Composite laminated soft magnetic belt with controllable properties

By stacking amorphous alloy belt and nanocrystalline alloy belt on the silicon steel sheet belt, a wider composite laminated soft magnetic belt is formed, which solves the mechanical strength and magnetostriction problems in large magnetic products, and achieves low noise and high efficiency magnetism Parts manufacturing.

CN119054033APending Publication Date: 2024-11-29ECDL LIMITED LIABILITY COMPANY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380033034.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-08-02
Filing Date
2023-07-21
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The prior art is difficult to prepare magnetic components with sufficient characteristics, especially in the manufacturing of large magnetic products. The mechanical strength and rigidity of nanocrystal alloy laminated belts are insufficient, and the magnetostrictive of the amorphous alloy belts leads to noise and vibration. The method is not suitable for the manufacturing of large magnetic products.

Method used

By stacking soft magnetic tapes with different characteristics, including amorphous alloy tapes and nanocrystalline alloy tapes, and aligning these tapes on silicon steel sheet tapes, to form a wider composite laminated soft magnetic tape, using the amorphous alloy tapes The reinforcement improves the rigidity of the nanocrystal alloy tape and forms magnetic components with excellent characteristics by winding and fixing.

Benefits of technology

The preparation of low-noise, small self-support transformers is realized, and the process is reduced. It is suitable for the manufacturing of magnetic components of large transformers, motors and generators, reducing the volume and weight of magnetic components, while improving magnetic permeability and iron loss performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119054033A_ABST
    Figure CN119054033A_ABST
Patent Text Reader

Abstract

The purpose of the present invention is to provide a composite laminated soft magnetic tape by laminating magnetic components such as transformers and motor cores, based on a combination of material advantages, on the basis of taking into account the advantages and disadvantages of a single soft magnetic tape such as a silicon steel sheet tape, an amorphous alloy tape, a nanocrystal alloy tape, and the like, to obtain maximum efficiency. A magnetic member is prepared into a composite laminated soft magnetic tape by laminating a plurality of types of soft magnetic metal tapes (wherein the plurality of types of soft magnetic metal tapes include amorphous alloy tapes and nanocrystal alloy tapes) having different characteristics and equal width, and stacking and then fixing the plurality of the laminated soft magnetic tapes. A wider magnetic component is prepared from a composite laminated soft magnetic tape obtained by stacking and then fixing a plurality of laminated soft magnetic tapes. The laminated soft magnetic tape is formed by laminating one or more layers having a narrower amorphous alloy tape and a nanocrystal alloy tape aligned on a wider silicon steel sheet tape such that a total width of the narrower amorphous alloy tape and the nanocrystal alloy tape can be substantially equal to a width of the wider silicon steel sheet tape.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a composite laminated soft magnetic tape, which is a soft magnetic tape such as a silicon steel sheet tape, an amorphous alloy tape and a nanocrystalline alloy tape overlapped with each other. It relates to using the composite laminated soft magnetic tape to manufacture a magnetic core, a reactor, a toroidal magnetic core, a large laminate and a motor for a transformer, a stator magnetic core, a rotor magnetic core and a magnetic circuit for a generator, etc. Background Art

[0002] Amorphous alloy ribbons are prepared by rapid cooling from their molten state and do not have a crystal structure at the atomic level. They are a state that does not have a specific periodic structure under electron microscopy and X-ray diffraction. Therefore, amorphous alloy ribbons prepared in a rapidly cooled state are usually annealed at a temperature lower than the crystallization temperature to eliminate internal stress and have softer magnetic properties for further use.

[0003] Since the amorphous alloy ribbon is manufactured by rapid cooling from a molten state, the ribbon has a width of about 20 cm. Currently, the manufacture and utilization of wide ribbons is limited.

[0004] Although amorphous alloy ribbons can be used to manufacture soft magnetic ribbons having various properties, generally, the types of soft magnetic ribbons on the market are limited. Although it is known that the soft magnetic properties and iron loss of amorphous alloy ribbons mainly containing ordinary iron are much better than those of silicon steel sheet ribbons, its only disadvantage is that since the amorphous alloy ribbon has a higher magnetostriction constant than nanocrystalline alloy ribbons and silicon steel sheet ribbons, it has magnetic properties such as magnetic permeability and iron loss that are deteriorated by applying thermal shrinkage and residual deformation of the resin caused by bonding.

