more; and a copper-clad laminate and a flexible printed wiring board using the copper foil.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a copper foil and a flexible printed circuit board (FPC) using the same. In particular, the present invention relates to a copper foil that can be suitably used for a curved portion of a circuit, and a copper-clad laminate and a flexible printed circuit board using the same. Background Art

[0002] Flexible printed circuit boards are flexible and can be stored in electronic equipment by bending, twisting, winding and overlapping, thereby saving space in the equipment. Therefore, they are used in various fields. For example, the FPC used in the curved part of the circuit of mobile phones is manufactured by the following methods: a method called casting, in which polyimide varnish is applied to copper foil, heated to dry and harden to form a laminate; or a method called lamination, in which a polyimide film pre-coated with thermoplastic polyimide having adhesive force is overlapped with copper foil and laminated by a heating roller or the like. The flexible copper-clad laminate obtained by these methods is called a double-layer flexible copper-clad laminate.

[0003] In addition to mobile phones, flexible printed circuit boards are also widely used in computer-related products, audio-visual products, cameras, and automobile circuits.

[0004] The properties required of flexible printed wiring boards include good bendability represented by MIT folding resistance and high cycle bending resistance represented by IPC bending resistance. Copper foils and copper-resin substrate laminates (copper-clad laminates) having such properties have been developed in the past.

[0005] For example, Patent Document 1 (Japanese Patent Application Laid-Open No. 2010-100887) discloses a copper foil obtained by previously forming preferentially oriented recrystallization nuclei in the copper foil and growing grains having a preferential orientation in (200). The copper foil is described as having excellent bendability and ensuring strength.

[0006] Patent document 2 (Japanese Patent Publication No. 2009-111203) discloses that bendability can be improved by increasing the number of grain boundaries that intersect a straight line connecting one surface to another surface at the shortest distance, and discloses that a rolled copper foil for a flexible printed circuit board can be provided that can suppress crack propagation even under severe bending conditions and achieve high bendability.

[0007] Patent document 3 (Japanese Patent Publication No. 2007-207812) discloses that by forming a Ni-Cr alloy layer on the surface of a copper foil and forming an oxide layer of a specified thickness on the surface of the alloy layer, the adhesion to a resin substrate can be greatly improved even when the copper layer surface is smooth and the anchoring effect is low. It is also disclosed that a copper foil for a printed circuit board can be provided, wherein the copper layer surface is smooth and has excellent etching properties and adhesion to a resin substrate.

[0008] Prior art literature

[0009] Patent Literature

[0010] Patent Document 1: Japanese Patent Application Publication No. 2010-100887

[0011] Patent Document 2: Japanese Patent Application Publication No. 2009-111203

[0012] Patent Document 3: Japanese Patent Application Publication No. 2007-207812 Summary of the invention

[0013] [Problems to be solved by the invention]

[0014] The technological trend in recent years is the emergence of many new forms of mobile devices, such as foldable, wearable, and rollable. Unlike previous electronic devices that have various parts arranged in a non-flexible shell, these devices require different characteristics of the flexible printed circuit boards used because the shell can be deformed. For example, the sliding bending resistance that can withstand repeated bending deformation at the radius of the hinge of a foldable phone is required to be higher than that of existing flexible printed circuit boards.

[0015] In order to meet such market requirements, the patent document Efforts have been made to control the crystal structure of copper foil used in existing flexible printed wiring boards, represented by the technology disclosed in , but it is predicted that it will not be able to cope with future technological trends.

[0016] The present invention has been made in view of the above problems, and in one embodiment, the present invention aims to provide a copper foil having high sliding bending resistance. In another embodiment, the present invention aims to provide a copper-clad laminate and a flexible printed wiring board using such a copper foil.

[0017] [Methods to solve the problem]

[0018] The inventors have made intensive research and found that by orienting the copper foil cube {001} <100> The area ratio of the copper foil is increased to an unprecedentedly high range, and the sliding bending resistance of the copper foil is significantly improved. The present invention is completed based on the above findings, and the following aspects are exemplified. [1]

[0020] A copper foil having a cubic orientation {001} <100> The area rate is over 92%. [2]

[0022] The copper foil according to [1] has a cubic orientation of {001} <100> The area rate is more than 99%. [3]

[0024] The copper foil according to [1] or [2], wherein the cubic orientation {001} <100> The average grain size is 27 μm or more. [4]

[0026] A copper-clad laminate comprising the copper foil according to any one of [1] to [3] and a resin. [5]

[0028] A flexible printed wiring board using the copper-clad laminate according to [4].

