Device and method for coating ultrathin coating on surface of solid-state battery electrode
By designing a double-sided simultaneous coating device for solid-state batteries, using the combination of gravure rollers and liquid reservoirs, combined with infrared drying and flow control, the problems of uneven double-sided and uneven thickness in micro-gravure coating are solved, and the problem of uneven double-sided and uneven thickness in micro-gravure coating is achieved. Efficient and uniform ultra-thin coating, improving the quality and efficiency of the electrode surface.
Patent Information
- Application Number
- CN202411428536.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-14
- Publication Date
- 2024-12-03
AI Technical Summary
The existing microgravure coating process has problems such as uneven double-sided, uneven thickness and many baking times in the ultra-thin coating of solid-state battery electrode surfaces, resulting in problems such as wrinkling and broken belts of electrode rolls, which are difficult to achieve 2 ~10um accuracy requirements.
Design a coating device with ultra-thin coating on the surface of solid-state battery electrodes, including substrate, coating device, drying device and monitoring device, to realize double-side simultaneous coating, through the design of gravure rollers and liquid reservoirs, combined with infrared drying and flow control to ensure uniform distribution of coating liquid and thickness control.
The time saving, efficiency improvement, uniform stress distribution, and uniformity of thickness and surface density of double-sided coating are achieved, the number of baking times is reduced, the coating quality and efficiency is improved, and the impact of hot air on the coating is avoided.
Smart Images

Figure CN119056685A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of battery production and processing, and specifically relates to a coating device and method for an ultra-thin coating on the surface of a solid-state battery electrode. Background Art
[0002] In new solid-state batteries, it is often necessary to apply a second layer of ultra-thin solid electrolyte on the surface of the pole piece to replace the separator in the battery cell. The secondary coating process on the surface of the pole piece has very high requirements for the thickness of the electrolyte layer, usually 2 to 10um, and because the surface flatness of the positive and negative pole pieces is much lower than that of metal foil, the coating accuracy of the equipment is very high. Conventional transfer coating and extrusion coating are difficult to achieve an accuracy of 2 to 10um, while micro-gravure coating is suitable for ultra-thin coating.
[0003] The current mainstream micro-gravure coating process is to coat one side in sequence, that is, coat one side first and dry it before coating the other side. However, since the coating substrate is the positive and negative electrode coil, it has already undergone two baking and winding when the positive and negative electrode materials themselves are coated, resulting in the weakening of the current collector strength. Micro-gravure coating also requires two bakings, which can easily lead to problems such as wrinkling of the electrode coil, breaking of the tape, uneven coating on the front and back sides, and uneven thickness. Summary of the invention
[0004] In view of the shortcomings of the prior art, the present invention provides a coating device and method for an ultra-thin coating on the surface of a solid-state battery electrode, which can perform double-sided coating at the same time, saving time and improving coating efficiency. During double-sided coating, stress is evenly distributed, the uniformity of the coating surface is enhanced, and the coating quality is improved.
[0005] In order to achieve the above-mentioned purpose, the present invention provides a coating device for an ultra-thin coating on the surface of a solid-state battery electrode, comprising a substrate, a coating device, a drying device and a monitoring device; the substrate is placed vertically, and a current collector flows through it; a coating device, a drying device and a monitoring device are sequentially arranged on both sides of the substrate along the direction in which the current collector flows; the coating device, the drying device and the monitoring device are symmetrically arranged on both sides of the substrate, and there is a gap between the two sides of the substrate; the coating device comprises a gravure roller and a liquid storage tank; the gravure roller is rotatably and symmetrically arranged on both sides of the substrate; the outer surface of the gravure roller is connected to the lower baffle of the liquid storage tank; the coating liquid is stored in the liquid storage tank, and the outer surface of the gravure roller is in contact with the coating liquid.
