Medium carbon steel composite board with high interface bonding rate and preparation method thereof

Through the preparation method of single-pass rolling medium-carbon steel composite plates in a vacuum environment, the problems of unsatisfactory interface bonding rate and complex process are solved, and high-efficiency and low-cost medium-carbon steel composite plates are achieved. The interface combination is carried out. The rate reaches more than 96%.

CN119056875AActive Publication Date: 2024-12-03KUNMING UNIV OF SCI & TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411563667.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-05
Publication Date
2024-12-03
Estimated Expiration
2044-11-05

AI Technical Summary

Technical Problem

The interface bonding rate of existing medium-carbon steel composite panels is not ideal, the process is complex, the production efficiency is low, and it requires multiple rolling, which is difficult to control.

Method used

A high interfacial bonding rate medium carbon steel composite plate preparation method, including material preparation, cleaning, pretreatment, rolling and cooling steps, by performing single-pass rolling in a vacuum environment, the rolling temperature is 1100℃-1200 ℃, the pressure rate is 16%-22%, cooled to room temperature, simplifying the process flow and improving efficiency.

Benefits of technology

The interface bonding rate is achieved with a simple and easy to control process, a short processing cycle and low cost, reducing rolling passes, simplifying the process flow, and improving production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119056875A_ABST
    Figure CN119056875A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a medium carbon steel composite plate with a high interface bonding rate, and belongs to the technical field of metal composite plate manufacturing, a medium carbon steel billet plate is heated to 1100-1300 DEG C, heat preservation is carried out for at least 5 min, then single-pass rolling is carried out, the rolling temperature is 1100-1200 DEG C, and the reduction rate is 16%-22%. The method has the advantages that the interface bonding rate of the prepared medium carbon steel composite plate is larger than 96%, the process is simple, control is easy, the machining period is short, and the machining cost is low.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal composite plate manufacturing, and in particular to a medium carbon steel composite plate with high interface bonding rate and a preparation method thereof. Background Art

[0002] Layered metal composite plate is a composite material composed of two or more layers of metal plates with different properties that are processed by special technology to achieve a strong metallurgical bond at the interface. Metal composite plates can be divided into heterogeneous metal composite plates and homogeneous metal composite plates. With the continuous improvement of equipment size and safety requirements, there is a strong demand for homogeneous metal composite plates in the manufacturing of heavy equipment such as ship decks, armored vehicle shells, large hydropower station gates, offshore oil platforms, and nuclear power plant nuclear reactor shells. Medium-carbon high-quality carbon structural steel has excellent comprehensive mechanical properties, such as high strength, plasticity and toughness, and good cutting performance. It has now been used by many domestic and foreign companies as blanks for the production of stainless steel composite plates, titanium / steel composite plates, and extra-thick composite steel plates.

[0003] In recent years, the production of extra-thick composite steel plates is mainly carried out by vacuum hot rolling composite method, that is, ordinary continuous casting billets are combined by vacuum electron beam welding to form composite continuous casting billets and then hot rolled. The currently public data use different rolling processes and different heat treatment processes for different materials, and the performance of the obtained products varies greatly. The interface bonding rate of the products of some processes is not ideal, and some processes require multiple rolling, which is complicated, difficult to control, and has low production efficiency.

[0004] Therefore, developing a medium carbon steel composite plate with high interface bonding rate, simple process and easy control and a preparation method thereof have application prospects. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a method for preparing a medium carbon steel composite plate with a high interface bonding rate. The process flow is simple, easy to control, and the processing cycle is short. The interface bonding rate of the prepared medium carbon steel composite plate is higher than 96%.

[0006] In order to solve the above technical problems, the technical solution of the present invention is a method for preparing a medium carbon steel composite plate with a high interface bonding rate, comprising the following steps: S1. Material preparation: prepare two medium carbon steel slabs; S2. Cleaning: Clean the bonding interface of the medium carbon steel slab to remove oil stains and oxides; S3. Pretreatment: align the bonding interface of the medium carbon steel slab, heat it to 1100℃-1300℃, and keep it warm for at least 5 minutes; S4, rolling: placing the double-layer medium carbon steel slab in a vacuum environment for single-pass rolling, the rolling temperature is 1100℃-1200℃, and the reduction rate is 16%-22%; S5. Cooling: Cool to room temperature.