[0029] Effects of the Invention

[0030] According to the present invention, there are provided a copper foil having high sliding bending resistance, and a copper-clad laminate and a flexible printed wiring board using the same. DETAILED DESCRIPTION

[0031] The present invention is not limited to the following embodiments, and it should be understood that appropriate design changes, improvements, etc. can be made based on the common knowledge of those skilled in the art within the scope of the present invention.

[0032] (Composition of copper foil)

[0033] The material of the copper foil of the present invention is not particularly limited, and for example, tough pitch copper conforming to JIS-H3100-C1100 or oxygen-free copper conforming to JIS-H3100-C1020 is preferred. Since their compositions are close to those of pure copper, the conductivity of the copper foil does not decrease, and it is suitable for forming a circuit. The oxygen concentration contained in the copper foil is usually 0.05% by weight or less in the case of tough pitch copper, and is usually 0.001% by weight or less in the case of oxygen-free copper.

[0034] The copper foil of the present invention is formed of copper used in industry and contains inevitable impurities. Examples of inevitable impurities include P, Fe, Zr, Mg, S, Ge and Ti. If there are too many of these inevitable impurities, the crystal orientation is easily rotated due to the bending deformation of the copper foil, and shear bands are easily formed. When the bending deformation is repeated, cracks and fractures are easily generated, so it is not preferred. Therefore, the copper foil of the present invention preferably controls the total of inevitable impurities, i.e., one or more selected from the group consisting of P, Fe, Zr, Mg, S, Ge and Ti, to less than 0.002% by weight.

[0035] In addition, when the term "copper foil" is used alone in this specification, it also includes copper alloy foil, and when "tough pitch copper and oxygen-free copper" is used alone, it includes copper alloy foil using tough pitch copper and oxygen-free copper as a base.

[0036] (Cube Orientation Area Ratio of Copper Foil)

[0037] In one embodiment of the present invention, the cube orientation {001} <100> The area ratio is more than 92%. <100> When the area ratio is increased to such a high range, the sliding bending and folding resistance of the copper foil will be significantly improved.

[0038] Although not intending to be bound by theory, by increasing the cubic orientation {001} <100> The reason why the sliding bending resistance of copper foil is improved by increasing the area ratio can be inferred as follows. That is, copper is a metal with a face-centered cubic lattice. In the cubic orientation ({100} <001> ) grains, when stress is applied in the stress axis of the FPC circuit, i.e., the rolling direction (RD) or the rolling perpendicular direction (TD), the strain is not easily accumulated because eight slip systems are active at the same time. Therefore, the cubic orientation of the copper foil is {001} <100> The higher the area ratio, the less strain is accumulated in the entire tissue, and a high resistance to bending can be obtained.

[0039] Based on the above viewpoints, in the copper foil according to another embodiment of the present invention, the cubic orientation {001} <100> The area ratio is preferably 93% or more, more preferably 94% or more, further preferably 95% or more, further preferably 96% or more, further preferably 97% or more, further preferably 98% or more, further preferably 99% or more. Cubic orientation {001} <100> The upper limit of the area ratio is not particularly set, but is typically 99.99% or less, for example, 99.9% or less.

[0040] In the present invention, the area ratio of the cube orientation {001}<100> is obtained by measuring the crystal orientation distribution by the EBSD method (Electron Back Scatter Diffraction) after one cleaning by the Grain Dilation method and using the crystal orientation distribution function. Specifically, under the following electrolyte and test conditions, electrolytic polishing is carried out, and after removing about 1 μm thickness from the sample surface, a square sample of 1 mm in length × 1 mm in width arbitrarily set is scanned step by step at 3 μm with one side of the observation field parallel to the rolling direction, the crystal orientation distribution is measured, and the crystal orientation distribution function is analyzed to obtain the area ratio of the region within 15° from the cube orientation {001}<100>. The above analysis can be carried out using OIM Analysis manufactured by AME TEK.

[0041] In addition, the details of the cleaning by the Grain Dilation method are as follows.

[0042] Software used: TSL OIM Analysis 8

[0043] Parameter setting (cleaning parameter):

[0044] Grain Tolerance Angle = 0.5°

[0045] Minimum grain size = 10

[0046] Grain must contain multiple rows = Yes

[0047] The specific conditions of the EBSD method are as follows.