[0006] A coating device for an ultra-thin coating on the surface of a solid-state battery electrode comprises a substrate, a coating device, a drying device and a monitoring device, which can coat both sides of the substrate to achieve simultaneous double-sided coating, effectively improve the coating quality and enhance the coating efficiency. The substrate is placed vertically, and the coating device, the drying device and the monitoring device are symmetrically arranged on both sides of the substrate to achieve coating on both sides of the substrate, ensure the consistency of the gravity of the coating liquid on both sides of the substrate after coating and the uniformity of the coating, and after coating, the coating liquid is dried by the drying device to form an ultra-thin coating, and then the coating thickness and surface density are monitored by the monitoring device to ensure the quality of the coating. The coating device comprises a gravure roller and a liquid storage tank, the coating liquid is stored in the liquid storage tank, the gravure roller is in full contact with the coating liquid, the coating liquid infiltrates the outer surface of the gravure roller, the gravure roller drives the coating liquid to rotate, and as the gravure roller rotates, the coating liquid is transferred to the surface of the substrate, and an ultra-thin coating is formed by the drying device to achieve the coating effect.
[0007] Furthermore, the coating device also includes a scraper; the scraper is symmetrically arranged on both sides of the substrate; the scraper is arranged above the gravure roller and there is a gap between the scraper and the outer surface of the gravure roller.
[0008] The gravure roller is in full contact with the coating liquid, and the coating liquid infiltrates the outer surface of the gravure roller. The gravure roller drives the coating liquid to rotate. When passing through the scraper, the scraper adjusts the coating liquid on the outer surface of the gravure roller to ensure the coating thickness.
[0009] Furthermore, the coating device also includes a mother liquid tank and a flow control device; the coating liquid outlet end of the mother liquid tank is connected to the coating liquid inlet end of the storage tank; the flow control device is connected in series to the connecting pipeline between the coating liquid outlet end of the mother liquid tank and the coating liquid inlet end of the storage tank.
[0010] The coating device also includes a mother liquid tank, in which the coating liquid is stored, and the coating liquid is provided to the liquid storage tank. The flow control device is used to ensure that the coating liquid pages in the liquid storage tanks on both sides of the substrate are kept at the same level.
[0011] The present invention also provides a method for coating an ultra-thin coating on the surface of a solid-state battery electrode, which is performed using the above-mentioned coating device for coating an ultra-thin coating on the surface of a solid-state battery electrode. The method comprises the following steps:
[0012] Step S1, treating the substrate so that the substrate is placed vertically;
[0013] Step S2, injecting the coating liquid into the mother liquid tank and the liquid storage tank, adjusting the liquid level in the liquid storage tank to maintain the same level through the flow control device, and adjusting the position of the liquid storage tank to ensure that the gravure roller is in full contact with the coating liquid in the liquid storage tank;
[0014] Step S3, adjusting the gap between the gravure rollers on both sides of the substrate to ensure that the substrate can be normally reeled and unreeled, adjusting the gap between the scraper and the gravure roller, and ensuring that the gap between the scraper and the gravure roller on both sides of the substrate is consistent;
[0015] Step S4, start the coating device, the drying device and the monitoring device, the gravure roller rotates, the coating liquid infiltrates the outer surface of the gravure roller, the scraper adjusts the amount of the coating liquid on the outer surface of the gravure roller so that the thickness of the coating liquid on the outer surface of the gravure roller remains unchanged, the coating liquid is transferred to the surface of the substrate to form an ultra-thin liquid film, the ultra-thin liquid film passes through the drying device, and the solvent evaporates quickly to form an ultra-thin coating; and then the ultra-thin coating is monitored by the monitoring system.
[0016] Furthermore, in step S1, the substrate is selected from a positive electrode roll or a negative electrode roll; and the thickness of the substrate is 150 to 400 um.
[0017] Furthermore, in step S3, the gap between the gravure rollers on both sides of the substrate is adjusted, and the difference between the gravure gap on both sides of the substrate and the thickness of the substrate is 0 to 200 um.
[0018] Furthermore, in step S3, the gap between the scraper and the gravure roller is adjusted, and the gap between the scraper and the gravure roller is 0 to 100 um.
[0019] Furthermore, in step S4, the drying device is infrared drying.
[0020] Further, in step S4, the monitoring system is an area density measurement system; the area density measurement system is selected from a β-ray area density measuring instrument or an X-ray area density measuring instrument.
[0021] Furthermore, in step S4, the thickness of the coating liquid on the outer surface of the gravure roller remains unchanged, and the thickness of the coating liquid is 0 to 100 um.
