Atomizing core, atomizer and electronic atomizing device

By using porous glass ceramic matrix and metal heating body, the problem of insufficient strength of the porous matrix of the electronic cigarette atomized core is solved, and a higher service life and stability are achieved, ensuring performance under thermal shock.

CN119054965APending Publication Date: 2024-12-03SMOORE INTERNATIONAL HOLDINGS LIMITED
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310647629.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-06-01
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The porous matrix of existing electronic cigarette atomized cores has poor strength and insufficient thermal shock resistance, resulting in a short service life.

Method used

The porous glass ceramic matrix is ​​used as the porous matrix of the atomized core. By controlling the difference in the content of main elements in any two measurement areas in the matrix to be within 10%, the stability and strength of the matrix are ensured, and combined with the use of metal heating bodies.

Benefits of technology

It significantly improves the strength and stability of the atomized core, extends the service life, enhances resistance under thermal shock conditions, and improves the oil conduction effect and taste.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119054965A_ABST
    Figure CN119054965A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of electronic atomization, in particular to an atomization core, an atomizer and an electronic atomization device. The atomizing core provided by the invention comprises a porous matrix and a heating body, the porous substrate is a porous glass ceramic substrate, any two measurement areas on the porous glass ceramic substrate are respectively marked as a first measurement area and a second measurement area, in terms of atomic percent, the main element content of the first measurement area is marked as M at%, the corresponding main element content of the second measurement area is marked as N at%, and M-N / M is less than 10% and / or M-N / N is less than 10%; the length of the measurement area is at least greater than 1 [mu] m; the main element is an element with the element content of more than 20 at% in the porous glass ceramic matrix. By controlling the conditions, the strength of the porous matrix can be effectively improved, the stability of the matrix is better, and the service life of the matrix is effectively prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of electronic atomization, and in particular to an atomization core, an atomizer and an electronic atomization device. Background Art

[0002] As a good substitute for traditional cigarettes, the advantage of electronic cigarettes is that they reduce harmful substances such as tar and CO in smoke. At present, the atomization method of electronic cigarettes on the market is mainly resistance heating atomization, which atomizes the electronic cigarette oil through the heat of the atomizer core. The existing atomizer core usually includes a porous matrix and a heating element. The porous matrix usually uses materials with a porous structure such as cotton core and porous ceramics to achieve the function of guiding the atomized medium to the heating element.

[0003] However, in the prior art, ceramic materials are usually prepared using materials such as diatomaceous earth. The components of traditional ceramic materials such as diatomaceous earth are complex, resulting in poor strength of the porous matrix of the electronic cigarette, poor thermal shock resistance, and easy local detachment and fracture, which in turn affects its service life. Summary of the invention

[0004] The purpose of the present invention is to overcome the defect in the prior art that the porous matrix of the atomizer core has poor strength and affects its service life, and further provide an atomizer core, an atomizer and an electronic atomization device.

[0005] In order to achieve the above object, the present invention adopts the following technical scheme:

[0006] The present invention provides an atomizer core, which includes a porous matrix and a heating element;

[0007] The porous substrate is a porous glass ceramic substrate, and any two measurement areas on the porous glass ceramic substrate are respectively recorded as a first measurement area and a second measurement area, and in terms of atomic percentage, the main element content of the first measurement area is recorded as Mat%, and the corresponding main element content of the second measurement area is recorded as Nat%, wherein |MN| / M is less than 10% and / or |MN| / N is less than 10%;

[0008] The length of the measuring area is at least greater than 1 μm; the main element is an element with an element content greater than 20 at % in the porous glass-ceramic matrix.

[0009] Preferably, in terms of atomic percentage, the main element content in the first measurement area is recorded as Mat%, and the corresponding main element content in the second measurement area is recorded as Nat%, wherein |MN| / M is less than 5% and / or |MN| / N is less than 5%.

[0010] Preferably, the main elements include a first main element and a second main element; in terms of atomic percentage, the content of the first main element in the porous glass-ceramic matrix is ​​55-64 at %; the content of the second main element is 20-36 at %.

[0011] Preferably, the first main element is oxygen, and the second main element is silicon;

[0012] Optionally, any two measurement areas on the porous glass-ceramic substrate are respectively recorded as the first measurement area and the second measurement area. In atomic percentage, the O element content in the first measurement area is recorded as Mat%, and the corresponding O element content in the second measurement area is recorded as Nat%, wherein |MN| / M is less than 10% and / or |MN| / N is less than 10%; the Si element content in the first measurement area is recorded as M'at%, and the corresponding Si element content in the second measurement area is recorded as N'at%, wherein |M'-N'| / M' is less than 10% and / or |M'-N'| / N' is less than 10%; the length of the measurement area is at least greater than 1 μm.