[0048] <Composition of electrolyte (example)>

[0049] · 250 ml of distilled water

[0050] · 125 ml of phosphoric acid

[0051] · 2.5 g of urea

[0052] · 125 ml of primary ethanol

[0053] · 25 ml of 1-propanol

[0054] <Electrolytic polishing conditions>

[0055] Applied voltage: 10 V

[0056] Electrolysis time: 10 s

[0057] <Measurement conditions of EBSD, etc.>

[0058] ·SEM conditions

[0059] Equipment: Scanning electron microscope manufactured by JEOL Ltd. (JSM-IT500HR or equivalent)

[0060] Type of electron gun: Field emission electron gun (Schottky type)

[0061] Electron gun emitter: ZrO tungsten cathode

[0062] Type of objective lens: out-lens type

[0063] Focus correction: Yes (dynamic focus: 50)

[0064] ·Beam conditions

[0065] Accelerating voltage: 15 kV

[0066] Working distance: 15mm

[0067] Irradiation current: 15nA

[0068] SEM probe diameter: 0.5~2nm

[0069] Observation magnification: 90 times

[0070] ·EBSD device conditions

[0071] Detector: Slow-scan CCD camera manufactured by TSL Solutions, Inc.

[0072] Data processing conditions

[0073] Data collection software: OIM Data Collection software manufactured by TSL Solutions, Inc.

[0074] Phase: Copper

[0075] CCD camera pixel count: 1394 × 1040 pixels

[0076] Binning: 8×8

[0077] Exposure (exposure time): 8 milliseconds

[0078] Gains:

[0079] Background processing: Yes

[0080] Scanning method of measuring points: Hexagonal grid

[0081] Hough transform

[0082] (1) Hough type: Classic

[0083] (2) Hough resolution: Low

[0084] (3) Classic Hough

[0085] · Convolution Mask: 9×9

[0086] · Min Peak Magnitude: 5

[0087] · Min Peak Distance: 23

[0088] · Peak Symmetry: 0.75

[0089] · Vertical Bias: 0

[0090] (4) Common parameters

[0091] · Binned Pattern Size: 120

[0092] · Theta Step Size: 1°

[0093] · Rho Fraction: 90%

[0094] · Max Peak Count: 8

[0095] · Min Peak Count: 3

[0096] Then, analyze the crystallographic orientation distribution function, and calculate the area ratio by dividing the area of the grains with orientations within 15° of the cube orientation by the measured area. The above measurement data was collected using OIM Data Collection of TSL Solutions Co., Ltd., and the data analysis was performed using OIM Analysis V8 of TSL Solutions Co., Ltd. In addition, the information obtained by EBSD for orientation analysis includes the orientation information of the electron beam penetrating the sample to a depth of up to several tens of nm. However, since it is sufficiently small relative to the measured area, it is recorded as an area ratio.

[0097] <Data analysis conditions for OIM Analysis V8>

[0098] · New Map window

[0099] Map Style

[0100] Grayscale: Select <none>.

[0101] Color Coded: Select Crystal Orientation.

[0102] Boundaries

[0103] Second Partition: Select <none>.

[0104] ·Cristal Orientation window (screen displayed when clicking on the color-coded edit in the map style window)

[0105] Representation: Select Euler Angles (Bunge).

[0106] • Enforce Orthotropic Sample Symmetry check box: Enter a check mark.

[0107] Add Cristal Orientation Range window (screen displayed when clicking Add Cristal Orientation Range window)

[0108] Direction tab

[0109] Phase: Select copper.

[0110] Euler angle (Bunge): (φ1, φ, φ2) = (0, 0, 0)

[0111] · Input values ​​of hkl: 001

[0112] uvw input values: 100

[0113] Tolerance tab

[0114] Minimum input value: 0

[0115] Maximum input value: 15

[0116] The total score of the crystal orientation measurement results performed under the above-mentioned setting conditions was defined as the cube orientation area ratio.

[0117] (Cubic average crystal grain size of copper foil)

[0118] In one embodiment of the present invention, the cubic orientation {001} <100> The average crystal grain size is 27 μm or more. In order to improve the sliding bending resistance of the copper foil, it is more preferred to have a cubic orientation of {001} <100> The average grain size is large. Thus, strain accumulation can be further suppressed.