[0022] Beneficial Effects
[0023] The coating device and method for the ultra-thin coating on the surface of the solid-state battery electrode provided by the present invention have the following beneficial effects:
[0024] 1. The coating device and method of the present invention can simultaneously apply ultra-thin coatings on both sides, which saves coating time and improves coating efficiency compared to sequential single-sided coating;
[0025] 2. The coating device and method of the present invention can coat both sides simultaneously, and the front and back sides are symmetrical, resulting in uniform stress distribution on the front and back sides, thereby effectively improving the coating quality;
[0026] 3. After single-sided coating, the electrode material needs to be baked twice; however, the coating device and method of the present invention only needs to be baked once for double-sided coating, which greatly saves energy consumption;
[0027] 4. The coating device and method of the present invention can better control the coating thickness deviation and surface density deviation on the front and back sides, and improve the overall uniformity;
[0028] 5. The drying system used in the coating device and method of the present invention is infrared drying rather than hot air drying, which avoids the influence of hot air fluid on the surface quality of the coating during the drying process and improves the uniformity of the coating surface. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is a schematic diagram of the structure of a coating device for an ultra-thin coating on the surface of a solid-state battery electrode;
[0030] Figure 2 It is a schematic diagram of solvent volatilization and tension distribution when single-sided coating is performed using a common gravure coating process;
[0031] Figure 3 A schematic diagram of solvent evaporation and tension distribution when a coating method for an ultra-thin coating on the surface of a solid-state battery electrode is used for simultaneous double-sided coating.
[0032] In the attached drawings: 1. substrate; 2. coating device; 3. drying device; 4. monitoring device; 21. gravure roller; 22. liquid storage tank; 23. scraper; 24. mother liquid tank; 25. flow control device. DETAILED DESCRIPTION
[0033] Example 1
[0034] like Figure 1 A coating device for an ultra-thin coating on the surface of a solid-state battery electrode is shown, comprising a substrate 1, a coating device 2, a drying device 3 and a monitoring device 4; the substrate 1 is placed vertically, and a current collector flows through it; the coating device 2, the drying device 3 and the monitoring device 4 are sequentially arranged on both sides of the substrate 1 along the direction in which the current collector flows; the coating device 2, the drying device 3 and the monitoring device 4 are symmetrically arranged on both sides of the substrate 1, with gaps between the two sides of the substrate 1; the coating device 2 comprises a gravure roller 21 and a liquid storage tank 22; the gravure roller 21 is rotatably and symmetrically arranged on both sides of the substrate 1; the lower baffle of the liquid storage tank 22 is made of rubber material, and the outer surface of the gravure roller 21 is connected to the lower baffle of the liquid storage tank 22; the coating liquid is stored in the liquid storage tank 22, and the outer surface of the gravure roller 21 is in contact with the coating liquid.
[0035] A coating device for an ultra-thin coating on the surface of a solid-state battery electrode includes a substrate 1, a coating device 2, a drying device 3, and a monitoring device 4. The coating can be applied to both sides of the substrate 1 to achieve simultaneous double-sided coating, effectively improving the coating quality and the coating efficiency. The substrate 1 is placed vertically, and the coating device 2, the drying device 3, and the monitoring device 4 are symmetrically arranged on both sides of the substrate 1 to achieve double-sided coating of the substrate 1, ensuring that the gravity of the coating liquid on both sides of the substrate 1 is consistent and the coating is uniform after coating. After coating, the coating liquid is dried by the drying device 3 to form an ultra-thin coating, and then the coating thickness and surface density are monitored by the monitoring device 4 to ensure the quality of the coating. The coating device 2 includes a gravure roller 21 and a liquid storage tank 22. The liquid storage tank 22 stores the coating liquid. The gravure roller 21 is in full contact with the coating liquid. The lower baffle of the liquid storage tank 22 is made of a flexible rubber material. The outer surface of the gravure roller 21 is connected to the lower baffle of the liquid storage tank 22. The two are in direct contact. The lower baffle of the liquid storage tank 22 will not affect the rotation of the gravure roller 21. The coating liquid infiltrates the outer surface of the gravure roller 21, and the gravure roller 21 drives the coating liquid to rotate. As the gravure roller 21 rotates, the coating liquid is transferred to the surface of the substrate 1, and an ultra-thin coating is formed through the drying device 3 to achieve a coating effect.