[0005] Silicon steel strip, one of the soft magnetic strips, has a high saturation magnetic flux density, which reduces the volume and weight of magnetic parts. Amorphous alloy strips and nanocrystalline alloy strips have magnetic properties such as magnetic permeability and iron loss that are superior to silicon steel strips, and their magnetic parts are excellent in energy saving. Nanocrystalline alloy strips have made progress in the application of magnetic parts because they have good magnetic properties including magnetostriction, but their only disadvantage is low rigidity.

[0006] Optimally preparing magnetic components using amorphous alloy ribbons can achieve 97% or higher energy efficiency in transformers or motors, which is suitable for energy saving. In addition, since nanocrystalline alloy ribbons have lower magnetostriction, limitations in manufacturing such as machining and molds may be greatly alleviated.

[0007] Since amorphous alloy strips and nanocrystalline alloy strips usually have a thickness of about 0.03 mm, which is much thinner than silicon steel sheets, amorphous alloy strips and nanocrystalline alloy strips have lower eddy current losses and are often wound and stacked for use.

[0008] As described above, each of these soft magnetic tapes has its advantages and disadvantages, and if used alone to construct a magnetic component, sufficient performance cannot be obtained. Currently, it is difficult to try to improve their characteristics in combination with another material, and the device is constructed from silicon steel sheet tape alone, amorphous alloy tape alone, or nanocrystalline alloy tape alone.

[0009] According to Patent Document 1, in order to ensure the mechanical strength or rigidity which is the only drawback of the nanocrystalline alloy laminated magnetic core, a support member that holds a non-magnetic body in the lamination direction of the laminated blocks is used.

[0010] According to patent document 2, a method for manufacturing a magnetic core rolled into a strip shape is applied, the method comprising: crystallizing a portion of an amorphous alloy strip that can be nano-crystallized; selecting an amorphous alloy strip having a similar shrinkage rate to the amorphous alloy strip; selecting a nanocrystalline alloy strip having stable characteristics; nano-crystallizing it and heat treating it to obtain stable characteristics.

[0011] According to Patent Document 3, an amorphous ferromagnetic core transformer is produced by opposing amorphous alloy ribbons, aligning wide and large amorphous alloy ribbons so that the opposed surfaces of the layers are offset from each other, and stacking them.

[0012] According to the method of Patent Document 4, three rolls of soft magnetic alloy ribbons are bonded by coating epoxy resin therein to laminate them into one roll, wherein the laminate of the soft magnetic alloy ribbons is bonded by using two thermosetting resins having different glass transition temperatures.

[0013] According to a typical manufacturing method in the past, the stator and magnetic core of the motor are prepared by stamping and laminating silicon steel sheets. Since amorphous alloy strips and nanocrystalline alloy strips are thin and hard, the life of the die used for the stamping is short, and the steps take time to collect, process and stack the stamped strips, so this method is not suitable for lamination to prepare the stator and magnetic core. According to Patent Document 5, an amorphous alloy strip is wound into a fan shape and applied to a stator ferromagnetic core for a motor to prepare an axial gap motor, which is applied to a fan device.

[0014] Patent Document 6 relies on bonding, and soft magnetic alloy strips are stacked and laminated while applying a resin therein, and are pressed under heating to produce a laminated body.

[0015] According to non-patent document 1, nanocrystalline alloy ribbons are applied to magnetic cores for transformers to test characteristics. Non-patent document 2 discloses a low iron loss amorphous ferromagnetic core structure, which is constructed as follows: the shape of the ferromagnetic core is maintained by cutting and stacking amorphous metal foils and then inserting them into a resin ferromagnetic core holding part.