[0013] Preferably, the elements in the porous glass-ceramic matrix further include at least one element of sodium, magnesium, aluminum and calcium.

[0014] Preferably, the average pore size of the porous glass-ceramic matrix is ​​15-45 μm.

[0015] Preferably, the length of the measuring area is at least twice the average pore diameter.

[0016] Preferably, the compressive strength of the porous glass-ceramic matrix is ​​greater than 1.5 MPa;

[0017] Preferably, the compressive strength of the porous glass-ceramic matrix is ​​6-18 MPa.

[0018] Preferably, the porous glass-ceramic matrix includes a crystalline phase and an amorphous phase;

[0019] Preferably, the proportion of the crystalline phase is greater than 50wt%;

[0020] Preferably, the crystalline phase includes a quartz phase.

[0021] Preferably, the measurement area is at least one of circular, elliptical or rectangular.

[0022] Preferably, the heating element is a metal heating film.

[0023] The present invention provides an atomizer, wherein the atomizer comprises the atomizing core described above.

[0024] The present invention further provides an electronic atomization device, wherein the atomizer described above in the electronic atomization device further includes a battery assembly.

[0025] Beneficial effects of the present invention:

[0026] The present invention uses a porous glass ceramic substrate as the porous substrate of the atomizer core, and controls the main element content between any two measurement areas of the porous glass ceramic substrate at the same time. Any two measurement areas on the porous glass ceramic substrate are respectively recorded as the first measurement area and the second measurement area. In terms of atomic percentage, the main element content of the first measurement area is recorded as Mat%, and the corresponding main element content of the second measurement area is recorded as N at%, wherein |MN| / M is less than 10% and / or |MN| / N is less than 10%; the length of the measurement area is at least greater than 1μm; the main element is an element with an element content greater than 20at% in the porous glass ceramic substrate. The inventors found that by controlling the above conditions, the strength of the porous substrate and the atomizer core can be effectively improved, the stability of the substrate is better, and its service life is effectively extended. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0028] Figure 1 A physical picture of the atomizer core of Example 1 of the present invention;

[0029] Figure 2 A physical picture of the porous substrate of the atomizer core of Example 1 of the present invention;

[0030] Figure 3 SEM image of the porous matrix of the atomizer core of Example 2 of the present invention and the measurement area selected in Test Example 1;

[0031] Figure 4 The measurement area selected for the porous substrate of Example 2 in Test Example 1 of the present invention;

[0032] Figure 5 A schematic structural diagram of the atomizer of the present invention;

[0033] Figure 6 A schematic diagram of the structure of the electronic atomization device of the present invention;

[0034] Figure numerals: 1-atomizer, 2-battery assembly. DETAILED DESCRIPTION

[0035] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.

[0036] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.

[0037] In the prior art, ceramic materials are usually prepared using materials such as diatomaceous earth. The components of traditional ceramic materials such as diatomaceous earth are complex, and the porous matrix prepared therefrom has poor strength and poor thermal shock resistance, and is prone to detachment and breakage, thereby affecting its service life.

[0038] To this end, the present invention provides an atomizer core, which includes a porous matrix and a heating element; the porous matrix is ​​a porous glass ceramic matrix, and any two measurement areas on the porous glass ceramic matrix are respectively recorded as the first measurement area and the second measurement area, in terms of atomic percentage, the main element content of the first measurement area is recorded as Mat%, and the corresponding main element content of the second measurement area is recorded as N at%, wherein |MN| / M is less than 10% and / or |MN| / N is less than 10%; the length of the measurement area is at least greater than 1 μm, and the main element is an element with an element content greater than 20 at% in the porous glass ceramic matrix. The inventor found that by controlling the above conditions, the strength of the porous matrix and the atomizer core containing the matrix can be effectively improved, the stability of the matrix is ​​better, and its service life is effectively extended. In addition, the overall strength of the prepared porous matrix is ​​uniform, the composition is uniform, and the stability of the porous matrix is ​​also stronger under thermal shock during the atomization process. It is not easy to cause local cracks, damage, etc. due to different components, and its pore structure is easy to control, the oil guide effect is good, it is not easy to produce smoke stains, and the taste is not affected. Therefore, the atomizer core prepared by the porous matrix has a longer service life, a better oil conduction effect, and does not affect the taste.