[0036] The coating device 2 further includes a scraper 23 ; the scraper 23 is symmetrically arranged on both sides of the substrate 1 ; the scraper 23 is arranged above the gravure roller 21 , and there is a gap between the scraper 23 and the outer surface of the gravure roller 21 .
[0037] The gravure roller 21 is in full contact with the coating liquid, and the coating liquid infiltrates the outer surface of the gravure roller 21. The gravure roller 21 drives the coating liquid to rotate. When passing through the scraper 23, the scraper 23 adjusts the coating liquid on the outer surface of the gravure roller 21 to ensure the coating thickness.
[0038] The coating device 2 also includes a mother liquid tank 24 and a flow control device 25; the coating liquid outlet end of the mother liquid tank 24 is connected to the coating liquid inlet end of the liquid storage tank 22; the flow control device 25 is connected in series to the connecting pipeline between the coating liquid outlet end of the mother liquid tank 24 and the coating liquid inlet end of the liquid storage tank 22.
[0039] The coating device 2 further comprises a mother liquid tank 24, in which the coating liquid is stored, and provides the coating liquid to the liquid storage tank 22. The flow control device 25 is used to ensure that the coating liquid pages in the liquid storage tanks 22 on both sides of the substrate 1 are kept at the same level.
[0040] Example 2
[0041] A method for coating an ultra-thin coating on the surface of a solid-state battery electrode comprises the following steps:
[0042] Step S1, the positive electrode roll is placed by the winding and unwinding system, the positive electrode roll is placed vertically, and the thickness of the positive electrode roll is 160 um;
[0043] Step S2, injecting a coating liquid into the mother liquid tank and the liquid storage tank, wherein the coating liquid is 20% LATP-2% PVDF-NMP slurry with a viscosity of 260-300 mPs, adjusting the liquid level in the liquid storage tank to maintain the same horizontal plane through a flow control device, and adjusting the position of the liquid storage tank to ensure that the gravure roller is in full contact with the coating liquid in the liquid storage tank;
[0044] Step S3, adjusting the gap between the gravure rollers on both sides of the positive electrode roll to 240 μm to ensure that the positive electrode roll can be normally reeled and unreeled, adjusting the gap between the scraper and the gravure roller, and ensuring that the gap between the scraper and the gravure roller on both sides of the positive electrode roll is consistent;
[0045] Step S4, start the coating device, the drying device and the monitoring device, the gravure roller rotates, the belt speed of the gravure roller is 5m / min, the roller speed ratio is 1.5, the coating liquid infiltrates the outer surface of the gravure roller, the scraper adjusts the amount of coating liquid on the outer surface of the gravure roller so that the thickness of the coating liquid on the outer surface of the gravure roller remains unchanged, the coating liquid is transferred to the surface of the positive electrode coil to form an ultra-thin liquid film, the ultra-thin liquid film is infrared dried at 80°C, and the ultra-thin coating is formed after the solvent evaporates quickly; then the thickness of the ultra-thin coating at 20 random positions on both sides of the positive electrode coil is monitored by the monitoring system.
[0046] Example 3
[0047] A method for coating an ultra-thin coating on the surface of a solid-state battery electrode comprises the following steps:
[0048] Step S1, the positive electrode roll is placed by the winding and unwinding system, the positive electrode roll is placed vertically, and the thickness of the positive electrode roll is 160 um;
[0049] Step S2, injecting a coating liquid into the mother liquid tank and the liquid storage tank, wherein the coating liquid is 30% LATP-5% PVDF-NMP slurry with a viscosity of 660-900 mPs, adjusting the liquid level in the liquid storage tank to maintain the same horizontal plane through a flow control device, and adjusting the position of the liquid storage tank to ensure that the gravure roller is in full contact with the coating liquid in the liquid storage tank;
[0050] Step S3, adjusting the gap between the gravure rollers on both sides of the positive electrode roll to ensure that the positive electrode roll can be normally retracted and unreeled, adjusting the gap between the scraper and the gravure roller, and ensuring that the gap between the scraper and the gravure roller on both sides of the positive electrode roll is consistent;
[0051] Step S4, start the coating device, the drying device and the monitoring device, the gravure roller rotates, the belt speed of the gravure roller is 5m / min, the roller speed ratio is 1.5, the coating liquid infiltrates the outer surface of the gravure roller, the scraper adjusts the amount of coating liquid on the outer surface of the gravure roller so that the coating liquid thickness on the outer surface of the gravure roller remains unchanged, the coating liquid is transferred to the surface of the positive electrode roll to form an ultra-thin liquid film, the ultra-thin liquid film is infrared dried, and the solvent evaporates quickly to form an ultra-thin coating; then the surface coating density of the ultra-thin coating at 16 random positions on both sides of the positive electrode roll is monitored by the monitoring system.
