Preparation process of catalyst for sulfur-containing tail gas treatment

Through the high-temperature roasting and low-temperature combustion of the composite catalyst, a stable structure is formed, which solves the problems of low efficiency and poor stability in sulfur-containing exhaust gas treatment, and achieves the catalytic effect of efficient conversion and long life.

CN119056477APending Publication Date: 2024-12-03SHANGHAI DONGHUA ENVIRONMENT ENG +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411174964.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Sulfur-containing exhaust gas poses a serious threat to the environment and human health. The existing catalysts are inefficient and have poor stability in treatment, making it difficult to effectively reduce sulfide emissions.

Method used

A composite catalyst is used, consisting of silicon oxide, silicon carbide, perovskite, aluminum nitrate and tungsten sulfide, and a stable structure is formed through high-temperature calcination and low-temperature combustion, which increases the active site and specific surface area, and improves catalytic efficiency and stability.

Benefits of technology

It achieves efficient conversion of sulfur-containing exhaust gas, and the catalyst maintains activity and structural stability in a high-temperature environment, extends its service life, and reduces environmental pollution.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a preparation process of a catalyst for sulfur-containing tail gas treatment, and belongs to the technical field of catalysts. Silicon oxide and silicon carbide are mixed and roasted at the temperature of 1800 DEG C to prepare the non-metal catalytic component, nitrogen is used for slow cooling, and the prepared non-metal catalytic component has multiple active sites and high catalytic efficiency; in order to combine perovskite and aluminum nitrate nonahydrate by selecting a low-temperature combustion method and selecting glycine and urea as fuels, the method has the advantages of low ignition temperature, reaction self-maintenance and short synthesis time, and the specific surface area of the prepared catalyst is large due to heat release in the reaction; the composite catalyst with excellent sulfur removal performance is obtained by combining a non-metal catalytic component silicon oxide and silicon carbide mixture, a metal catalytic component perovskite and aluminum nitrate conjugate and a metal catalytic component tungsten sulfide.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of catalysts and relates to a preparation process of a catalyst for treating sulfur-containing tail gas. Background Art

[0002] The emission of sulfur-containing tail gas into the atmosphere will seriously affect the air quality, increase the PM2.5 index, and form pollution phenomena such as haze. Sulfide will generate acid rain when it meets water, which will corrode buildings and damage sculptures, and this damage is irreversible. Acid rain will also acidify the soil, leading to the loss of soil nutrients and adversely affecting the growth of crops. In addition, acid rain will affect the survival and reproduction of aquatic plants and animals and destroy the ecological balance; sulfur-containing tail gas will also irritate the eyes and respiratory system, causing discomfort and disease. Hydrogen sulfide has the smell of rotten eggs, and its lethal concentration is extremely low, posing a serious threat to human health. People who are exposed to sulfur-containing tail gas for a long time may experience symptoms such as dizziness, headache, and respiratory inflammation. In severe cases, it may cause pulmonary edema, laryngeal edema, or vocal cord spasm and suffocation.

[0003] In order to reduce the impact on the environment, catalytic oxidation can be used to treat sulfur-containing tail gas. Under the action of the catalyst, hydrogen sulfide is oxidized into sulfur or sulfuric acid, reducing the sulfur content in the exhaust gas, thereby reducing the impact of sulfides on the environment and human health. Summary of the invention

[0004] The object of the present invention is to provide a preparation process of a catalyst for treating sulfur-containing tail gas, which has the characteristics of multiple active sites and high catalytic efficiency.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A process for preparing a catalyst for treating sulfur-containing tail gas, wherein the specific process for preparing the catalyst is as follows:

[0007] S1: Silicon carbide and silicon oxide were mixed in a molar ratio of 0.8:1, and ground in a ball mill at a speed of 300 r / min for 1 h to obtain a mixture A;

[0008] S2: heating the mixture A from room temperature to 1800°C, and calcining at 1800°C for 3 hours. After the calcination, nitrogen is evenly sprayed on the powder to cool it slowly. After the cooling is completed, a mixture B is obtained, and the mixture B is stored in a nitrogen atmosphere;

[0009] S3: mixing glycine and urea in a mass ratio of 2:1, mixing evenly, and grinding in a ball mill at a speed of 300 r / min to obtain a mixture C;