[0039] In an optional embodiment, the first measurement area and the second measurement area may or may not intersect, and optionally, the first measurement area and the second measurement area do not intersect. In terms of atomic percentage, the main element content of the first measurement area is recorded as Mat%, and the corresponding main element content of the second measurement area is recorded as N at%, wherein |MN| / M and / or |MN| / N is less than 5%; for example, |MN| / M and / or |MN| / N can be selected to be 0.01%, 0.1%, 0.2%, 0.5%, 0.7%, 0.9%, 1%, 1.3%, 1.4%, 1.6%, 1.8%, 1.9%, 2%, 2.1%, 2.6%, 2.8%, 2.9%, 3%, 3.4%, 3.6%, 3.7%, 3.8%, 3.9%, 4%, 4.2%, 4.3%, 4.5%, 4.7%, 4.8%, 4.9%. The inventors found that by controlling |MN| / M and / or |MN| / N to be less than 5%, the strength uniformity of the porous matrix can be further improved, the stability of the matrix is ​​better, and its service life is further effectively extended.

[0040] In an optional embodiment, the main elements include a first main element and a second main element; optionally, in terms of atomic percentage, the content of the first main element in the porous glass-ceramic matrix is ​​55-64at%; the content of the second main element is 20-36at%. For example, the content of the first main element can be 55at%, 57at%, 59at%, 60at%, 61at%, 63at%, 64at%, and the content of the second main element can be 20at%, 21at%, 22at%, 24at%, 26at%, 27at%, 28at%, 29at%, 30at%, 31at%, 32at%, 33at%, 34at%, 35at%, 36at%. Further, the first main element is oxygen (O) and the second main element is silicon (Si).

[0041] In an optional embodiment, any two measurement areas on the porous glass-ceramic substrate are respectively recorded as the first measurement area and the second measurement area. In terms of atomic percentage, the O element content in the first measurement area is recorded as Mat%, and the corresponding O element content in the second measurement area is recorded as Nat%, wherein |MN| / M is less than 10% and / or |MN| / N is less than 10%; the Si element content in the first measurement area is recorded as M'at%, and the corresponding Si element content in the second measurement area is recorded as N'at%, wherein |M'-N'| / M' is less than 10% and / or |M'-N'| / N' is less than 10%; the length of the measurement area is at least greater than 1 μm.

[0042] In an optional embodiment, the elements in the porous glass-ceramic matrix also include at least one element of sodium, magnesium, aluminum, and calcium. Optionally, in terms of atomic percentage, the elements in the porous glass-ceramic matrix also include at least one element of sodium 2.4-6at%, magnesium 0.13-3.18at%, aluminum 0.23-2.42at%, and calcium 1.35-6at%.

[0043] In an optional embodiment, the porous glass-ceramic matrix includes a crystalline phase and an amorphous phase, and the crystalline phase accounts for more than 50wt%. For example, it can be selected that the crystalline phase accounts for 50wt%, 55wt%, 60wt%, 65wt%, 66wt%, 70wt%, 75wt%, 80wt%, 85wt%, 90wt%, 95wt%. Further, the crystalline phase includes a quartz phase. The matrix material of the porous glass-ceramic matrix prepared in this application is essentially glass-ceramic (Glass-ceramic), and glass-ceramic has excellent mechanical and thermal properties such as corrosion resistance, high temperature resistance, thermal shock resistance, and adjustable thermal expansion. It is especially used in atomization cores. Good corrosion resistance determines its good safety and is not easy to precipitate harmful components; good high temperature resistance and thermal shock resistance determine that it has good mechanical stability and reliability under repeated high temperature shocks.

[0044] In an optional embodiment, the average pore size of the porous glass-ceramic matrix is ​​15-45 μm. For example, the average pore size of the porous glass-ceramic matrix can be 15 μm, 16 μm, 17 μm, 18 μm, 19 μm, 20 μm, 21 μm, 22 μm, 23 μm, 24 μm, 25 μm, 26 μm, 27 μm, 28 μm, 29 μm, 30 μm, 31 μm, 32 μm, 33 μm, 34 μm, 35 μm, 36 μm, 37 μm, 38 μm, 39 μm, 40 μm, 41 μm, 42 μm, 43 μm, 44 μm, 45 μm. The pore size range is moderate, and it has both the effect of guiding and locking liquid. It should be noted that the pore size of the porous glass-ceramic matrix can also be controlled and adjusted by the selection of raw glass bubbles. Through appropriate screening, raw glass bubbles of the required particle size can be obtained. Through suitable raw glass bubbles and preparation process, the pore structure of the porous glass-ceramic matrix can be controlled.