[0052] Example 4
[0053] A method for coating an ultra-thin coating on the surface of a solid-state battery electrode comprises the following steps:
[0054] Step S1, the positive electrode roll is placed by the winding and unwinding system, the positive electrode roll is placed vertically, the thickness of the positive electrode roll is 160um, and the length is 500m;
[0055] Step S2, injecting a coating liquid into the mother liquid tank and the liquid storage tank, wherein the coating liquid is 20% LATP-2% PVDF-NMP slurry with a viscosity of 260-300 mPs, adjusting the liquid level in the liquid storage tank to maintain the same horizontal plane through a flow control device, and adjusting the position of the liquid storage tank to ensure that the gravure roller is in full contact with the coating liquid in the liquid storage tank;
[0056] Step S3, adjusting the gap between the gravure rollers on both sides of the positive electrode roll to ensure that the positive electrode roll can be normally retracted and unreeled, adjusting the gap between the scraper and the gravure roller, and ensuring that the gap between the scraper and the gravure roller on both sides of the positive electrode roll is consistent;
[0057] Step S4, start the coating device, the drying device and the monitoring device, the gravure roller rotates, the belt speed of the gravure roller is 5m / min, the roller speed ratio is 1.5, the coating liquid infiltrates the outer surface of the gravure roller, the scraper adjusts the amount of coating liquid on the outer surface of the gravure roller so that the coating liquid thickness on the outer surface of the gravure roller remains unchanged, the coating liquid is transferred to the surface of the positive electrode roll to form an ultra-thin liquid film, the ultra-thin liquid film is infrared dried, and the solvent evaporates quickly to form an ultra-thin coating; then the ultra-thin coating is monitored by the monitoring system.
[0058] Comparative Example 1
[0059] A coating method of a common gravure coating process comprises the following steps:
[0060] Step S1, the positive electrode roll is placed by the winding and unwinding system, and the thickness of the positive electrode roll is 160um;
[0061] Step S2, injecting a coating liquid into the liquid reservoir, wherein the coating liquid is 20% LATP-2% PVDF-NMP slurry with a viscosity of 260-300 mPs, and adjusting the position of the liquid reservoir to ensure that the gravure roller is in full contact with the coating liquid in the liquid reservoir;
[0062] Step S3, adjusting the gap between the scraper and the gravure roller;
[0063] Step S4, start the coating device and the drying device, the gravure roller rotates, the belt speed of the gravure roller is 5m / min, the roller speed ratio is 1.5, the coating liquid infiltrates the outer surface of the gravure roller, the scraper adjusts the amount of coating liquid on the outer surface of the gravure roller, and the coating liquid is transferred to one side of the positive electrode roll to form an ultra-thin liquid film. The ultra-thin liquid film is dried by hot air at 80°C, and the ultra-thin coating is formed after the solvent evaporates quickly; then the other side of the positive electrode roll is coated and dried; after the coating is completed, the thickness of the ultra-thin coating at 20 random positions on one side of the positive electrode roll is monitored by the monitoring system.