[0007] Furthermore, in the S3, pretreatment step, the temperature is heated to 1200° C., and the heating rate during the heating process is not higher than 2° C. / s.

[0008] Furthermore, the temperature is kept constant during the S4, rolling step.

[0009] Furthermore, the strain rate in the S4 rolling step is 0.01s -1 -0.05s -1 .

[0010] Furthermore, the vacuum degree in the S4 rolling step is not higher than 5×10 -2 Pa.

[0011] Furthermore, the interface bonding surface roughness in the cleaning step S2 is required to be less than or equal to 1.6 m.

[0012] Furthermore, the cooling method in the cooling step S5 is air cooling.

[0013] Furthermore, the material of the medium carbon steel slab in the material preparation step S1 is medium carbon high-quality carbon structural steel.

[0014] The present invention also provides a medium carbon steel composite plate prepared by the above preparation method.

[0015] Beneficial effects of the present invention: The present invention does not require vacuum electron beam welding for assembling, but only requires vacuuming during the rolling process; it only requires single-pass rolling, which greatly reduces the number of rolling passes compared to the existing process, simplifies the process flow, and improves the composite efficiency. The entire operation process is easy to control, the process is simple, the processing cycle is short, and the processing cost is low; the medium carbon steel composite plate can be prepared within a relatively small reduction rate of 16%-22%, and the interface bonding rate is higher than 96%. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 The metallographic image of the composite interface of the medium carbon steel composite plate prepared in Example 1; Figure 2 This is a metallographic image of the composite interface of the medium carbon steel composite plate prepared in Example 2; Figure 3 This is a metallographic image of the composite interface of the medium carbon steel composite plate prepared in Example 3; Figure 4 This is a metallographic image of the composite interface of the medium carbon steel composite plate prepared in Example 4; Figure 5This is a metallographic image of the composite interface of the medium carbon steel composite plate prepared in Example 5; Figure 6 This is a metallographic image of the composite interface of the medium carbon steel composite plate prepared in Example 6; Figure 7 This is a metallographic image of the composite interface of the medium carbon steel composite plate prepared in Example 7; Figure 8 This is a metallographic image of the composite interface of the medium carbon steel composite plate prepared in Example 8; Fig. 9 This is a metallographic image of the composite interface of the medium carbon steel composite plate prepared in Comparative Example 1; Fig.10 This is a metallographic image of the composite interface of the medium carbon steel composite plate prepared in Comparative Example 2. DETAILED DESCRIPTION

[0017] The specific embodiments of the present invention are further described below in conjunction with the accompanying drawings. It should be noted that the description of these embodiments is used to help understand the present invention, but does not constitute a limitation of the present invention. In addition, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0018] Example 1 A method for preparing a medium carbon steel composite plate with a high interface bonding rate comprises the following steps: S1. Material preparation: prepare two medium carbon steel slabs; the material of the medium carbon steel slabs is medium carbon high-quality carbon structural steel; S2. Cleaning: Clean the interface bonding surface of the medium carbon steel slab to remove oil stains and oxides. The surface roughness of the bonding interface is required to be less than or equal to 1.6 m; S3. Pretreatment: Align the bonding surface of the medium carbon steel billet and heat it to 1200℃, with a heating rate of no more than 2℃ / s, and keep it warm for 5 minutes; S4, rolling: immediately place the double-layer medium carbon steel billet in a vacuum environment for single-pass rolling, with a vacuum degree not higher than 5×10 -2 Pa, the rolling temperature is 1200℃, the temperature is kept constant during the rolling process, the reduction rate is 16%, and the strain rate is 0.01s -1 Keeping the temperature constant during rolling can avoid the temperature gradient caused by a sharp drop in temperature, thereby reducing the impact of temperature difference on the composite effect; S5. Cooling: air cool to room temperature.