[0045] D50 glass ceramic bubble particle size corresponds to the particle size corresponding to the cumulative particle size distribution percentage of glass ceramic bubbles reaching 50%. Its physical meaning is that glass ceramic bubbles with a particle size larger than it account for 50%, and glass ceramic bubbles with a particle size smaller than it also account for 50%. D50 is also called the median diameter or median particle size; similarly, D50 pore size corresponds to the pore size corresponding to the cumulative pore size distribution percentage of the porous glass ceramic matrix reaching 50%. Its physical meaning is that pores with a pore size larger than it account for 50%, and pores with a pore size smaller than it also account for 50%.

[0046] In an optional embodiment, the length of the measurement area is at least twice the average pore size; for example, the length of the measurement area can be selected to be at least 2 times, 3 times, 5 times, 10 times, 20 times, 30 times, 50 times, 100 times, 150 times, 200 times the average pore size. The aspect ratio of the selected measurement area is less than 2. The inventors found that the measurement area selected within this range can effectively improve the strength of the matrix by controlling its main content components, while achieving the strength uniformity of the porous matrix. The present invention adopts the method of glass bubble sintering to obtain the matrix material, and the composition of the porous matrix has uniformity within a specific range, which can make its structure controllable, and the strength, strength consistency and reliability of the finished product are higher.

[0047] In an optional embodiment, the compressive strength of the porous glass-ceramic matrix is ​​greater than 1.5 MPa; further preferably, the compressive strength of the porous glass-ceramic matrix is ​​6-18 MPa. For example, it can be selected that the compressive strength of the porous glass-ceramic matrix is ​​6MPa, 6.1MPa, 6.3MPa, 6.5MPa, 6.6MPa, 6.7MPa, 6.8MPa, 6.9MPa, 7MPa, 7.1MPa, 7.3MPa, 7.4MPa, 7.5MPa, 7.6MPa, 7.8MPa, 7.9MPa, 8MPa, 8.5MPa, 9MPa, 9.5MPa, 10MPa, 10.5MPa, 11MPa, 11.5MPa, 12MPa, 12.5MPa, 13MPa, 13.5MPa, 14MPa, 14.5MPa, 15MPa, 15.5MPa, 16MPa, 16.5MPa, 17MPa, 17.5MPa, 18MPa.

[0048] In an optional embodiment, the porous glass-ceramic matrix includes a crystalline phase and an amorphous phase, and the crystalline phase accounts for more than 50%. For example, the crystalline phase can be selected to account for 50%, 55%, 60%, 65%, 66%, 70%, 75%, 80%, 85%, 90%, 95%, 99%, 100%. Further, the crystalline phase includes a quartz phase.

[0049] In an optional embodiment, the porosity in the porous glass-ceramic matrix is ​​50-90%; for example, the porosity in the porous glass-ceramic matrix can be 50%, 55%, 60%, 65%, 66%, 70%, 75%, 80%, 85%, or 90%.

[0050] The present invention is further described below in conjunction with the preparation method.

[0051] In some optional embodiments, the method for preparing the atomizer core comprises the following steps:

[0052] 1) mixing glass raw materials with a binder, a lubricant and water and extruding the mixture to obtain a green body;

[0053] 2) subjecting the green body in step 1) to a first sintering, a second sintering and a third sintering to obtain a porous glass-ceramic matrix;

[0054] 3) The raw material of the heating element is prepared on the porous glass ceramic substrate in step 2) and sintered into shape.

[0055] In some optional embodiments, in step 1): the glass raw material is selected from at least one of glass bubbles and glass powder; the binder can be an organic binder; specifically, the binder is selected from at least one of methyl cellulose, hydroxyethyl cellulose, and hydroxypropyl methyl cellulose; the lubricant can be an aliphatic hydrocarbon lubricant, such as paraffin, metal stearate; specifically, the lubricant is sodium stearate.

[0056] In some optional embodiments, the pressure of the extrusion molding in step 1) is 1-40 bar. Most of the glass bubbles do not break during the extrusion molding process, and the single glass bubble maintains a complete spherical shape. Therefore, the extrusion molding pressure can be appropriately adjusted according to the compressive strength of the selected glass bubble.

[0057] In some optional embodiments, the first temperature of the first sintering in step 2) is at least 200° C., such as 300° C. to 400° C., and / or the first residence time is at least 1 minute, such as 1 to 10 hours. During the sintering process at this temperature, substances such as solvents and binders in the green body are removed.