[0064] Comparative Example 2
[0065] A coating method of a common gravure coating process comprises the following steps:
[0066] Step S1, the positive electrode roll is placed by the winding and unwinding system, and the thickness of the positive electrode roll is 160um;
[0067] Step S2, injecting a coating liquid into the liquid reservoir, wherein the coating liquid is 30% LATP-5% PVDF-NMP slurry with a viscosity of 660-900 mPs, and adjusting the position of the liquid reservoir to ensure that the gravure roller is in full contact with the coating liquid in the liquid reservoir;
[0068] Step S3, adjusting the gap between the scraper and the gravure roller;
[0069] Step S4, start the coating device and the drying device, the gravure roller rotates, the belt speed of the gravure roller is 5m / min, the roller speed ratio is 1.5, the coating liquid infiltrates the outer surface of the gravure roller, the scraper adjusts the amount of coating liquid on the outer surface of the gravure roller, and the coating liquid is transferred to one side of the positive electrode roll to form an ultra-thin liquid film. The ultra-thin liquid film is dried with hot air at 80°C, and the ultra-thin coating is formed after the solvent evaporates quickly; then the other side of the positive electrode roll is coated and dried; after the coating is completed, the surface coating density of the ultra-thin coating at 16 random positions on one side of the positive electrode roll is monitored by the monitoring system.
[0070] Comparative Example 3
[0071] A coating method of a common gravure coating process comprises the following steps:
[0072] Step S1, the positive electrode roll is placed by the winding and unwinding system, the thickness of the positive electrode roll is 160um and the length is 500m;
[0073] Step S2, injecting a coating liquid into the liquid reservoir, wherein the coating liquid is 20% LATP-2% PVDF-NMP slurry with a viscosity of 260-300 mPs, and adjusting the position of the liquid reservoir to ensure that the gravure roller is in full contact with the coating liquid in the liquid reservoir;
[0074] Step S3, adjusting the gap between the scraper and the gravure roller;
[0075] Step S4, start the coating device and the drying device, the gravure roller rotates, the belt speed of the gravure roller is 5m / min, the roller speed ratio is 1.5, the coating liquid infiltrates the outer surface of the gravure roller, the scraper adjusts the amount of coating liquid on the outer surface of the gravure roller, the coating liquid is transferred to one side of the positive electrode roll to form an ultra-thin liquid film, the ultra-thin liquid film is dried at 80°C hot air, and the ultra-thin coating is formed after the solvent evaporates quickly; then the other side of the positive electrode roll is coated and dried; after coating is completed, the ultra-thin coating is monitored by the monitoring system.
[0076] Ultra-thin coating thickness analysis
[0077] Table 1 shows the thickness data of the ultra-thin coating obtained by the coating methods of Example 2 and Comparative Example 1. The coating thickness data of 20 random positions in the ultra-thin coating obtained by the coating method of Example 2 are 5, 7, 5, 6, 5, 6, 7, 5, 6, 5, 6, 7, 6, 7, 6, 5, 6, 7um, and the thickness distribution is between 5 and 7um; while the coating thickness data of 20 random positions on one side of the ultra-thin coating obtained by the coating method of Comparative Example 1 are 5, 7, 8, 6, 5, 6, 7, 6, 7, 5, 7, 8, 6, 6, 4, 4, 5, 7, 5, 4um, and the thickness distribution is between 4 and 8um. Compared with Comparative Example 1, the coating thickness distribution of Example 2 is more concentrated and the variance is smaller. Therefore, the double-sided coating method of Example 2 has a more uniform thickness and a more concentrated thickness distribution, which improves the coating quality.
[0078] Table 1 Thickness data of ultra-thin coatings
[0079] Sample No. #1 #2 #3 #4 #5 #6 #7 #8 Example 2 5 7 5 6 5 6 5 6 Comparative Example 1 5 7 8 6 5 6 7 6 Sample No. #9 #10 #11 #12 #13 #14 #15 #16 Example 2 7 5 6 5 6 7 6 7 Comparative Example 1 7 5 7 8 6 6 4 4 Sample No. #17 #18 #19 #20 Minimum Maximum variance Example 2 6 5 6 7 5 7 0.621 Comparative Example 1 5 7 5 4 4 8 1.568
[0080] Surface coating density analysis
[0081] Table 2 shows the surface coating density data of the ultra-thin coating obtained by the coating method of Example 3 and Comparative Example 2. The surface coating density data of 16 random positions in the ultra-thin coating obtained by the coating method of Example 3 are 1.36, 1.52, 1.47, 1.56, 1.46, 1.56, 1.49, 1.56, 1.55, 1.58, 1.53, 1.54, 1.60, 1.52, 1.47, 1.38 mg / cm 2Surface coating density distribution 1.36~1.60mg / cm 2 The surface coating density data of 16 random positions on one side of the ultra-thin coating obtained by the coating method of Comparative Example 2 are 1.21, 1.12, 1.46, 1.58, 1.33, 1.68, 1.28, 1.10, 1.38, 1.56, 1.65, 1.58, 1.68, 1.56, 1.64, 1.62 mg / cm 2 Surface coating density distribution 1.12~1.68mg / cm 2 Compared with Comparative Example 2, the surface coating density distribution of the double-sided coating method of Example 3 is more concentrated, the variance is smaller, and the coating quality is improved.