[0119] In the present invention, the average crystal grain size of the cube texture {001}<100> can be obtained in the same manner as described above. After performing cleaning once by the Grain Dilation method, within the aforementioned square region of 1 mm in length and 1 mm in width measured by the EBSD method, the grain boundary is defined as the region between two measurement points with an orientation difference of 0.5° or more, and the average crystal grain size is obtained by the line segment method. The line segment method refers to the following method: 76 horizontal lines are drawn within the region, the average length of the line segments passing through each crystal grain is set as the grain size of that crystal grain, and the average value of the grain sizes is obtained for the crystal grains within the region.

[0120] Specifically, the average crystal grain size of the copper foil can be obtained by the following operations using OIM Analysis V8 and by the line segment method.

[0121] <Average crystal grain size analysis conditions of OIM Analysis V8>

[0122] · New chart window

[0123] Chart style

[0124] · Select GS (intercept length).

[0125] After the above operations, the <average intercept length> displayed in the GS (intercept length) window is used as the average crystal grain size of the copper foil obtained by the line segment method.

[0126] Based on the above viewpoints, in the copper foil of another embodiment of the present invention, the average crystal grain size of the cube texture {001}<100> is preferably 30 μm or more, more preferably 33 μm or more. There is no particular upper limit for the average crystal grain size of the cube texture {001}<100>, typically it is 100 μm or less, for example, 85 μm or less.

[0127] (Thickness of the copper foil)

[0128] The thickness of the copper foil of the present invention is not particularly limited. For example, it can be set to 2 - 100 μm. If the copper foil is too thin, it is not preferred in terms of maintaining the folding resistance of sliding bending. If the copper foil is too thick, it is not preferred in terms of flexibility and miniaturization. Therefore, the thickness of the copper foil can be set to 5 μm or more, or can be set to 10 μm or more. In addition, the thickness of the copper foil can be set to 40 μm or less, or can be set to 35 μm or less.

[0129] (Manufacturing method of the copper foil)

[0130] The manufacturing method of the copper foil of the present embodiment is not particularly limited, and for example, an ingot can be obtained by casting in a non-oxidizing atmosphere. Thereafter, homogenization annealing is performed at a temperature above 900°C, followed by hot rolling, appropriate surface processing, cold rolling, intermediate annealing, final cold rolling and other processing, and high temperature annealing described later, to obtain a copper foil of a specified thickness.

[0131] The composition of the rolled copper foil is measured by wet analysis using ICP emission spectrometry. Specifically, the measurement can be performed using an ICP emission spectrometry analyzer (ICP-OES) SPS3100 manufactured by Hitachi High-Tech Sciences, Inc. In the case of ICP emission spectrometry, the sample is dissolved in a nitric acid aqueous solution (nitric acid: water = 1:1 by volume) and diluted for use.

[0132] In the prior art, the cube orientation {001} <100> Measures to improve the area ratio include readjusting the added elements of the raw materials, the grain size during intermediate annealing, rolling conditions, copper foil processing degree, etc., but the cube orientation {001} <100> The area ratio limit is about 90% in copper foil (for copper foil with a thickness of 12 μm). In one embodiment of the present invention, the copper foil after final cold rolling (i.e., copper foil processed to a specified thickness) is subjected to high temperature annealing (e.g., above 600°C) in a hydrogen atmosphere, thereby obtaining a cubic orientation {001} of 92% or more. <100> In addition, by this high temperature annealing, a cubic orientation {001} of 27 μm or more can be obtained. <100> Based on the increase of the cubic orientation {001} <100> From the viewpoint of the driving force of the area ratio, that is, the void density inside copper, annealing is preferably performed in a hydrogen atmosphere.

[0133] (Copper clad laminates and flexible printed circuit boards)

[0134] Regarding the flexible printed circuit board of the present invention, if a copper-clad laminate formed by laminating the copper foil and resin of the present invention is used, it can be a circuit board formed by laminating a resin previously made into a film with or without an adhesive, or it can be a circuit board formed by coating a non-film-like resin material as a resin on the copper foil and then forming a film. As the resin layer, polyimide, liquid crystal polymer, PTFE (polytetrafluoroethylene) can be listed, but it is not limited to these.

[0135] Example

[0136] Hereinafter, the present invention will be specifically described by way of examples, but the description here is for illustrative purposes only and is not intended to be limiting.

[0137] First, a copper ingot is cast in a non-oxidizing atmosphere. The copper ratio in the copper ingot is 99.98% or more. The ingot is homogenized and annealed at a temperature above 900°C, followed by hot rolling, surface processing, cold rolling, intermediate annealing, and final cold rolling to obtain a copper foil with a thickness of 12 μm or 33 μm.