[0016] Prior art literature

[0017] Patent Literature

[0018] Patent Document 1: Japanese Patent Laid-Open No. 2021-68865

[0019] Patent Document 2: Japanese Patent Laid-Open No. 2021-9921

[0020] Patent Document 3: Japanese Patent Laid-Open No. 2013-98349

[0021] Patent Document 4: Japanese Patent Laid-Open No. 2021-154732

[0022] Patent Document 5: Japanese Patent Laid-Open No. 2009-284578

[0023] Patent Document 6: Japanese Patent Laid-Open No. 2007-281314

[0024] Non-patent literature 1: Kazuhiro Idei, Fumio Kurihara, Yoshinori Sunaga, "Application of Next-Generation Nanocrystalline Soft Magnetic Materials to Transformer Cores", Toko Takaoka Giho, VOL.7, (2020), pp.15-18

[0025] Non-patent document 2: Yuji Enomoto, Hirooki Tokoi, Takao Imagawa, ToshifumiSuzuki, Takeshi Obata, Kenichi Souma, "Kokusai Koukouritsukikaku IE5 level wotasseishita amorufasumota (Amorphous Motor Achieving International High-efficiency Standard IE5 level)", Hitachihyoron, combined issue for June andJuly,2015,PP.50-55 Summary of the invention

[0026] Technical issues

[0027] Even with various conventional devices, it cannot be said that the prepared magnetic components have obtained sufficient characteristics. In order to solve the following remaining problems, it is necessary to provide a method for further controlling the properties and laminating soft magnetic tapes with different characteristics to prepare a magnetic component with excellent characteristics.

[0028] Although small nanocrystalline alloy laminated tapes can have rigidity improved by molds, etc., there is the following problem: the transformer core requires support components to ensure mechanical strength and rigidity, which are the only disadvantages of large nanocrystalline alloy laminated tapes. In addition, when nanocrystalline alloy laminated tapes are used for magnetic cores in motors or generators, noise, vibration, etc. caused by external force dragging and deformation caused by repulsive force may occur. Transformers using amorphous alloy tapes with large magnetostriction may emit loud noise.

[0029] Currently, for both amorphous alloy ribbons and nanocrystalline alloy ribbons, the maximum ribbon width that can be produced is about 20 cm. In order to produce large magnetic products, it is necessary to develop composite laminated soft magnetic ribbons with larger widths.

[0030] Since the nanocrystalline alloy ribbons are heat treated before lamination, they are weaker than before the heat treatment.

[0031] In order to improve the efficiency of the motor, it is desired to prepare high-efficiency and high-productivity stators and motors by applying amorphous alloy strips or nanocrystalline alloy strips characterized by higher magnetic permeability and lower iron loss than silicon steel sheets. In the past, methods for controlling properties and promoting production by a good combination of soft magnetic metals with different characteristics have not been explored.

[0032] From the viewpoint of energy saving, an ideal soft magnetic ribbon magnetic product is produced using an amorphous alloy ribbon or a nanocrystalline alloy ribbon on which no compressive stress caused by a mold is applied.

[0033] The magnetic components to be excited vary according to the purpose of use, ranging from low power to high power. Therefore, the magnetic material can include materials with low coercivity and low saturation flux density and silicon steel sheet materials with higher coercivity and high saturation flux density.

[0034] Although silicon steel sheets with high magnetic flux density are used as the main body in order to reduce the volume and weight of magnetic parts by using soft magnetic tapes, silicon steel sheets have worse properties such as magnetic permeability and iron loss than amorphous alloy tapes and nanocrystalline tapes. Therefore, although the magnetic parts obtained have increased volume and weight, from the viewpoint of energy saving, the development of transformers, motors, etc. with amorphous alloy tapes or nanocrystalline alloy tapes as the main body has made progress. In order to prepare large transformers by using nanocrystalline alloy tapes, non-magnetic supports are required to be strengthened to cover up the disadvantage of low rigidity. It is necessary to develop a composite laminated soft magnetic tape in which the nanocrystalline alloy tape is held and covered by silicon steel sheets or amorphous alloy tapes so that the nanocrystalline alloy tapes can be self-supporting without the use of a support.

[0035] The present invention is made in view of the above-mentioned problems. The purpose of the present invention is to provide a composite laminated soft magnetic tape by stacking magnetic components such as transformers and motor cores, which takes into account the advantages and disadvantages of individual soft magnetic tapes such as silicon steel sheet tapes, amorphous alloy tapes, nanocrystalline alloy tapes, etc., and combines the advantages of materials to obtain maximum efficiency.

[0036] Solutions to the problem

[0037] According to a composite laminated soft magnetic tape of the present invention, it is obtained by laminating and stacking multiple types of soft magnetic metal tapes with different properties and equal widths, and then fixing the multiple laminated soft magnetic tapes, and is characterized in that the multiple types of soft magnetic tapes always include amorphous alloy tapes and nanocrystalline alloy tapes.