[0082] Table 2 Surface coating density data of ultra-thin coating
[0083] Sample No. #1 #2 #3 #4 #5 #6 #7 Example 3 1.36 1.52 1.47 1.56 1.46 1.56 1.49 Comparative Example 2 1.21 1.12 1.46 1.58 1.33 1.68 1.28 Sample No. #8 #9 #10 #11 #12 #13 #14 Example 3 1.56 1.55 1.58 1.53 1.54 1.6 1.52 Comparative Example 2 1.1 1.38 1.56 1.65 1.58 1.68 1.56 Sample No. #15 #16 Minimum Maximum variance Example 3 1.47 1.38 1.36 1.6 0.005 Comparative Example 2 1.64 1.62 1.1 1.68 0.040
[0084] Coating yield analysis
[0085] Table 3 shows the coating yield data of the ultra-thin coating obtained by the coating methods of Example 4 and Comparative Example 3. In Example 4, after deducting the debugging time, the coating took a total of 80 minutes, and the coating yield was 78% after deducting the debugging loss; in Comparative Example 3, after deducting the debugging time, the coating took a total of 180 minutes, and the coating yield was 62% after deducting the debugging loss. Compared with Comparative Example 3, the double-sided coating method of Example 4 takes less time, is conducive to saving energy consumption, and improves the coating yield.
[0086] Table 3 Coating yield data
[0087]
[0088] Coating Stress Analysis
[0089] Figure 2 This is a schematic diagram of solvent volatilization and tension distribution when single-sided coating is performed using a common gravure coating process; Figure 3 The diagram is a schematic diagram of solvent evaporation and tension distribution when a coating method for an ultra-thin coating on the surface of a solid-state battery electrode is used for simultaneous double-sided coating.
[0090] The coating substrate is the positive and negative electrodes, and the electrodes are porous structures at the microscopic level. Therefore, when the coating liquid is transferred to the electrode surface, the solvent will quickly penetrate into the electrode under the action of the capillary pores. When passing through the drying system, the solvent will quickly evaporate and dry. Figure 2 As shown in the figure, when the method of sequential single-sided coating is adopted, the solvent can easily cause uneven stress on the front and back sides of the electrode during penetration and rapid evaporation, especially in the blank area of the electrode or the junction of the material area, which can easily cause problems such as electrode roll wrinkles or even broken tape. Figure 3 As shown, when a coating method for an ultra-thin coating on the surface of a solid-state battery electrode is used for double-sided coating at the same time, since both sides are coated at the same time and the front and back sides are symmetrical, the stress on the front and back sides is also evenly distributed, thereby effectively improving the coating quality.
Claims
1. A coating device for an ultra-thin coating on the surface of a solid-state battery electrode, characterized in that: The invention comprises a substrate (1), a coating device (2), a drying device (3) and a monitoring device (4); the substrate (1) is placed vertically and a current collector flows through it; the coating device (2), the drying device (3) and the monitoring device (4) are arranged in sequence on both sides of the substrate (1) along the direction in which the current collector flows; the coating device (2), the drying device (3) and the monitoring device (4) are symmetrically arranged on both sides of the substrate (1) and there is a gap between the two sides of the substrate (1); the coating device (2) comprises a gravure roller (21) and a liquid storage tank (22); the gravure roller (21) is rotatably symmetrically arranged on both sides of the substrate (1); the outer surface of the gravure roller (21) is connected to the lower baffle of the liquid storage tank (22); the liquid storage tank (22) stores a coating liquid, and the outer surface of the gravure roller (21) is in contact with the coating liquid.