[0058] In some optional embodiments, the second temperature of the second sintering is greater than 400°C and less than the softening point of the glass of the glass bubble; for example, 500°C, 600°C, 700°C, etc., and the second residence time is at least 1 minute, for example, 1 to 10 hours. The second temperature is higher than 400°C and lower than the softening point of the glass of the glass bubble / glass powder. The purpose is to keep the original shape of the blank unchanged. At the same time, since the temperature is already higher than 400°C, the glass component in the glass bubble / glass powder begins to undergo a phase change, and the disordered glass phase partially crystallizes into a crystalline phase within this temperature range. The glass bubble is transformed into a glass ceramic bubble or the proportion of the crystalline phase in the glass bubble begins to increase. At the same time, due to this transformation, some glass bubbles begin to break and have at least one opening. Therefore, the sintering time within this temperature range can be appropriately adjusted to adjust the crystallinity of the porous glass ceramic. It can be understood that the raw glass bubble / glass powder itself can also contain a certain proportion of crystalline phases, which can shorten the sintering time in this process.

[0059] In some optional embodiments, the third temperature of the third sintering is greater than the softening point of the glass. Specifically, the softening point temperature of the glass is less than 900°C. The third residence time can be at least 1 minute, for example, 1 to 10 hours. At this temperature, the glass component has fluidity, so the adjacent glass-ceramic bubbles are directly bonded to each other, and the glass-ceramic bubbles are bonded to form a porous glass-ceramic matrix of an integral structure; at the same time, because the glass-ceramic bubbles still have crystalline phase components, the crystalline phase components serve as a skeleton so that their morphology does not collapse, and they still maintain a basically complete morphology. In addition, the glass-ceramic bubbles further crack to form a large number of openings, which are interconnected to form pores, and the pores extend through the porous glass-ceramic matrix and reach the surface of the porous glass-ceramic matrix.

[0060] The third temperature is higher than the softening point of the glass of the glass bubble. The glass ceramic bubble is heated to at least the softening temperature of the amorphous glass in the glass ceramic bubble, so that most of the glass ceramic bubbles are opened due to the expansion of the gas in the bubble, and the adjacent glass ceramic bubbles are sintered together by heating to form a bond. From the overall point of view, the bonded open glass ceramic bubbles form pores in the porous glass ceramic matrix, which can be used in atomizers and electronic atomization devices to effectively improve the atomization efficiency and liquid guiding effect.

[0061] In some optional embodiments, the mass ratio of glass raw material to binder, lubricant and water is (100-200): (10-50): (1-10): (50-150); optionally, the glass raw material is selected from glass bubbles and glass powder; optionally, the mass ratio of glass bubbles to glass powder is (1-100): (0-100).

[0062] In some optional embodiments, in step 3): the raw material of the heating element can be at least one of electronic paste (metal paste), heating wire or heating mesh. The electronic paste can be directly coated on the surface of the porous glass-ceramic substrate in a preset shape by silk-screen printing, and sintered at a preset temperature. The sintering temperature can be adaptively adjusted according to the type of bonding phase and metal components in the electronic paste, and the sintering temperature is usually 400-800°C. Optionally, in some other embodiments, the heating element can also be evaporated / deposited on the substrate by physical vapor deposition (PVD) or chemical vapor deposition (CVD). Alternatively, the metal wire or metal mesh is directly welded / attached to the surface of the substrate.

[0063] In some optional embodiments, the glass component in the glass bubble may be soda-lime silicate glass, borosilicate glass or other glass. Specifically, the glass component may include: SiO2 74-85%, CaO 6.5-10%, B2O3 5-9%, Al2O3 0.4-2%, Fe2O3 0.01-1%, Na2O 1-3%, K2O 0.1-0.5%.

[0064] In some optional embodiments, step 1) further includes adding a pore former. Optionally, the pore former is selected from at least one of starch, polymethyl methacrylate (PMMA), polystyrene (PS), and graphite. Optionally, the particle size range of the pore former can be 1-150 μm. It can be understood that the addition of the pore former can further improve the porosity of the porous glass ceramic matrix while ensuring the strength of the raw glass bubble.

[0065] In some optional embodiments, step 1) further includes a second inorganic material. The second inorganic material can be at least one of clay, talc, silica, and alumina. The melting point or softening point of the above materials is higher than the softening point of the glass in the glass bubble. Optionally, the particle size range of the pore former can be 1-200 μm.