[0019] In this embodiment, the initial thickness of the medium carbon steel double-layer billet is 10 mm, and the thickness of the medium carbon steel composite plate prepared after rolling is 8.4 mm. The bonding interface of the prepared medium carbon steel composite plate was observed microscopically, and the results are as follows: Figure 1 As shown, there is no obvious composite interface and holes, and the grains at the interface have been recrystallized into complete and continuous grains shared by the two billets. According to statistics and calculations, the number of holes in the entire composite interface is 2, the average hole size is 8.7, and the bonding rate is 99.7%, indicating a good composite effect.

[0020] Example 2 A method for preparing a medium carbon steel composite plate with a high interface bonding rate comprises the following steps: S1. Material preparation: prepare two medium carbon steel billets; the material of the medium carbon steel billets is medium carbon high-quality carbon structural steel; S2. Cleaning: Clean the interface bonding surface of the medium carbon steel billet to remove oil stains and oxides. The surface roughness of the bonding interface is required to be less than or equal to 1.6 m; S3. Pretreatment: Align the bonding surface of the medium carbon steel billet and heat it to 1200℃, with a heating rate of no more than 2℃ / s, and keep it warm for 5 minutes; S4, rolling: take out the double-layer medium carbon steel billet and place it in a vacuum environment for single-pass rolling. The vacuum degree is not higher than 5×10 -2 Pa, the rolling temperature was controlled at 1150 °C, the temperature was kept constant during the rolling process, the reduction rate was 16%, and the strain rate was 0.05 s -1 ; S5. Cooling: air cool to room temperature.

[0021] In this embodiment, the initial thickness of the medium carbon steel double-layer billet is 10 mm, and the thickness of the medium carbon steel composite plate prepared after rolling is 8.4 mm. The bonding interface of the prepared medium carbon steel composite plate was observed microscopically, and the results are as follows: Figure 2 As shown in the figure, there is no obvious composite interface and pores. The grains at the interface have been recrystallized into complete and continuous grains shared by the two billets. According to statistics and calculations, the number of pores in the entire composite interface is 31, and the average pore size is 6.7 m, the binding rate is 96.2%, indicating that the composite effect is good.

[0022] Example 3 A method for preparing a medium carbon steel composite plate with a high interface bonding rate comprises the following steps: S1. Material preparation: prepare two medium carbon steel billets; the material of the medium carbon steel billets is medium carbon high-quality carbon structural steel; S2. Cleaning: Clean the interface bonding surface of the medium carbon steel billet to remove oil stains and oxides. The surface roughness of the bonding interface is required to be less than or equal to 1.6 m; S3. Pretreatment: Align the bonding surface of the medium carbon steel billet and heat it to 1200℃, with a heating rate of no more than 2℃ / s, and keep it warm for 5 minutes; S4, rolling: take out the double-layer medium carbon steel billet and place it in a vacuum environment for single-pass rolling. The vacuum degree is not higher than 5×10 -2 Pa, the rolling temperature is 1100℃, the temperature is kept constant during the rolling process, the reduction rate is 16%, and the strain rate is 0.02s -1 ; S5. Cooling: air cool to room temperature.

[0023] In this embodiment, the initial thickness of the medium carbon steel double-layer billet is 10 mm, and the thickness of the medium carbon steel composite plate prepared after rolling is 8.4 mm. The bonding interface of the prepared medium carbon steel composite plate was observed microscopically, and the results are as follows: Figure 3 As shown in the figure, there is no obvious composite interface and pores. The grains at the interface have been recrystallized into complete and continuous grains shared by the two billets. According to statistics and calculations, the number of pores in the entire composite interface is 12, and the average pore size is 6.7 m, the binding rate is 98.5%, indicating that the composite effect is good.

