Preparation method of rotor disc forge piece of steam turbine

Through the methods of upsetting, punching and reaming, rolling ring forming and tempering, the problems of coarse grains and poor performance in the forgings of the steam turbine rotor disk are solved, and the comprehensive performance of the material and the strength and toughness of the forgings are improved. .

CN119056989APending Publication Date: 2024-12-03SHANDONG IRAETA HEAVY IND
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411244014.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The forgings of steam turbine rotor disks are prone to problems such as coarse grains and poor tensile performance and low-temperature impact performance.

Method used

By using upsetting forging, punching and reaming, rolling ring forming, post-forging treatment and tempering treatment, the grain uniformity and structure of the blank are optimized by controlling process parameters such as heating temperature, insulation time and chemical composition. Reduce residual stress.

Benefits of technology

It improves the comprehensive performance of rotor disk materials, enhances grain uniformity, tensile performance and low-temperature impact performance, and optimizes the strength and toughness of forgings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119056989A_ABST
    Figure CN119056989A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of metal product forming, in particular to a steam turbine rotor disc forge piece manufacturing method which comprises the steps that 1, upsetting and drawing forging is conducted, specifically, a blank is heated and subjected to heat preservation, and then three times of upsetting and three times of drawing are conducted to obtain a round blank; 2, punching and chambering are conducted, specifically, the round blank is heated and subjected to heat preservation, then upsetting punching and chambering are conducted again, and a prefabricated blank is obtained; 3, ring rolling forming is conducted, specifically, the prefabricated blank is heated and subjected to heat preservation, then ring rolling forming is conducted, and a formed forge piece is obtained; 4, treatment after forging is conducted, specifically, cooling after forging, annealing after forging and normalizing and tempering are conducted on the formed forge piece in sequence, and a forge piece to be quenched and tempered is obtained; and fifthly, quenching and tempering treatment is conducted, specifically, rough turning, flaw detection, quenching and tempering are conducted on the forged piece to be quenched and tempered in sequence. According to the preparation method of the steam turbine rotor disc forge piece, the forge piece grains are fully refined, the hardenability and hardenability of the forge piece are improved, and therefore the tensile property of the forge piece is guaranteed, and the low-temperature impact property and the low residual stress level are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal product forming, and in particular to a method for preparing a steam turbine rotor disc forging. Background Art

[0002] A steam turbine is a rotary steam power device that can convert the thermal energy of steam into mechanical energy for the rotation of the turbine rotor. The high-temperature and high-pressure steam entering the turbine passes through a fixed nozzle to form an accelerated airflow, which is sprayed onto the blades, driving the rotor equipped with blade rows to rotate and perform work externally. Steam turbines are the main equipment of modern thermal power plants and are also widely used in the metallurgical industry, chemical industry, and ship power plants. The turbine body is the main component of the turbine equipment. It consists of a rotating part (rotor) and a fixed part (stator). The rotor is one of the most important components in the turbine and is responsible for the energy conversion of the working fluid and the transmission of torque. The rotor is in a high-temperature working fluid and rotates at a high speed. It not only bears the huge stress caused by the centrifugal force of the blades, impellers, and main shaft itself, but also bears the thermal stress caused by uneven temperature distribution. In addition, the centrifugal force of the unbalanced mass will also cause rotor vibration. The strength and mass uniformity of the rotor are crucial to the energy transfer process.

[0003] The turbine rotor is usually composed of an axially symmetrical rotor disk and an impeller. The rotor disk is a flat disk with a certain number of arc-shaped or straight blades installed on it, so it is also called a blade disk. The function of the rotor disk is to convert the energy of the imported high-pressure steam into rotational kinetic energy and discharge the outlet low-pressure steam at the same time. Since the impeller rotates at a high circumferential speed in a high-temperature, high-pressure steam medium for a long time, the rotor disk needs to withstand large external loads and internal stresses. The existing technology generally uses forging technology to process metal blanks, which makes it difficult to ensure the grain uniformity of the rotor disk material, and is prone to cold hardening, and the tensile properties and low-temperature impact properties are not ideal. Summary of the invention

[0004] In view of the technical problems that turbine rotor forgings are prone to coarse grains, unsatisfactory tensile properties and low-temperature impact properties, the present invention provides a method for preparing turbine rotor disc forgings, wherein the blank is subjected to upsetting forging, punching and expanding, ring rolling, post-forging treatment and tempering treatment in sequence, and the process parameters of each step are regulated to improve the comprehensive properties of the rotor disc material.