[0010] S4: perovskite and aluminum nitrate nonahydrate were mixed in a mass ratio of 1:2, and ground in a ball mill at a speed of 300 r / min until the product was a viscous mixture to obtain a mixture D, 1 wt % of the mixture C was added to the mixture D, and ultrasonicated at 25° C. for 0.5 h to obtain a mixture E;

[0011] S5: placing the mixture E into a preheated muffle furnace, burning for 1 to 3 minutes, and after complete combustion, heating from the preheating temperature to 500 to 600° C., calcining at 500 to 600° C. for 2 hours to obtain a mixture F;

[0012] S6: Under a nitrogen atmosphere, the mixture B, the mixture F and tungsten sulfide are mixed in a mass ratio of 2:2:1, and ground at 200° C. and 300 r / min for 2 h. After the grinding, the mixture is cooled to room temperature to obtain the catalyst.

[0013] Furthermore, the heating rate of the mixture A in S2 from room temperature to 1800° C. is 10° C. / min.

[0014] Furthermore, the injection parameters of the nitrogen in S2 are as follows: the injection flow rate is 1m 3 / min, the pressure is 1MPa.

[0015] Furthermore, the parameters of the ultrasound in S4 are a frequency of 47 kHz and a power of 30 W.

[0016] Furthermore, the preheating temperature in S5 is 200-300°C.

[0017] Furthermore, the heating rate in S5 is 5°C / min.

[0018] Furthermore, the cooling rate in S6 is 2°C / min.

[0019] Furthermore, the catalyst particles obtained by grinding in S6 have a particle size of 200 meshes.

[0020] The catalyst used in the present invention is a composite catalyst, which is composed of a metal catalytic component and a non-metallic catalytic component. When the two are combined, they can produce a synergistic effect and accelerate the reaction rate. Therefore, compared with a single catalyst, it has higher catalytic efficiency and better stability.

[0021] The present invention selects silicon oxide and silicon carbide for mixed calcination to obtain a non-metallic catalytic component. The present invention first performs calcination at 1800°C. At this temperature, the interaction between silicon oxide and silicon carbide can be effectively promoted to form a more stable mixed structure. This structure can provide more active sites, thereby enhancing the catalytic activity of the catalyst, so that it can show higher efficiency and performance when treating sulfur-containing compounds; during the calcination process at 1800°C, the silicon oxide will be partially decomposed and reorganized to form a rich pore structure. These pore structures can not only provide a larger specific surface area and increase the number of active sites, but also improve the adsorption performance of the catalyst, so that it can better adsorb and convert sulfur-containing compounds; calcination at 1800°C can further consolidate the stability of silicon oxide and silicon carbide, so that the prepared desulfurization catalyst can maintain its catalytic activity and structural stability in a high temperature environment; silicon oxide calcined at high temperature The internal structure of the mixture with silicon carbide will become tighter and more stable, thereby enhancing its mechanical strength. This high mechanical strength catalyst can better resist erosion and wear during gas flow and extend the service life of the catalyst. Both silicon oxide and silicon carbide are environmentally friendly materials, and no toxic or harmful by-products are produced during their preparation. These two materials are widely present in nature, easy to obtain and recycle, and have good sustainability and environmental protection. In addition, silicon carbide also has an adsorption effect. The adsorption effect of silicon carbide is achieved through the interaction between gas molecules and the surface of the material. There are some unsaturated chemical bonds and holes on the surface of silicon carbide. These holes will generate a gravitational field to attract gas molecules. When gas molecules come into contact with the surface of silicon carbide, chemical adsorption or physical adsorption will occur. The high adsorption of silicon carbide can increase the contact area between the reactant molecules and the catalyst, thereby improving the reaction efficiency.

[0022] In addition, the present invention uses nitrogen to slowly cool the calcined silicon oxide and silicon carbide. The nitrogen cooling process can further stabilize the structure of silicon oxide and silicon carbide and prevent structural damage caused by rapid cooling; nitrogen cooling can effectively prevent the catalyst from reacting with oxygen in the air at high temperature, causing the active sites on the catalyst surface to be oxidized and deactivated. Therefore, using nitrogen cooling can maintain the activity of the catalyst surface and improve the catalytic performance of the catalyst.