[0024] Example 4 A method for preparing a medium carbon steel composite plate with a high interface bonding rate comprises the following steps: S1. Material preparation: prepare two medium carbon steel billets; the material of the medium carbon steel billets is medium carbon high-quality carbon structural steel; S2. Cleaning: Clean the interface bonding surface of the medium carbon steel billet to remove oil stains and oxides. The surface roughness of the bonding interface is required to be less than or equal to 1.6 m; S3. Pretreatment: Align the bonding surface of the medium carbon steel billet and heat it to 1200℃, with a heating rate of no more than 2℃ / s, and keep it warm for 5 minutes; S4, rolling: take out the double-layer medium carbon steel billet and immediately place it in a vacuum environment for single-pass rolling. The vacuum degree is not higher than 5×10 -2 Pa, the rolling temperature is 1200℃, the temperature is kept constant during the rolling process, the reduction rate is 22%, and the strain rate is 0.05s -1 ; S5. Cooling: air cool to room temperature.

[0025] In this embodiment, the initial thickness of the medium carbon steel double-layer billet is 10 mm, and the thickness of the medium carbon steel composite plate prepared after rolling is 7.9 mm. The bonding interface of the prepared medium carbon steel composite plate was observed microscopically, and the results are as follows: Figure 4As shown in the figure, there is no obvious composite interface and pores, and the grains at the interface have been recrystallized into complete and continuous grains shared by the two billets. Due to the diffusion of C during the composite process, the carbon steel on one side may be decarburized near the interface, forming more ferrite ( Figure 4 The white part in the middle). According to statistics and calculations, the number of holes in the entire composite interface is 3, and the average hole size is 4.9 m, the binding rate is 99.7%, indicating that the composite effect is good.

[0026] Example 5 A method for preparing a medium carbon steel composite plate with a high interface bonding rate comprises the following steps: S1. Material preparation: prepare two medium carbon steel billets; the material of the medium carbon steel billets is medium carbon high-quality carbon structural steel; S2. Cleaning: Clean the interface bonding surface of the medium carbon steel billet to remove oil stains and oxides. The surface roughness of the bonding interface is required to be less than or equal to 1.6 m; S3. Pretreatment: Align the bonding surface of the medium carbon steel billet and heat it to 1200℃, with a heating rate of no more than 2℃ / s, and keep it warm for 5 minutes; S4, rolling: take out the double-layer medium carbon steel billet and place it in a vacuum environment for single-pass rolling. The vacuum degree is not higher than 5×10 -2 Pa, rolling temperature is 1150℃, the temperature is kept constant during rolling, the reduction rate is 22%, and the strain rate is 0.02s -1 ; S5. Cooling: air cool to room temperature.

[0027] In this embodiment, the initial thickness of the medium carbon steel double-layer billet is 10 mm, and the thickness of the medium carbon steel composite plate prepared after rolling is 7.9 mm. The bonding interface of the prepared medium carbon steel composite plate was observed microscopically, and the results are as follows: Figure 5 As shown in the figure, there is no obvious composite interface and pores, and the grains at the interface are complete and continuous recrystallized grains. According to statistics and calculations, the number of pores in the entire composite interface is 18, and the average pore size is 6.4 m, the binding rate is 98.0%, indicating that the composite effect is good.

[0028] Example 6 A method for preparing a medium carbon steel composite plate with a high interface bonding rate comprises the following steps: S1. Material preparation: prepare two medium carbon steel billets; the material of the medium carbon steel billets is medium carbon high-quality carbon structural steel; S2. Cleaning: Clean the interface bonding surface of the medium carbon steel billet to remove oil stains and oxides. The surface roughness of the bonding interface is required to be less than or equal to 1.6 m; S3. Pretreatment: Align the bonding surface of the medium carbon steel billet and heat it to 1200℃, with a heating rate of no more than 2℃ / s, and keep it warm for 5 minutes; S4, rolling: take out the double-layer medium carbon steel billet and place it in a vacuum environment for single-pass rolling. The vacuum degree is not higher than 5×10 -2 Pa, the rolling temperature is 1100℃, the temperature is kept constant during rolling, the reduction rate is 22%, and the strain rate is 0.01s -1 ; S5. Cooling: air cool to room temperature.