[0138] Thereafter, the copper foils of the examples and comparative examples were annealed at the temperatures shown in Table 1 or Table 2. In the examples, annealing was performed at the temperatures shown in Table 1 or Table 2 for 60 minutes in a hydrogen atmosphere, and the temperature was raised at 400°C / 30 minutes when the temperature was below 800°C until the temperature in Table 1 or Table 2 was reached, and the temperature was raised at 120°C / 10 minutes when the temperature exceeded 800°C and was below 1020°C. In the comparative examples, annealing was performed at the temperatures shown in Table 1 for 30 minutes, and the foil was placed in a high-temperature hot air dryer heated to 250°C.

[0139] The copper foil of the comparative example was annealed at a temperature (250° C.) assuming normal primary recrystallization, not at a high temperature.

[0140] (cubic orientation {001} <100> Area ratio)

[0141] Subsequently, for each embodiment and comparative example, as described above, a scanning electron microscope JSM-IT500HR manufactured by JEOL Ltd. was used to scan a square sample of 1 mm in length by 1 mm in width at a step of 3 μm by the EBSD method to measure the crystal orientation distribution, and to analyze the crystal orientation distribution function to obtain the crystal orientation distribution function corresponding to the cubic orientation {001} <100> The area ratio of the area within 15° difference.

[0142] (cubic orientation {001} <100> The average crystal particle size

[0143] The grain boundary was defined as a region between two measurement points with an orientation difference of 0.5° or more in the aforementioned square region of 1 mm in length by 1 mm in width, and was determined by the line segment method (76 horizontal lines) as described above.

[0144] (Sliding bending test)

[0145] With regard to Examples 1, 2 and Comparative Example 1, NIKAFLEX-CISV1215 manufactured by Nico Industrial Co., Ltd. was used as a base film, and the copper foil annealed at the temperature shown in Table 1 below was hot pressed and attached. During hot pressing, the copper foil was overlapped with the base film and placed in a furnace. After the set temperature was raised to 180°C for 30 minutes, it was pressed under the same temperature for 40 minutes and 2.5MPa. After that, it was taken out after the furnace was cooled to room temperature. Thereafter, after forming a circuit with a pattern of 300μm in width, a covering layer was set with NIKAFLEX-CISV1215 to prepare a flexible printed circuit board with a 3-layer structure. With regard to Examples 3 and 4, NIKAFLEX-CISV1215 manufactured by Nico Industrial Co., Ltd. was used as a base film, and the copper foil annealed at the temperature shown in Table 2 below was hot pressed and attached to prepare a flexible printed circuit board with a circuit formed with a pattern of 300μm in width.

[0146] For the obtained flexible printed circuit boards, for Examples 1, 2 and Comparative Example 1, an IPC sliding bending test was performed under the conditions of a speed of 1500 cpm (revolutions / minute), a stroke of 20 mm, and a bending radius of 0.5 mm, and the number of times the copper foil was broken was counted. For Examples 3 and 4, an IPC sliding bending test was performed under the conditions of a speed of 1500 cpm (revolutions / minute), a stroke of 20 mm, and a bending radius of 4.0 mm, and the number of times the copper foil was broken was counted.

[0147] [Table 1]

[0148]

[0149] [Table 2]

[0150]

[0151] As can be seen from Tables 1 and 2, in the examples where high temperature annealing was performed under the prescribed conditions, the cube orientation {001} <100> The area ratio is more than 92%, and the cube orientation is {001} <100> The average grain size of the quartz crystal was 27 μm or more. In addition, in the sliding bending test, a significantly larger number of bending times than the comparative example was obtained.

[0152] On the other hand, in Comparative Example 1, annealing was performed at a temperature assuming normal primary recrystallization, but as a result, the cube orientation {001} <100> The area ratio is out of the range of the present invention, and the result of the sliding bending test is worse than that of the example.< / none> < / none>

Claims

1. A copper foil having a cubic orientation {001} <100> The area rate is over 92%.

2. The copper foil according to claim 1, wherein the cubic orientation is {001} <100> The area rate is more than 99%.

3. The copper foil according to claim 1 or 2, in, Cube Orientation {001} <100> The average grain size is 27 μm or more. 4 . A copper-clad laminate comprising the copper foil according to claim 1 and a resin.

5. A flexible printed wiring board using the copper-clad laminate according to claim 4.

Citation Information

Cited By

  • Flexible electronic device bending performance characterization analysis method

    CN120030851A