[0023] Perovskite exhibits excellent catalytic performance due to its unique active center structure and high specific surface area. Combined with aluminum nitrate, it can form a composite catalyst with higher activity, which can effectively promote the decomposition and conversion of sulfides; Perovskite has high chemical stability and thermal stability, and can remain stable even in high temperature, high pressure, reducing or oxidizing environments. After combining with aluminum nitrate, this stability may be further enhanced, so that the catalyst can maintain its catalytic activity and performance in long-term use. In order to better combine perovskite and aluminum nitrate, the present invention uses a low-temperature combustion method to combine the two. Glycine and urea are selected as fuels. The mass ratio of glycine to urea in the present invention is 2:1. This is because if the proportion of urea is too high, it will lead to excessive oxygen content during the combustion process, which will increase the impurities in the prepared catalyst and reduce the performance of the catalyst; and if the proportion of glycine is too high, it will lead to insufficient combustion reaction, and unreacted raw materials will remain in the product.

[0024] Low-temperature combustion method is a technology obtained by combining combustion synthesis method and wet chemical method. Combustion synthesis is a synthesis method that uses the self-heating of chemical reaction to make the reaction continue. The biggest feature is the self-heating and self-sustaining of the synthesis reaction. No external energy supply is required during the synthesis process. However, due to the high combustion temperature, the particle size of the synthesized catalyst is too large and difficult to control. Therefore, the low-temperature combustion method is obtained by combining wet chemical method. This method has a low ignition temperature, self-sustaining reaction, short synthesis time, and heat release during the reaction, which makes the catalyst have a large specific surface area.

[0025] The essence of the combustion reaction is actually a redox reaction. Therefore, in the present invention, aluminum nitrate nonahydrate is selected as the oxidant, and a mixture of glycine and urea is selected as the reductant (fuel). The metal nitrate acts as an oxidant and also provides the metal ions required by the catalyst. In addition, the addition of the nitrate also ensures the good solubility of the metal particles.

[0026] As combustion agents, glycine and urea can burn rapidly at a relatively low temperature, releasing a large amount of heat. This rapid combustion process helps promote rapid mixing and melting of raw materials, making the reaction more uniform and efficient. In addition, the gases (such as carbon dioxide, water vapor, etc.) generated during the combustion process can play a good pore-forming role, increase the specific surface area of ​​the catalyst, and thus improve its catalytic activity; glycine and urea, as organic ligands, can form a complex with aluminum nitrate and perovskite precursors to form a stable complex. This complex can maintain structural stability during the combustion process, avoid volatilization and loss of raw materials at high temperatures, thereby ensuring the accuracy of the chemical composition and structure of the catalyst; glycine and urea can also produce a reducing atmosphere during the combustion process, which helps to reduce high-valent metal ions to low-valent states and improve the catalytic performance of the catalyst. For example, in the perovskite desulfurization reaction, low-valent metal ions often have higher catalytic activity; as combustion agents, glycine and urea have combustion products that are mainly harmless substances such as carbon dioxide and water vapor, which meet environmental protection requirements. At the same time, since the heat released during its combustion process can be fully utilized, it also helps to save energy and reduce consumption.

[0027] Tungsten sulfide exhibits extremely high catalytic activity in catalytic desulfurization reactions and can effectively convert sulfides into substances that are easy to handle, thereby significantly improving desulfurization efficiency; tungsten sulfide catalysts have good selectivity for sulfides and can accurately identify and catalyze sulfides in complex reaction systems, reducing interference with other components; tungsten sulfide catalysts have strong chemical and thermal stability and can operate stably for a long time under harsh environments such as high temperature and high pressure to maintain catalytic activity; tungsten sulfide catalysts are not easy to deactivate during the catalytic process, and even after deactivation, their catalytic activity can be restored through simple regeneration treatment, reducing the cost of use.

[0028] Therefore, the present invention combines a non-metallic catalyst component of a mixture of silicon oxide and silicon carbide, a metal catalyst component of a combination of perovskite and aluminum nitrate, and a metal catalyst component of tungsten sulfide to obtain a composite catalyst with excellent desulfurization performance.

[0029] Beneficial effects of the present invention:

[0030] The present invention selects silicon oxide and silicon carbide to mix and roast at 1800°C to obtain a non-metallic catalytic component, and uses nitrogen to slowly cool it. The obtained non-metallic catalytic component has many active sites and high catalytic efficiency.

[0031] The present invention uses a low-temperature combustion method to combine perovskite and aluminum nitrate nonahydrate, and uses glycine and urea as fuel. The method has a low ignition temperature, a self-sustaining reaction, a short synthesis time, and heat release during the reaction, so that the prepared catalyst has a large specific surface area.