[0038] A composite laminated soft magnetic tape according to the present invention is obtained by winding laminated soft magnetic tapes multiple times and fixing them, and is characterized in that the laminated soft magnetic tape is formed by laminating amorphous alloy tapes and nanocrystalline alloy tapes with equal widths.

[0039] According to a composite laminated soft magnetic tape of the present invention, which is obtained by stacking and then fixing a plurality of laminated soft magnetic tapes, the laminated soft magnetic tape is characterized in that the laminated soft magnetic tape is formed by stacking one or more layers of narrower amorphous alloy tapes and nanocrystalline alloy tapes aligned on a wider silicon steel sheet tape so that the total width of the narrower amorphous alloy tapes and the nanocrystalline alloy tapes can be substantially equal to the width of the wider silicon steel sheet tape.

[0040] A composite laminated soft magnetic tape according to the present invention is formed by: winding the laminated soft magnetic tape multiple times, the laminated soft magnetic tape is formed by aligning narrower amorphous alloy tapes and nanocrystalline alloy tapes on a wider silicon steel sheet tape so that the total width of the narrower amorphous alloy tapes and the nanocrystalline alloy tapes can be substantially equal to the width of the wider silicon steel sheet tape, and then only winding the aligned narrower amorphous alloy tapes and the nanocrystalline alloy tapes so that the total width of the narrower amorphous alloy tapes and the nanocrystalline alloy tapes can be substantially equal to the width of the wider silicon steel sheet tape and fixing them.

[0041] Advantageous Effects of the Invention

[0042] Combining amorphous alloy ribbons and nanocrystalline alloy ribbons can provide a magnetic component that maintains the soft magnetic properties with less iron loss and the weakness of the nanocrystalline alloy ribbon in rigidity is strengthened by the amorphous alloy ribbon. For example, a small self-supporting transformer that produces low noise can be prepared. Winding these ribbons to prepare the magnetic component can help reduce the process, and the magnetic component can be machined and directly used as a magnetic core for the stator of an axial gap motor.

[0043] By adopting a stacked soft magnetic strip having narrower amorphous alloy strips and nanocrystalline alloy strips aligned on a wider silicon steel sheet strip, a small excitation current operates in the amorphous alloy strip and the nanocrystalline alloy strip portions, and by utilizing the characteristic of the silicon steel sheet strip having a high saturation magnetization intensity, a magnetic component such as a motor stator with a reduced size that can operate even under a large excitation current can be provided.

[0044] By winding a laminated soft magnetic tape including a combination of an amorphous alloy tape and a nanocrystalline tape using a silicon steel sheet tape having a width of 25 cm or more, magnetic components for large transformers, motors, generators, etc. can be manufactured with reduced operation steps. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 3 is a diagram showing a composite laminated soft magnetic tape according to Example 1.

[0046] Figure 2 is a diagram showing a method for preparing a composite laminated soft magnetic tape according to Example 2.

[0047] Figure 3 3 is a diagram showing a composite laminated soft magnetic tape prepared according to Example 2.

[0048] Figure 4 This is a diagram showing a composite laminated soft magnetic tape according to Example 3.

[0049] Figure 5a is a diagram showing a method for preparing a composite laminated soft magnetic tape according to Example 4.

[0050] Figure 5b is a diagram showing a method for preparing a composite laminated soft magnetic tape according to Example 4.

[0051] Figure 6 3 is a diagram showing a composite laminated soft magnetic tape prepared according to Example 4.

[0052] Description of reference numerals:

[0053] 1 Composite laminated soft magnetic tape

[0054] 2 Soft magnetic tape

[0055] 3-layer soft magnetic tape

[0056] 4 Silicon steel strip

[0057] 5 Amorphous alloy ribbon

[0058] 6 Nanocrystalline Alloy Ribbon

[0059] 7 Guide frame DETAILED DESCRIPTION

[0060] Before describing the embodiments of the present invention, the principle of the present invention is described first.