[0066] In some optional embodiments, the mass ratio of glass raw material to binder, lubricant, water, pore former and second inorganic material is (100-200): (10-50): (1-10): (50-150): (0-125): (0-9); optionally, the glass raw material is selected from glass bubbles and glass powder; optionally, the mass ratio of glass bubbles to glass powder is (1-100): (0-100).

[0067] like Figure 5 As shown, the present invention also provides an atomizer, wherein the atomizer includes the atomizer core described above. The atomizer includes a shell, and a liquid storage tank and an atomization cavity are formed in the shell. The liquid storage tank is used to store liquid atomization medium, and the atomization cavity is used to accommodate the atomization core described above. The atomization core can atomize the liquid atomization medium.

[0068] like Figure 6 As shown, the present invention also provides an electronic atomization device, which includes the above-mentioned atomizer 1 and a battery assembly 2. The battery assembly and the atomizer can be an integrated structure or a detachable structure. The battery assembly is used to power the atomizer according to a preset mode, so that the atomizer atomizes the liquid atomization medium according to the preset mode.

[0069] The present invention is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed by the present invention.

[0070] The glass bubbles of the present invention are made of soda-lime silicate glass, and the following embodiments all use raw glass bubbles of the same composition. The raw material parameters are shown in Table 1, and the specific implementation is described as follows.

[0071] Example 1

[0072] This embodiment provides an atomizer core, and a preparation method thereof includes the following steps:

[0073] 1) 100 g of glass bubbles were mixed with 25 g of hydroxyethyl cellulose, 2.5 g of sodium stearate and 50 g of water and extruded to obtain a green body at a molding pressure of 7 bar;

[0074] 2) subjecting the green body in step 1) to a first sintering, a second sintering and a third sintering to obtain a porous glass ceramic substrate, wherein the first sintering temperature is 230° C., the first sintering time is 1 hour, the second sintering temperature is 650° C., the second sintering time is 2 hours; the third sintering temperature is 1050° C., the third sintering time is 1 hour; finally, the green body is naturally cooled in the furnace to obtain a porous glass ceramic substrate;

[0075] 3) Printing the heating element slurry on the porous glass ceramic substrate in step 2), sintering and forming, the sintering temperature is 620° C., the sintering time is 1 hour, and the atomization core is obtained. The heating element slurry is stainless steel.

[0076] like Figure 1 As shown, the prepared atomizer core has a porous matrix of a porous glass ceramic matrix (such as Figure 2 ), the porous matrix has a pore structure that is interconnected.

[0077] Example 2

[0078] This embodiment provides an atomizer core, and a preparation method thereof includes the following steps:

[0079] 1) 100 g of glass bubbles were mixed with 25 g of hydroxyethyl cellulose, 2.5 g of sodium stearate, 25 g of a pore former and 67 g of water, and the mixture was extruded to obtain a green body at a molding pressure of 14 bar.

[0080] 2) subjecting the green body in step 1) to a first sintering, a second sintering and a third sintering to obtain a porous glass ceramic substrate, wherein the first sintering temperature is 230° C., the first sintering time is 1 hour, the second sintering temperature is 650° C., the second sintering time is 2 hours; the third sintering temperature is 1210° C., the third sintering time is 1 hour; finally, the green body is naturally cooled in the furnace to obtain a porous glass ceramic substrate;

[0081] Step 3) is the same as in Example 1.

[0082] Example 3

[0083] This embodiment provides an atomizer core, and a preparation method thereof includes the following steps:

[0084] 1) 100 g of glass bubbles were mixed with 25 g of hydroxyethyl cellulose, 2.5 g of sodium stearate and 75 g of water and extruded to obtain a green body at a molding pressure of 24 bar.

[0085] Step 2) and step 3) are the same as in Example 1.

[0086] Example 4

[0087] This embodiment provides an atomizer core, and a preparation method thereof includes the following steps:

[0088] 1) 20g of glass bubbles, 80g of glass powder, 25g of hydroxyethyl cellulose, 2.5g of sodium stearate, 50g of pore former and 75g of water were mixed and extruded to obtain a green body, and the molding pressure was 13 bar. The pore former was polymethyl methacrylate (PMMA). The glass powder had no cavities inside, and the glass type of the glass powder was the same as that of the glass bubbles; the particle size of the glass powder was 1-20 μm.

[0089] Step 2) and step 3) are the same as in Example 1.

[0090] Example 5

[0091] This embodiment provides an atomizer core, and a preparation method thereof includes the following steps:

[0092] 1) 20g of glass bubbles, 80g of glass powder, 25g of hydroxyethyl cellulose, 2.5g of sodium stearate, 50g of pore former and 75g of water were mixed and extruded to obtain a green body at a molding pressure of 24 bar. The pore former was polymethyl methacrylate (PMMA). The glass powder had no cavities inside, and the glass type of the glass powder was the same as that of the glass bubbles; the particle size of the glass powder was 1-20 μm.