[0032] The present invention combines a non-metallic catalyst component of a silicon oxide and silicon carbide mixture, a metal catalyst component of a perovskite and aluminum nitrate combination, and a metal catalyst component of tungsten sulfide to obtain a composite catalyst with excellent desulfurization performance. DETAILED DESCRIPTION

[0033] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in combination with the embodiments.

[0034] Example 1

[0035] S1: Silicon carbide and silicon oxide were mixed in a molar ratio of 0.8:1, and ground in a ball mill at a speed of 300 r / min for 1 h to obtain a mixture A;

[0036] S2: Mixture A was heated from room temperature to 1800°C at 10°C / min and calcined at 1800°C for 3h. After calcination, nitrogen was evenly sprayed on the powder at a flow rate of 1m 3 / min, the pressure is 1MPa, and it is slowly cooled. After the cooling is completed, a mixture B is obtained, and the mixture B is stored under a nitrogen atmosphere;

[0037] S3: mixing glycine and urea in a mass ratio of 2:1, mixing evenly, and grinding in a ball mill at a speed of 300 r / min to obtain a mixture C;

[0038] S4: perovskite and aluminum nitrate nonahydrate were mixed in a mass ratio of 1:2, and ground in a ball mill at a speed of 300 r / min until the product was a viscous mixture to obtain a mixture D, 1 wt% of the mixture C was added to the mixture D, and ultrasonicated at 25° C. for 0.5 h, with the parameters of the ultrasonication being a frequency of 47 kHz and a power of 30 W, to obtain a mixture E;

[0039] S5: Place the mixture E in a muffle furnace preheated to 200°C, and burn for 3 minutes. After the combustion is complete, heat the mixture from the preheating temperature to 500°C at a rate of 5°C / min, and calcine at 500°C for 2 hours to obtain a mixture F.

[0040] S6: Under a nitrogen atmosphere, mixture B, mixture F and tungsten sulfide were mixed in a mass ratio of 2:2:1, and ground at 200°C at a speed of 300 r / min for 2 h. After grinding, the mixture was cooled to room temperature at a speed of 2°C / min to obtain the catalyst. The catalyst particle size obtained by grinding was 200 mesh.

[0041] The conversion rate of the catalyst prepared in this example to sulfur-containing tail gas is 99.6%.

[0042] Example 2

[0043] S1: Silicon carbide and silicon oxide were mixed in a molar ratio of 0.8:1, and ground in a ball mill at a speed of 300 r / min for 1 h to obtain a mixture A;

[0044] S2: Mixture A was heated from room temperature to 1800°C at 10°C / min and calcined at 1800°C for 3h. After calcination, nitrogen was evenly sprayed on the powder at a flow rate of 1m 3 / min, the pressure is 1MPa, and it is slowly cooled. After the cooling is completed, a mixture B is obtained, and the mixture B is stored under a nitrogen atmosphere;

[0045] S3: mixing glycine and urea in a mass ratio of 2:1, mixing evenly, and grinding in a ball mill at a speed of 300 r / min to obtain a mixture C;

[0046] S4: perovskite and aluminum nitrate nonahydrate were mixed in a mass ratio of 1:2, and ground in a ball mill at a speed of 300 r / min until the product was a viscous mixture to obtain a mixture D, 1 wt% of the mixture C was added to the mixture D, and ultrasonicated at 25° C. for 0.5 h, with the parameters of the ultrasonication being a frequency of 47 kHz and a power of 30 W, to obtain a mixture E;

[0047] S5: Place the mixture E in a muffle furnace preheated to 300°C, and burn for 1 minute. After the combustion is complete, heat the mixture from the preheating temperature to 500°C at a rate of 5°C / min, and calcine at 500°C for 2 hours to obtain a mixture F.

[0048] S6: Under a nitrogen atmosphere, mixture B, mixture F and tungsten sulfide were mixed in a mass ratio of 2:2:1, and ground at 200°C at a speed of 300 r / min for 2 h. After grinding, the mixture was cooled to room temperature at a speed of 2°C / min to obtain the catalyst. The catalyst particle size obtained by grinding was 200 mesh.

[0049] The catalyst prepared in this example has a conversion rate of 98.9% for sulfur-containing tail gas.