[0061] Soft magnetic tapes such as silicon steel sheets, amorphous alloy tapes and nanocrystalline alloy tapes are well known, but they may have different advantages and disadvantages in magnetic properties, mechanical properties, etc. Most of them contain layers of one material stacked to prepare magnetic parts. The good properties of different tapes are macro-synthesized to be used as composite laminated soft magnetic tapes.

[0062] According to the present invention, the composite laminated soft magnetic tape uses silicon steel sheet tape, amorphous alloy tape, etc. to maintain the nanocrystalline alloy tape, so it can be composed of 100% soft magnetic tape without adhesive, instead of being reinforced with a non-magnetic support body, which allows the volume and weight of the magnetic component to be reduced.

[0063] Such a laminated soft magnetic ribbon using an amorphous alloy ribbon and a nanocrystalline alloy ribbon exhibits a higher magnetic permeability than a silicon steel sheet, and thus can provide a magnetic component that achieves energy saving and reduced iron loss.

[0064] The laminated soft magnetic tape mainly comprises nanocrystalline alloy tape, so magnetostriction can be reduced and the hum of the transformer can be reduced. In addition, although the laminated soft magnetic tape mainly comprising nanocrystalline tape may cause the magnetic core of the motor comprising it to deform by external force, the deformation of the magnetic core can be expected to be reduced because its rigidity is improved by the amorphous alloy tape therein. Compared with the case of using one material, the laminated soft magnetic tape combining the advantages of different types of materials can be used to increase the possibility of preparing high-function products.

[0065] Silicon steel sheet strip has a wide range of advantages, and the thickness can be arbitrarily adjusted. It can be used to prepare composite laminated soft magnetic strips with a width greater than or equal to 25 cm, which enables the development of magnetic components for larger transformers, motors, generators, etc.

[0066] By combining a magnetic material having low coercivity and a material having high saturation magnetic flux density, the material having low coercivity reaches the saturation magnetic flux density with a smaller excitation energy, and when further excitation energy is subsequently applied, the material having high saturation magnetic flux density withstands it, thereby making it possible to prepare a composite material that utilizes the advantages of each other.

[0067] Example 1

[0068] Figure 1: is a diagram showing a composite laminated soft magnetic tape 1 according to Example 1. In order to improve the characteristics, multiple types of soft magnetic tapes 2 with equal widths and different characteristics are stacked and fixed to prepare a laminated soft magnetic tape 3. It is assumed that the multiple types of soft magnetic tapes 2 always include amorphous alloy tapes and nanocrystalline alloy tapes. As a third soft magnetic tape, a silicon steel sheet tape or the like can be added. The number of stacked layers can be selected within the range of 2 to 5 as required. A plurality of the laminated soft magnetic tapes 3 are further stacked and fixed to prepare the composite laminated soft magnetic tape 1. Although Figure 1 The figure shows that two layers are actually stacked, but for example, about 100 layers may be stacked to obtain a certain thickness. The fixing may be performed by bonding.

[0069] Although described nanocrystalline alloy band helps to improve the magnetic property of the magnetic component that obtains, when it is used alone, rigidity is low, is difficult to self-supporting.Therefore, the magnetic component that obtains is likely to be out of shape.Through the amorphous alloy band of the reinforced body of the laminated soft magnetic band and the nanocrystalline alloy band used in combination, the composite laminated soft magnetic band that obtains can keep good magnetic property, can also use in a self-supporting mode.

[0070] From the viewpoint of energy saving, the composite laminated soft magnetic ribbon 1 in which the nanocrystalline alloy ribbon and the amorphous alloy ribbon are combined is used.

[0071] The low rigidity of the nanocrystalline alloy band is made up by the amorphous alloy band, so the composite laminated soft magnetic band 1 holding them can be used as a large laminate. Combining four rectangular cuboids can provide a transformer. By stamping and laminating them, it can be used as a motor core. The amorphous alloy band has a higher magnetostriction constant, so if it is used for a transformer, it vibrates with alternating current and may cause noise. But by controlling the amount of the amorphous alloy band to be lower than the amount of the nanocrystalline alloy band, the vibration with alternating current can be reduced.