[0005] The technical solution of the present invention is as follows: A method for preparing a steam turbine rotor disc forging comprises the following steps: Step 1: Upsetting and drawing forging, heating the billet to 1230-1250℃ and keeping it warm, then performing two upsetting and three drawing to obtain a round billet, wherein the holding time is 0.8-2.0min / mm calculated based on the average thickness; Step 2: Punching and expanding, heating the round blank to 1210-1240°C and keeping it warm for 1-2 hours, and then upsetting, punching and expanding it again to obtain a preform; Step 3: Ring rolling forming, heating the preform to 1180-1200℃ and keeping it warm for 1-2h, then ring rolling forming to obtain a formed forging; Step 4: Post-forging treatment, sequentially performing post-forging cooling, post-forging annealing, normalizing + tempering on the formed forgings to obtain the forgings to be quenched and tempered; Step 5: Quenching and tempering treatment, rough turning, flaw detection, quenching and tempering are carried out on the quenched and tempered forgings in sequence.

[0006] Further, in step 1, the blank includes the following chemical compositions in mass percentage: C 0.26%-0.30%, Si≤0.10%, Mn 0.30%-0.60%, P ≤0.010%, S ≤0.003%, Cr 1.35%-1.75%, Ni 3.30%-3.90%, Mo0.50%-0.80%, V 0.10%-0.20%, Al 0.010%-0.020%, Ti≤0.003%, B≤0.0005%, Cu≤0.10%, N≤0.007%, [O] ≤15 ppm, [H]≤1.5 ppm, As ≤0.010%, Sn ≤0.005%, Sb ≤0.002%, Pb ≤0.010%, Bi ≤0.010%, the remainder being Fe and other inevitable impurity elements. The present invention optimizes the chemical composition of the billet, effectively controls the content of harmful elements such as P, S, As, Sn, Pb, Sb, Bi, etc. in the billet, reduces the gas content, and improves the quality level of the billet.

[0007] Furthermore, in step 1, the upsetting ratios of the first upsetting and the second upsetting are controlled to be 2.0-3.0 respectively, and controlling the upsetting ratios of the first upsetting and the second upsetting is conducive to ensuring that the inside of the blank is fully forged. The upsetting ratio is calculated according to the following formula: upsetting ratio = blank height before upsetting / blank height after upsetting.

[0008] Furthermore, in step 2, the upsetting ratio of the second upsetting is controlled to be 2.5-3.0, and the punch specification is not less than φ200mm. The hole expansion size is controlled to ensure that the axial and radial deformations of the preform are coordinated in the next step of ring rolling, to ensure that the preform can be smoothly engaged during ring rolling, and to successfully complete the radial and axial rolling process under the action of the cone roller, main roller and core roller of the ring rolling machine.

[0009] Furthermore, in step 4, the formed forging is slowly cooled in a slow cooling furnace to a surface temperature of ≤300° C. and then taken out of the furnace and air-cooled to room temperature.

[0010] Furthermore, in step 4, the post-forging annealing includes the following five stages in sequence: the first stage, heating to 350°C at a rate of ≤80°C / h and keeping warm for 1-4h; the second stage, heating to 650°C at a rate of ≤50°C / h and keeping warm for 1-4h; the third stage, heating to 880-930°C at a rate of ≤150°C / h and keeping warm, and the holding time is 30-50mm / h calculated according to the wall thickness of the forging; the fourth stage, air cooling to a surface temperature of 600-650°C after being taken out of the furnace; the fifth stage, returning to the furnace to isothermal, the isothermal temperature is 550-650°C, the isothermal time is 15-30mm / h calculated according to the wall thickness of the forging, and after the isothermal is completed, air cooling to room temperature after being taken out of the furnace.