[0093] Step 2) and step 3) are the same as in Example 1.

[0094] Table 1 Example raw material glass bubble parameters

[0095]

[0096] Test Example 1

[0097] The porous glass ceramic substrate of the atomizer core of the embodiment of the present invention was scanned by SEM and the element content was detected. The element content was detected by energy dispersive spectrometer (EDS). The pore size was measured by mercury intrusion method (the testing instrument was mercury intrusion instrument).

[0098] Figure 3 and Figure 4 They are the SEM images of Example 2 and the EDS analysis of different measurement areas and different range sizes. Figure 3As shown in the measurement area, two different measurement areas are selected, and the aspect ratios of the selected measurement areas are all less than 2, which are respectively marked as area 1 (or marked as M) and area 2 (or marked as N). The element contents of each measurement area are detected as shown in Table 2. Among them, the detection area is a rectangle, and the length of the detection area is 151.17μm; the D50 of the raw material particles is 41μm, and the average pore size of the finished porous glass-ceramic matrix is ​​23.07μm. Obviously, the differences in the main elements of area 1 (or marked as M) and area 2 (or marked as N) are 1% (oxygen element) and 0% (silicon element), respectively. Similarly, the results shown in Table 2 are obtained by measuring other embodiments.

[0099] Table 2 Element contents of examples

[0100]

[0101] like Figure 4 As shown, different regions were selected in the porous glass-ceramic matrix obtained in Example 2 for measurement. The test results are shown in Table 3.

[0102] Table 3 Element contents in different regions of Example 2

[0103]

[0104]

[0105] As shown in Table 3, the measurement area length of region 1 is about 5 μm, and its width is about 3 μm; the difference between its main component oxygen content and that of region 2 is 8%, and the difference between another main component silicon and that of region 2 is 28%. Similarly, the difference between region 2 and region 3 is also very significant. The above-mentioned composition difference is much greater than the composition difference in different embodiments in Table 1. The inventor of the present application analyzed and believed that due to the phase change of the glass bubble or glass powder of the present application during the sintering process, composition segregation occurred, but the composition segregation only occurred in a very small range, usually not exceeding the range of a single glass bubble; therefore, when the length / range of each different measurement area is greater than the length / range of a single glass bubble, the difference in its composition will be very small, that is, the composition is uniform and consistent. Similarly, when the length / range of each different measurement area is less than the length / range of a single glass bubble, the difference in its composition will be very large, that is, the composition is uneven and inconsistent, and the reason is that the different smaller areas may actually correspond to different compositions such as the crystal phase or glass phase in the matrix material, and the composition has significant differences. Generally, the grain size in glass ceramics is less than 1 μm; therefore, when the length / range of the measurement area is greater than 1 μm, several crystalline phase areas and amorphous phase areas can be included in the measurement area in equal proportions, so that the test results of the composition tend to be consistent; that is, the composition of different measurement areas is uniform and consistent. Furthermore, since a completely molten liquid environment is not formed in the present application, the flow of the liquid phase is usually only carried out in a small range between adjacent / adjacent monomer glass bubbles. Therefore, when the length / range of the measurement area is greater than 2 times the pore size of the matrix, at least several sub-areas with composition differences can be included in equal proportions, and the composition results of different measurement areas tend to be uniform and consistent. For simple description, the average pore size is used as the length / range standard of the glass ceramic bubble in the matrix in the present application. The average pore size of the matrix in the present application is about 15-45 μm, and the corresponding measurement area length / range is greater than 30-90 μm. It should be noted that when the measurement area is elliptical, the length of its measurement area is its major axis; similarly, when the measurement area is selected as a circle, the length of its measurement area is its diameter. At the same time, the aspect ratio of the measurement area should not be too large. Usually, a ratio less than 2 can more accurately reflect the composition of the measurement area.

[0106] Among them, Figure 4 As shown in region 1 in FIG. 1 , its microstructure is significantly different from the surrounding tissue, and it can be seen that the porous glass-ceramic matrix includes a crystalline phase. Furthermore, the crystalline phase includes a quartz phase.