[0072] It should be noted that according to Example 1, the amorphous alloy ribbon and the nanocrystalline alloy ribbon are necessary, and sometimes a soft magnetic ribbon such as a silicon steel sheet ribbon is also used. On the other hand, although the volume and weight are more or less increased, when a magnetic component driven only by a low current is constructed without using a silicon steel sheet ribbon and only using an amorphous alloy ribbon and a nanocrystalline alloy ribbon, low coercivity and greatly reduced iron loss can be achieved. Therefore, the magnetic component can be activated with a low current, which is conducive to energy saving.

[0073] Example 2

[0074] Figure 2 is a diagram showing a method for producing a composite laminated soft magnetic tape 1 according to Example 2.

[0075] In order to improve the characteristics, a plurality of amorphous alloy ribbons and nanocrystalline alloy ribbons having equal widths and different characteristics are stacked and fixed to prepare a laminated soft magnetic ribbon 3, and the laminated soft magnetic ribbon 3 is wound and then fixed to prepare the composite laminated soft magnetic ribbon 1.

[0076] The number of stacked layers can be selected in the range of two to five layers as required. The combination of the soft magnetic tape 2 includes an alternating arrangement of amorphous alloy tapes and nanocrystalline alloy tapes or an arrangement of an amorphous alloy tape and two nanocrystalline alloy tapes, for example, which can be selected to adjust the total thickness. The fixing can be an adhesive method so as to compensate for mechanical strength and rigidity.

[0077] The composite laminated soft magnetic tape 1 thus prepared can be cut as necessary to prepare a magnetic component for a transformer, a toroidal core, a reactor, or the like.

[0078] Prepare a 2cm wide amorphous alloy ribbon wound on one reel and a 2cm wide nanocrystalline alloy ribbon wound on two reels. Two nanocrystalline alloy ribbons are stacked on the amorphous alloy ribbon and then wound. By winding it 100 times to make a 6cm wide, 2cm high rectangle, prepare Figure 3 The 1 cm thick composite laminated soft magnetic tape 1 shown. The use of the nanocrystalline alloy tape allows for use as a transformer core that exhibits good properties and can be self-supporting without the use of non-magnetic reinforcements. A similar method can be used to prepare reactors, motor cores and bulk laminates. As with Example 1, this combination of soft magnetic tapes according to Example 2 can provide less hysteresis loss and eddy current loss, reduced iron loss and good soft magnetic properties, which is most suitable for energy-saving magnetic components.

[0079] Although currently amorphous alloy strips are cut, stacked and provided in a housing within the stator of an axial gap motor (see non-patent document 2), the cylindrical magnetic core prepared from the composite laminated soft magnetic strip 1 of Example 2 can be machined and a coil can be wound around it so that it can be used for the stator of an axial gap motor.

[0080] When the magnetic core portion of the axial gap motor is prepared with an amorphous alloy tape, the amorphous alloy tape is fixed by resin bonding to fix the magnetic core around which the amorphous alloy tape is wound. Due to the bonding and fixing, stress is applied to the magnetic core, and large magnetostriction deteriorates the soft magnetic properties. However, in the magnetic core portion prepared by the composite laminated soft magnetic tape 1 of Example 2, the use of the nanocrystalline alloy tape can reduce the deterioration of the soft magnetic properties. Therefore, the operating efficiency of the manufacturing step can be improved.

[0081] Example 3

[0082] Figure 4FIG. 1 is a diagram showing a composite laminated soft magnetic tape 1 according to Example 3. FIG.

[0083] The laminated soft magnetic tape 3 is formed by laminating one or more layers having narrower amorphous alloy tapes and nanocrystalline alloy tapes (as soft magnetic tapes 2) aligned on a wider silicon steel sheet tape 4 so that the total width of the narrower amorphous alloy tapes and the nanocrystalline alloy tapes can be substantially equal to the width of the wider silicon steel sheet tape 4. A plurality of the laminated soft magnetic tapes 3 are further laminated and fixed to prepare the composite laminated soft magnetic tape 1. Although Figure 4 The laminated soft magnetic tape 3 in the embodiment includes a silicon steel sheet tape 4 and a soft magnetic tape 2, but a silicon steel sheet tape and a plurality of soft magnetic tapes may be laminated to form the laminated soft magnetic tape 3. Figure 4 The figure shows that two laminated soft magnetic tapes 3 are laminated to form the composite laminated soft magnetic tape 1, but it is also possible to actually laminate, for example, about 100 layers to obtain a certain thickness.