[0011] Furthermore, in step 4, normalizing + tempering includes the following six processes in sequence: process 1, heating to 350°C at a rate of ≤80°C / h and keeping warm for 1-4h; process 2, heating to 650°C at a rate of ≤50°C / h and keeping warm for 1-5h; process 3, heating to 840-900°C at a rate of ≤150°C / h and keeping warm, and the holding time is 30-50mm / h calculated according to the wall thickness of the forging; process 4, air cooling to the surface temperature of 200-300°C after being taken out of the furnace, and returning to the furnace for tempering; process 5, heating to 300°C and isothermal, and the isothermal time is 3-6h; process 6, heating to 650°C at a rate of ≤80°C / h and keeping warm, and the holding time is 20-40mm / h calculated according to the wall thickness of the forging. After the insulation is completed, the forging is cooled with the furnace to a furnace temperature of ≤300°C, and then air cooled after being taken out of the furnace.

[0012] Furthermore, in step five, quenching includes the following four processes in sequence: process a, heating to 350°C at a rate of ≤80°C / h and keeping warm for 1-4h; process b, heating to 650°C at a rate of ≤50°C / h and keeping warm for 1-4h; process c, heating to 830-860°C at a rate of ≤150°C / h and keeping warm, and the holding time is 30-50mm / h calculated based on the wall thickness of the forging after rough turning; process d, quenching cooling is carried out by water-air alternating cooling, which improves the hardenability and hardenability of the forging.

[0013] Further, in step 5, tempering includes the following three processes in sequence: process ①, heating to 300℃ isothermal, the isothermal time is 1-4h; process ②, heating to 600-650℃ tempering at a speed of ≤80℃ / h, and the tempering holding time is 20-40mm / h calculated according to the wall thickness of the forging after rough turning; process ③, after the tempering and holding is completed, slow cooling with the furnace, controlling the slow cooling speed to 15-25℃ / h, and the slow cooling time to 15-30h; process ④, after the forging is slowly cooled to 300-320℃, it is air-cooled out of the furnace. The present invention effectively reduces the internal residual stress of the forging by controlling the slow cooling speed, slow cooling time and air cooling temperature out of the furnace during the tempering process after quenching.

[0014] The beneficial effects of the present invention are: The invention provides a preparation method of a steam turbine rotor disc forging, wherein the blank is subjected to upsetting forging, punching and expanding, ring rolling, post-forging treatment and quenching and tempering treatment in sequence, and the blank is heated and kept warm before and after two upsettings and three drawing processes, thereby providing a guarantee for fully forging the blank; by controlling the heat treatment parameters in the upsetting forging, punching and expanding, and ring rolling processes, the residual stress inside the forging is reduced, the internal segregation of the forging is reduced, the internal organizational structure and grains of the forging are fully refined, and the grain uniformity is improved; in the process of post-forging treatment, the formed forging is subjected to post-forging cooling, post-forging annealing, normalizing+tempering in sequence, thereby further reducing the residual stress generated by the forging during the forging process, thereby achieving the optimization and improvement of the strength, plasticity and toughness of the forging. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0016] Figure 1 This is a microstructure diagram of the forging product body sampled in Example 1.

[0017] Figure 2 This is the microstructure diagram of the forging product body sample in Example 2. DETAILED DESCRIPTION

[0018] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0019] Example 1 A steam turbine rotor disc forging with an outer diameter of φ1275 mm, an inner diameter of φ550 mm, and a height of 340 mm, wherein the preparation method comprises the following steps: Step 1: blanking and upsetting forging. The specific operations are as follows: (1) Cutting: The steel ingot is cut into square billets with a cross-sectional side length of 700 mm. Billets with a sawing height of 1005 mm are used for forging this product.