[0107] Test Example 2

[0108] The compressive strength test was carried out on the porous glass-ceramic matrix in the above embodiment. Five parallel samples were taken from the same embodiment and tested separately. The test method was referred to GB / T 4740-1999 "Test Method for Compressive Strength of Ceramic Materials". The pore size and porosity of the porous glass-ceramic matrix and other related parameters were measured by mercury intrusion method (the test instrument was a mercury intrusion instrument). The atomizer core in the above embodiment was tested for failure during the preset number of puffs (the preset number of puffs in the present invention was 500 puffs), and the life span was statistically recorded. The failure mainly included: 1. The resistance of the atomizer core changed significantly abnormally (such as: the resistance increased significantly due to the breakage and shedding of the heating element); 2. The amount of mist output was less than half of the initial atomization amount. The above test conditions were 6.5W power, bare chip (not assembled as an atomizer), and each puff process (i.e., each puff) included: puffing for 3s and then pausing for 8s. The test results are shown in Table 4.

[0109] Table 4

[0110]

[0111] As shown in Table 4, the inventors analyzed that: the overall compressive strength of the porous glass-ceramic matrix is ​​good, and all matrices are greater than 1.5MPa. For example, the porosity corresponding to Example 2 is 77.80%, and the porosity is very high, close to 80%, and it can still maintain a high compressive strength. In some embodiments, the compressive strength is greater than 6Mpa, and the corresponding porosity is greater than 60%. The inventors analyzed that above the range greater than a single glass bubble or glass powder, the composition uniformity is extremely high, so that the overall compressive strength of the matrix is ​​improved, and at the same time, the strength of each position of the matrix is ​​uniform, without obvious local strength defects, that is, the effect of improving the strength uniformity of the porous matrix is ​​achieved. At the same time, due to the uniform composition, the porous matrix is ​​more stable under thermal shock during the atomization process, and it is not easy to cause local cracks, damage, etc. due to different compositions; and there are no harmful substances such as heavy metals that can be precipitated in the composition. Therefore, the service life of the atomizer core is longer, safer and more reliable.

[0112] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.

Claims

1. An atomizer core, characterized in that: The atomizing core comprises a porous matrix and a heating element; The porous substrate is a porous glass ceramic substrate, and any two measurement areas on the porous glass ceramic substrate are respectively recorded as a first measurement area and a second measurement area, and in terms of atomic percentage, the main element content of the first measurement area is recorded as Mat%, and the corresponding main element content of the second measurement area is recorded as Nat%, wherein |MN| / M is less than 10% and / or |MN| / N is less than 10%; The length of the measuring area is at least greater than 1 μm; the main element is an element with an element content greater than 20 at % in the porous glass-ceramic matrix.

2. The atomizer core according to claim 1, characterized in that: In terms of atomic percentage, the main element content in the first measurement area is recorded as Mat%, and the corresponding main element content in the second measurement area is recorded as Nat%, wherein |MN| / M is less than 5% and / or |MN| / N is less than 5%.

3. The atomizer core according to claim 1 or 2, characterized in that: The main elements include a first main element and a second main element; in terms of atomic percentage, the content of the first main element in the porous glass-ceramic matrix is ​​55-64 at%; the content of the second main element is 20-36 at%; Preferably, the first main element is oxygen, and the second main element is silicon; Preferably, the elements in the porous glass-ceramic matrix further include at least one element of sodium, magnesium, aluminum and calcium.

4. The atomizer core according to any one of claims 1 to 3, characterized in that: The average pore size of the porous glass-ceramic matrix is ​​15-45 μm.

5. The atomizer core according to claim 4, characterized in that: The length of the measurement area is at least twice the average pore diameter.

6. The atomizer core according to any one of claims 1 to 5, characterized in that: The compressive strength of the porous glass-ceramic matrix is ​​greater than 1.5 MPa; Preferably, the compressive strength of the porous glass-ceramic matrix is ​​6-18 MPa.

7. The atomizer core according to any one of claims 1 to 6, characterized in that: The porous glass-ceramic matrix includes a crystalline phase and an amorphous phase; Preferably, the proportion of the crystalline phase is greater than 50wt%; Preferably, the crystalline phase includes a quartz phase.

8. The atomizer core according to any one of claims 1 to 7, characterized in that: The measurement area is at least one of a circle, an ellipse or a rectangle.

9. The atomizer core according to any one of claims 1 to 8, characterized in that: The heating element is a metal heating film.

10. An atomizer, characterized in that: The atomizer comprises the atomizer core according to any one of claims 1 to 9.

11. An electronic atomization device, characterized in that: The electronic atomization device includes the atomizer according to claim 10 and also includes a battery assembly.

Citation Information

Cited By

  • Atomization core, atomizer and electronic atomization device

    EP4721601A1