[0084] The composite laminated soft magnetic ribbon 1 can be machined as needed to prepare magnetic parts such as magnetic cores of motors, bulk laminates, magnetic core parts of generators, etc. Although a plurality of teeth as a part of a stator are connected into a ring to prepare a large motor magnetic core with a conventional amorphous alloy ribbon, this embodiment can facilitate the preparation of a wider motor magnetic core than before through a single stamping operation.

[0085] The part of the composite laminated soft magnetic strip 1 containing amorphous alloy strips and nanocrystalline alloy strips works with a small excitation current and the silicon steel strip has a high saturation magnetization. These maximum properties are most suitable for magnetic components such as stators of small motors, which can utilize the size reduction achieved to the greatest extent by the properties. In addition, it is also suitable for the following magnetic components: it works with nanocrystalline alloy strips and amorphous alloy strips at lower outputs, and although the energy efficiency is reduced during the maximum power consumption, it also works with silicon steel strips with high saturation magnetization. When it is applied to a transformer, the transformer works by using nanocrystalline alloy strips and amorphous alloy strips with standby power consumption. In the case of using a motor, the motor also works with nanocrystalline alloy strips and amorphous alloy strips in a low output mode, and also works with a part of silicon steel strips in a maximum output mode. Although the soft magnetic properties of silicon steel strips are worse than those of nanocrystalline alloy strips and amorphous alloy strips, and also have the disadvantage of increased energy consumption, since the silicon steel strips show a smaller magnetostriction than the amorphous alloy strips, it will not produce large vibrations in the transformer.

[0086] Example 4

[0087] Figure 5a and 5b is a diagram showing a method for preparing a composite laminated soft magnetic tape 1 according to Example 4. Figure 5a As shown in FIG. 1 , a silicon steel sheet strip 4 having a thickness of 0.1 mm, a width of 50 cm, and a length of 6 m wound on one reel, an amorphous alloy strip 5 having a thickness of 0.03 mm, a width of 20 cm, and a length of about 1000 m wound on two reels, and a nanocrystalline alloy strip 6 having a thickness of 0.02 mm, a width of 10 cm, and a length of about 1000 m wound on one reel were prepared. The strips were pulled out from the respective reels, as shown in FIG. Figure 5b As shown, the 20cm wide amorphous alloy belt, the 10cm wide nanocrystalline alloy belt and the 20cm wide amorphous alloy belt are aligned and stacked on the 50cm wide silicon steel sheet belt 4 so that the total width can be equal to 50cm, equal to the total thickness of the silicon steel sheet to form a laminated soft magnetic belt 3, and wound by a guide frame 7. In order to obtain a square with a side length of 50cm, the belt is wound three times by bending 90 degrees at four positions per turn. By keeping a total width of 50cm even after the silicon steel sheet ends, the 20cm wide amorphous alloy belt, the 10cm wide nanocrystalline alloy belt and the 20cm wide amorphous alloy belt are continuously wound 30 times, and when the thickness is equal to 1.29mm, the amorphous alloy belt is cut. In the case where the amorphous alloy belt has equal thickness to the nanocrystalline alloy belt, the nanocrystalline alloy belt is also cut, and it is completed. But in the above-mentioned embodiment, the thickness of the nanocrystalline alloy belt is small, and the nanocrystalline alloy belt is wound 15 times again separately. If it is confirmed that the difference between the total thickness of the amorphous alloy ribbon wound 30 times and the total thickness of the nanocrystalline alloy ribbon wound 45 times is equal to or less than 0.1 mm, the nanocrystalline alloy ribbon is also cut to prepare Figure 6 The composite laminated magnetic tape 1 is shown.

[0088] After the cubic composite laminated magnetic tape 1 prepared in this way is fixed, its four corners are cut to obtain four plates with dimensions of 50 cm×50 cm×1.29 mm, respectively. The plates are punched to obtain motor core materials.

[0089] The composite magnetic ribbon 1 of this embodiment can be used as a magnetic core of a generator.

[0090] The magnetic components such as the motor core and the generator core prepared by this embodiment are advantageously no longer limited by the width of the tape, and wide composite soft magnetic tapes can be used. Since the preparation of large transformers or motor cores requires a wider and thicker composite tape with more turns, the method according to this embodiment is suitable.