[0050] Example 3

[0051] S1: Silicon carbide and silicon oxide were mixed in a molar ratio of 0.8:1, and ground in a ball mill at a speed of 300 r / min for 1 h to obtain a mixture A;

[0052] S2: Mixture A was heated from room temperature to 1800°C at 10°C / min and calcined at 1800°C for 3h. After calcination, nitrogen was evenly sprayed on the powder at a flow rate of 1m 3 / min, the pressure is 1MPa, and it is slowly cooled. After the cooling is completed, a mixture B is obtained, and the mixture B is stored under a nitrogen atmosphere;

[0053] S3: mixing glycine and urea in a mass ratio of 2:1, mixing evenly, and grinding in a ball mill at a speed of 300 r / min to obtain a mixture C;

[0054] S4: perovskite and aluminum nitrate nonahydrate were mixed in a mass ratio of 1:2, and ground in a ball mill at a speed of 300 r / min until the product was a viscous mixture to obtain a mixture D, 1 wt% of the mixture C was added to the mixture D, and ultrasonicated at 25° C. for 0.5 h, with the parameters of the ultrasonication being a frequency of 47 kHz and a power of 30 W, to obtain a mixture E;

[0055] S5: Place the mixture E in a muffle furnace preheated to 300°C, and burn for 1 minute. After the combustion is complete, heat the mixture from the preheating temperature to 600°C at a rate of 5°C / min, and calcine at 600°C for 2 hours to obtain a mixture F.

[0056] S6: Under a nitrogen atmosphere, mixture B, mixture F and tungsten sulfide were mixed in a mass ratio of 2:2:1, and ground at 200°C at a speed of 300 r / min for 2 h. After grinding, the mixture was cooled to room temperature at a speed of 2°C / min to obtain the catalyst. The catalyst particle size obtained by grinding was 200 mesh.

[0057] The catalyst prepared in this example has a conversion rate of 99.3% for sulfur-containing tail gas.

[0058] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. A process for preparing a catalyst for treating sulfur-containing tail gas, It is characterized in that The specific process of catalyst preparation is as follows: S1: Silicon carbide and silicon oxide were mixed in a molar ratio of 0.8:1, and ground in a ball mill at a speed of 300 r / min for 1 h to obtain a mixture A; S2: heating the mixture A from room temperature to 1800°C, and calcining at 1800°C for 3 hours. After the calcination, nitrogen is evenly sprayed on the powder to cool it slowly. After the cooling is completed, a mixture B is obtained, and the mixture B is stored in a nitrogen atmosphere; S3: mixing glycine and urea in a mass ratio of 2:1, mixing evenly, and grinding in a ball mill at a speed of 300 r / min to obtain a mixture C; S4: perovskite and aluminum nitrate nonahydrate were mixed in a mass ratio of 1:2, and ground in a ball mill at a speed of 300 r / min until the product was a viscous mixture to obtain a mixture D, 1 wt % of the mixture C was added to the mixture D, and ultrasonicated at 25° C. for 0.5 h to obtain a mixture E; S5: placing the mixture E into a preheated muffle furnace, burning for 1-3 min, and after complete combustion, heating from the preheating temperature to 500-600° C., calcining at 500-600° C. for 2 h to obtain a mixture F; S6: Under a nitrogen atmosphere, the mixture B, the mixture F and tungsten sulfide are mixed in a mass ratio of 2:2:1, and ground at 200° C. and 300 r / min for 2 h. After the grinding, the mixture is cooled to room temperature to obtain the catalyst.

2. A process for preparing a catalyst for treating sulfur-containing tail gas according to claim 1, It is characterized in that The heating rate of the mixture A in S2 from room temperature to 1800° C. is 10° C. / min.

3. The preparation process of a catalyst for treating sulfur-containing tail gas according to claim 1, It is characterized in that The injection parameters of nitrogen in S2 are: the injection flow rate is 1m 3 / min, the pressure is 1MPa.

4. The process for preparing a catalyst for treating sulfur-containing tail gas according to claim 1, It is characterized in that The parameters of ultrasound in S4 are a frequency of 47 kHz and a power of 30 W.

5. The process for preparing a catalyst for treating sulfur-containing tail gas according to claim 1, It is characterized in that The preheating temperature in S5 is 200-300°C.

6. The process for preparing a catalyst for treating sulfur-containing tail gas according to claim 1, It is characterized in that The heating rate in S5 is 5°C / min.

7. The process for preparing a catalyst for treating sulfur-containing tail gas according to claim 1, It is characterized in that The cooling rate in S6 is 2°C / min.

8. The process for preparing a catalyst for treating sulfur-containing tail gas according to claim 1, It is characterized in that The catalyst particles obtained by grinding in S6 have a particle size of 200 meshes.