[0029] In this embodiment, the initial thickness of the medium carbon steel double-layer billet is 10 mm, and the thickness of the medium carbon steel composite plate prepared after rolling is 7.9 mm. The bonding interface of the prepared medium carbon steel composite plate was observed microscopically, and the results are as follows: Figure 6 As shown in the figure, there is no obvious composite interface and pores, and the grains at the interface are complete and continuous recrystallized grains. According to statistics and calculations, the number of pores in the entire composite interface is 6, and the average pore size is 5.2 m, the binding rate is 99.4%, indicating that the composite effect is good.

[0030] Example 7 A method for preparing a medium carbon steel composite plate with a high interface bonding rate comprises the following steps: S1. Material preparation: prepare two medium carbon steel billets; the material of the medium carbon steel billets is medium carbon high-quality carbon structural steel; S2. Cleaning: Clean the interface bonding surface of the medium carbon steel billet to remove oil stains and oxides. The surface roughness of the bonding interface is required to be less than or equal to 1.6 m; S3. Pretreatment: Align the bonding surface of the medium carbon steel billet and heat to 1100°C, with a heating rate of no more than 2°C / s, and keep warm for 8 minutes; S4, rolling: take out the double-layer medium carbon steel billet and place it in a vacuum environment for single-pass rolling. The vacuum degree is not higher than 5×10 -2 Pa, the rolling temperature is 1100℃, the temperature is kept constant during rolling, the reduction rate is 19.5%, and the strain rate is 0.03s -1 ; S5. Cooling: air cool to room temperature.

[0031] In this embodiment, the initial thickness of the medium carbon steel double-layer billet is 10 mm, and the thickness of the medium carbon steel composite plate prepared after rolling is 8.05 mm. The bonding interface of the prepared medium carbon steel composite plate was observed microscopically, and the results are as follows: Figure 7As shown in the figure, there is no obvious composite interface and pores, and the grains at the interface are complete and continuous recrystallized grains. According to statistics and calculations, the number of pores in the entire composite interface is 10, and the average pore size is 5.3 m, the binding rate is 99%, indicating that the composite effect is good.

[0032] Example 8 A method for preparing a medium carbon steel composite plate with a high interface bonding rate comprises the following steps: S1. Material preparation: prepare two medium carbon steel billets; the material of the medium carbon steel billets is medium carbon high-quality carbon structural steel; S2. Cleaning: Clean the interface bonding surface of the medium carbon steel billet to remove oil stains and oxides. The surface roughness of the bonding interface is required to be less than or equal to 1.6 m; S3. Pretreatment: Align the bonding surface of the medium carbon steel billet and heat it to 1300℃, with a heating rate of no more than 2℃ / s, and keep it warm for 8 minutes; S4, rolling: take out the double-layer medium carbon steel billet and place it in a vacuum environment for single-pass rolling. The vacuum degree is not higher than 5×10 -2 Pa, the rolling temperature is 1200℃, the temperature is kept constant during rolling, the reduction rate is 19.5%, and the strain rate is 0.03s -1 ; S5. Cooling: air cool to room temperature.

[0033] In this embodiment, the initial thickness of the medium carbon steel double-layer billet is 10 mm, and the thickness of the medium carbon steel composite plate prepared after rolling is 8.05 mm. The bonding interface of the prepared medium carbon steel composite plate was observed microscopically, and the results are as follows: Figure 8 As shown in the figure, there is no obvious composite interface and pores, and the grains at the interface are complete and continuous recrystallized grains. According to statistics and calculations, the number of pores in the entire composite interface is 14, and the average pore size is 7.0 m, the binding rate is 98.1%, indicating that the composite effect is good.