[0091] Here, the properties of the magnetic members prepared according to Examples 1 to 4 can be compared and summarized as follows.

[0092] Although the saturation magnetic flux density of the magnetic components prepared by Examples 1 and 2 decreases during use in low output mode, since they involve energy-saving operation of nanocrystalline alloy strips and amorphous alloy strips with excellent soft magnetic properties, the methods of Examples 1 and 2 are suitable for magnetic components that require energy saving in low output mode.

[0093] Since the magnetic components prepared by Examples 3 and 4 have always used silicon steel strips with large iron loss, they generate a large amount of heat, which is not very advantageous from the perspective of energy saving. However, in low output mode, amorphous alloys and nanocrystalline alloys work, so a certain degree of energy-saving characteristics can be obtained. After switching to high output mode, even if the nanocrystalline alloy strips and amorphous alloy strips are saturated, the silicon steel strips with high saturation flux density are not saturated but work. The methods of Examples 3 and 4 are suitable for magnetic components used in a wide range from low output mode to high output mode.

[0094] Assuming that the same magnetic component such as a transformer or motor core is prepared, compared with Examples 1 and 3 which do not require winding but require stamping and lamination steps, Examples 2 and 4 involve winding and lamination, which can advantageously achieve a reduction in the number of manufacturing steps for the magnetic component.

[0095] Industrial Applicability

[0096] According to the present invention, since the number of production steps is reduced, large-scale laminated boards, transformers, inductors, magnetic cores for motors, magnetic core components for generators and other magnetic components with excellent properties can be prepared from composite laminated soft magnetic tapes into which various soft magnetic tapes have advantageous combinations inserted, so the industrial applicability is high.

Claims

1. A composite laminated soft magnetic tape, which is obtained by laminating and stacking a plurality of types of soft magnetic metal tapes having different characteristics and equal widths, and then fixing the plurality of laminated soft magnetic tapes, characterized in that: The plurality of types of soft magnetic ribbons always include amorphous alloy ribbons and nanocrystalline alloy ribbons.

2. A composite laminated soft magnetic tape, which is obtained by winding and fixing the laminated soft magnetic tape multiple times, characterized in that: The laminated soft magnetic ribbon is formed by laminating an amorphous alloy ribbon and a nanocrystalline alloy ribbon having equal widths.

3. A composite laminated soft magnetic tape, obtained by stacking and then fixing a plurality of laminated soft magnetic tapes, characterized in that: The laminated soft magnetic tape is formed by laminating one or more layers having narrower amorphous alloy tapes and nanocrystalline alloy tapes aligned on a wider silicon steel sheet tape so that the total width of the narrower amorphous alloy tapes and the nanocrystalline alloy tapes can be substantially equal to the width of the wider silicon steel sheet tape.

4. A composite laminated soft magnetic tape, which is formed by: winding the laminated soft magnetic tape multiple times, the laminated soft magnetic tape is formed by aligning narrower amorphous alloy tapes and nanocrystalline alloy tapes on a wider silicon steel sheet tape so that the total width of the narrower amorphous alloy tapes and the nanocrystalline alloy tapes can be substantially equal to the width of the wider silicon steel sheet tape, and then only winding the aligned narrower amorphous alloy tapes and the nanocrystalline alloy tapes so that the total width of the narrower amorphous alloy tapes and the nanocrystalline alloy tapes can be substantially equal to the width of the wider silicon steel sheet tape and fixing them.

5. A composite laminated soft magnetic tape, characterized in that: If the narrower amorphous alloy ribbon and the nanocrystalline alloy ribbon according to claim 4 do not have equal thickness, only the narrower amorphous alloy ribbon and the nanocrystalline alloy ribbon are wound multiple times, and then one of the thicker soft magnetic ribbons of the amorphous alloy ribbon and the nanocrystalline alloy ribbon is cut, and the other soft magnetic ribbon is further wound and cut and fixed when the total thickness of the other soft magnetic ribbon is substantially equal to the thickness of the thicker soft magnetic ribbon.

6. A magnetic component made of the composite laminated soft magnetic tape as claimed in claims 1 to 5, characterized in that: The magnetic component is one of a transformer, a reactor, a magnetic core of a motor, a magnetic core of a generator, and a large laminate.