2. The coating device for an ultra-thin coating on the surface of a solid-state battery electrode according to claim 1, characterized in that: The coating device (2) further comprises a scraper (23); the scraper (23) is symmetrically arranged on both sides of the substrate (1); the scraper (23) is arranged above the gravure roller (21) and there is a gap between the scraper (23) and the outer surface of the gravure roller (21).
3. The coating device for an ultra-thin coating on the surface of a solid-state battery electrode according to claim 2, characterized in that: The coating device (2) further comprises a mother liquid tank (24) and a flow control device (25); the coating liquid outlet end of the mother liquid tank (24) is connected to the coating liquid inlet end of the liquid storage tank (22); and the flow control device (25) is connected in series to the connecting pipeline between the coating liquid outlet end of the mother liquid tank (24) and the coating liquid inlet end of the liquid storage tank (22).
4. A method for coating an ultra-thin coating on the surface of a solid-state battery electrode, characterized in that: The coating is carried out according to the coating device for an ultra-thin coating on the surface of a solid-state battery electrode according to claim 3, wherein the method comprises the following steps: Step S1, treating the substrate so that the substrate is placed vertically; Step S2, injecting the coating liquid into the mother liquid tank and the liquid storage tank, adjusting the liquid level in the liquid storage tank to maintain the same level through the flow control device, and adjusting the position of the liquid storage tank to ensure that the gravure roller is in full contact with the coating liquid in the liquid storage tank; Step S3, adjusting the gap between the gravure rollers on both sides of the substrate to ensure that the substrate can be normally reeled and unreeled, adjusting the gap between the scraper and the gravure roller, and ensuring that the gap between the scraper and the gravure roller on both sides of the substrate is consistent; Step S4, start the coating device, the drying device and the monitoring device, the gravure roller rotates, the coating liquid infiltrates the outer surface of the gravure roller, the scraper adjusts the amount of the coating liquid on the outer surface of the gravure roller so that the thickness of the coating liquid on the outer surface of the gravure roller remains unchanged, the coating liquid is transferred to the surface of the substrate to form an ultra-thin liquid film, the ultra-thin liquid film passes through the drying device, and the solvent evaporates quickly to form an ultra-thin coating; and then the ultra-thin coating is monitored by the monitoring system.
5. The method for coating an ultra-thin coating on the surface of a solid-state battery electrode according to claim 4, characterized in that: In step S1, the substrate is selected from a positive electrode roll or a negative electrode roll; the thickness of the substrate is 150-400 um.
6. The method for coating an ultra-thin coating on the surface of a solid-state battery electrode according to claim 4, characterized in that: In step S3, the gap between the gravure rollers on both sides of the substrate is adjusted, and the difference between the gravure gap on both sides of the substrate and the thickness of the substrate is 0-200 um.
7. The method for coating an ultra-thin coating on the surface of a solid-state battery electrode according to claim 4, characterized in that: In step S3, the gap between the scraper and the gravure roller is adjusted, and the gap between the scraper and the gravure roller is 0-100 um.
8. The method for coating an ultra-thin coating on the surface of a solid-state battery electrode according to claim 4, characterized in that: In step S4, the drying device is infrared drying.
9. The method for coating an ultra-thin coating on the surface of a solid-state battery electrode according to claim 4, characterized in that: In step S4, the monitoring system is an area density measurement system; the area density measurement system is selected from a β-ray area density measurement instrument or an X-ray area density measurement instrument.
10. The method for coating an ultra-thin coating on the surface of a solid-state battery electrode according to claim 4, characterized in that: In step S4, the coating liquid thickness on the outer surface of the gravure roller remains unchanged, and the coating liquid thickness is 0-100 um.
Citation Information
Patent Citations
Thin electrode double-sided coating device and method for lithium ion battery
CN112808515A
Lithium battery pole piece double-sided coating equipment and method
CN114985217A
Double-sided coating device for lithium ion battery
CN216225137U
Double-channel coating device
CN221515041U
Coating device
JP2009178697A