[0034] Comparative Example 1 A method for preparing a medium carbon steel composite plate with a high interface bonding rate comprises the following steps: S1. Material preparation: prepare two medium carbon steel billets; the material of the medium carbon steel billets is medium carbon high-quality carbon structural steel; S2. Cleaning: Clean the interface bonding surface of the medium carbon steel billet to remove oil stains and oxides. The surface roughness of the bonding interface is required to be less than or equal to 1.6 m; S3. Pretreatment: Align the bonding surface of the medium carbon steel billet and heat it to 1200℃, with a heating rate of no more than 2℃ / s, and keep it warm for 5 minutes; S4, rolling: take out the double-layer medium carbon steel billet and immediately place it in a vacuum environment for single-pass rolling. The vacuum degree is not higher than 5×10 -2 Pa, the rolling temperature is 1200℃, the temperature is kept constant during the rolling process, the reduction rate is 10%, and the strain rate is 0.05s -1 ; S5. Cooling: air cool to room temperature.

[0035] In this comparative example, the initial thickness of the medium carbon steel double-layer billet is 10 mm, and the thickness of the medium carbon steel composite plate prepared after rolling is 9 mm. The bonding interface of the prepared medium carbon steel composite plate was observed microscopically, and the results are as follows: Fig. 9 As shown, the composite interface is obvious and there are two dimensions of about 63 m and 22 The grains at the composite interface partially recrystallized, but most of the grains had poor continuity, the grains on both sides were coarse and dislocated. According to statistics and calculations, there were 24 holes in the entire composite interface, with an average hole size of 15.6 m, and the binding rate is 92.7%, indicating that the composite effect is not ideal under this strain.

[0036] Comparative Example 2 A method for preparing a medium carbon steel composite plate with a high interface bonding rate comprises the following steps: S1. Material preparation: prepare two medium carbon steel billets; the material of the medium carbon steel billets is medium carbon high-quality carbon structural steel; S2. Cleaning: Clean the interface bonding surface of the medium carbon steel billet to remove oil stains and oxides. The surface roughness of the bonding interface is required to be less than or equal to 1.6 m; S3. Pretreatment: Align the bonding surface of the medium carbon steel billet and heat it to 1200℃, with a heating rate of no more than 2℃ / s, and keep it warm for 5 minutes; S4, rolling: take out the double-layer medium carbon steel billet and place it in a vacuum environment for single-pass rolling. The vacuum degree is not higher than 5×10 -2 Pa, the rolling temperature is 1150℃, the temperature is kept constant during the rolling process, the reduction rate is 5%, and the strain rate is 0.02s -1 ; S5. Cooling: air cool to room temperature.

[0037] In this comparative example, the initial thickness of the medium carbon steel double-layer billet is 10 mm, and the thickness of the medium carbon steel composite plate prepared after rolling is 9.5 mm. The bonding interface of the prepared medium carbon steel composite plate was observed microscopically, and the results are as follows: Fig.10 As shown, the composite interface is obvious and there is a size of about 76 The grain continuity at the composite interface is poor, and the grains on both sides are coarse and dislocated. According to statistics and calculations, the number of holes in the entire composite interface is 61, and the average hole size is 11.0 m, and the binding rate is 86.7%, indicating that the composite effect is not ideal under this strain.

[0038] In some of the above embodiments and comparative examples, the reason why the rolling temperature in step 4 is lower than the holding temperature in step 3 is that in large-scale production, when the medium carbon steel billet is taken out of the heating furnace and enters the next rolling process, the temperature is relatively high, and although the transfer time may be only a few seconds, a small drop in temperature will still occur. Therefore, the rolling temperature is slightly lower than the heating and holding temperature in accordance with the actual production rules, so it is necessary to explore.

[0039] From the results of Examples 1-8 and Comparative Examples 1-2, it can be seen that the interface bonding rate of the medium carbon steel composite plate prepared in the examples of the present application is higher than 96.2%, which is significantly higher than that of the comparative example. In addition, the present invention does not require vacuum electron beam welding for blanking, but only requires vacuuming during the rolling process; only single-pass rolling is required, which greatly reduces the number of rolling passes compared to the existing process, simplifies the process flow, improves production efficiency, and the entire operation process is easy to control, the process is simple, the processing cycle is short, and the processing cost is low.

[0040] The medium-carbon high-quality carbon structural steel used in Examples 1-8 and Comparative Examples 1-2 of the present application is the same material, and its chemical composition and mass percentage are: C: 0.42%-0.50%, Si: 0.17%-0.37%, Mn: 0.50%-0.80%, P: ≦0.035%, S: ≦0.035%, Ni: ≦0.30%, Cr: ≦0.25%, Cu: ≦0.25%, and the balance is Fe. The method in the present application is not limited to the above-mentioned steel, but is also applicable to other medium-carbon steels.

[0041] The heating process in Examples 1-8 and Comparative Examples 1-2 is carried out in a heating furnace, and the heating can be carried out in a vacuum state or in an inert gas atmosphere.

[0042] The embodiments of the present invention are described in detail above with reference to the accompanying drawings, but the present invention is not limited to the described embodiments. For those skilled in the art, various changes, modifications, substitutions and variations of these embodiments are made without departing from the principles and spirit of the present invention, and still fall within the scope of protection of the present invention.

Claims

1. A method for preparing a medium carbon steel composite plate with a high interface bonding rate, characterized in that: The steps include: S1. Material preparation: prepare two medium carbon steel slabs; S2. Cleaning: Clean the bonding interface of the medium carbon steel slab to remove oil stains and oxides; S3. Pretreatment: align the bonding interface of the medium carbon steel slab, heat it to 1100℃-1300℃, and keep it warm for at least 5 minutes; S4, rolling: placing the double-layer medium carbon steel slab in a vacuum environment for single-pass rolling, the rolling temperature is 1100℃-1200℃, and the reduction rate is 16%-22%; S5. Cooling: Cool to room temperature.

2. The method for preparing a medium carbon steel composite plate with a high interface bonding rate according to claim 1, characterized in that: In the S3, pretreatment step, the temperature is heated to 1200° C., and the heating rate during the heating process is not higher than 2° C. / s.

3. The method for preparing a medium carbon steel composite plate with a high interface bonding rate according to claim 1, characterized in that: In the step S4, the temperature is kept constant.

4. The method for preparing a medium carbon steel composite plate with a high interface bonding rate according to claim 1, characterized in that: The strain rate in the S4 rolling step is 0.01s -1 -0.05s -1 .

5. The method for preparing a medium carbon steel composite plate with a high interface bonding rate according to claim 1, characterized in that: The vacuum degree in the S4 and rolling steps is not higher than 5×10 -2 Pa.

6. The method for preparing a medium carbon steel composite plate with a high interface bonding rate according to claim 1, characterized in that: In the step S2, the cleaning step requires that the surface roughness of the bonding interface is less than or equal to 1.6 m.

7. The method for preparing a medium carbon steel composite plate with a high interface bonding rate according to claim 1, characterized in that: In the cooling step S5, the cooling method is air cooling.

8. The method for preparing a medium carbon steel composite plate with a high interface bonding rate according to any one of claims 1 to 8, characterized in that: The material of the medium carbon steel slab in the material preparation step S1 is medium carbon high-quality carbon structural steel.

9. A medium carbon steel composite plate, characterized in that: The composite plate is prepared by the method for preparing a medium carbon steel composite plate with a high interface bonding rate as described in any one of claims 1 to 9.

Citation Information

Patent Citations

  • Cumulative ply rolling method for preparing high-bonding-strength copper-chromium composite material

    CN112296086A

  • Method for preparing titanium-steel composite plate by adding pure iron interlayer through electromagnetic induction heating rolling

    CN112828039A

  • Method for manufacturing steel sheet by controlled temperature rolling

    GB1511622A

  • Stainless steel composite panel having excellent interface bonding and preparation method therefor

    WO2024221604A1