[0020] (2) Forging and drawing, the square billet is heated to 1250℃ in a furnace and kept at this temperature for 10.0h. The square billet includes the following chemical compositions by mass percentage: C 0.29%, Si 0.10%, Mn 0.48%, P 0.005%, S 0.001%, Cr 1.539%, Ni3.69%, Mo 0.60%, Al 0.012%, Ti 0.002%, Cu 0.030%, V 0.16%, B 0.0003%, As 0.0041%, Sn0.0025%, Pb 0.0009%, Sb 0.0001%, Bi 0.0001%, [O]=15 ppm, [H]=1.2 ppm, and the balance is Fe and other unavoidable impurity elements.

[0021] The square billet is upset twice and drawn twice in the following order: first drawn to a square billet with a cross-sectional side length of 620 mm and a height of 1255 mm, then upset to a square billet with a cross-sectional side length of 900 mm and a height of 595 mm, and the upsetting ratio of the first upsetting is about 2.11; the square billet that has completed the first upsetting is pulled to a square billet with a cross-sectional side length of 620 mm and a height of 1255 mm, then upset to a square billet with a cross-sectional side length of 900 mm and a height of 595 mm, and the upsetting ratio of the second upsetting is about 2.11; the square billet that has completed the second upsetting is pulled to a round billet with a diameter of 760 mm and a height of 1065 mm and returned to the furnace.

[0022] Step 2: Punching and expanding, the round blank is returned to the furnace and heated to 1230℃ and kept warm for 2.0h. After being taken out of the furnace, it is upset to a round blank with a height of 400mm, and the upsetting ratio of the third upsetting is controlled to be about 2.7. A φ240mm punch is used to punch the round blank with a height of 400mm, and the hole is expanded to φ300mm to obtain a preform, which is returned to the furnace.

[0023] Step 3: Ring rolling forming, the preform is returned to the furnace and heated to 1200℃ and kept warm for 2.0 hours. After it is taken out of the furnace, it is ring rolled to the preset size to obtain a formed forging.

[0024] Step 4: Post-forging treatment, sequentially perform post-forging cooling, post-forging annealing, normalizing + tempering on the formed forgings to obtain the forgings to be quenched and tempered. The specific operations are as follows: (1) Post-forging cooling and post-forging annealing: First, place the formed forging in a slow cooling furnace, slowly cool it to the surface temperature of the formed forging at 200°C, then take it out of the furnace and air cool it to room temperature. Then, place the formed forging in a heat treatment furnace with a temperature of ≤250°C, heat it to 350°C at a rate of 60°C / h and keep it at that temperature for 3.0h; heat it to 650°C at a rate of 30°C / h and keep it at that temperature for 3.0h; heat it to 920°C at a rate of 80°C / h and keep it at that temperature for 12.0h calculated according to the wall thickness of the formed forging; take it out of the furnace and air cool it to the surface temperature of 600°C, then return it to the furnace for isothermal treatment. The isothermal temperature is 600°C and the isothermal time is 30.0h calculated according to the wall thickness of the formed forging. After the isothermal treatment is completed, take it out of the furnace and air cool it to room temperature to complete the post-forging annealing.

[0025] (2) Normalizing + tempering: Place the forgings that have been annealed after forging in a heat treatment furnace with a temperature of ≤250℃, heat them to 350℃ at a rate of ≤120℃ / h and keep them at that temperature for 3.0h; heat them to 650℃ at a rate of 30℃ / h and keep them at that temperature for 5.0h; heat them to 870℃ at a rate of 80℃ / h and keep them at that temperature for 12.0h calculated based on the wall thickness of the forgings; air cool them out of the furnace until the surface temperature of the forgings reaches 200℃, and return them to the furnace for tempering; heat them to 300℃ and keep them at that temperature for 5.0h; heat them to 650℃ at a rate of 60℃ / h and keep them at that temperature for 20.0h calculated based on the wall thickness of the forgings. After the insulation is completed, cool the forgings with the furnace until the furnace temperature is ≤300℃, then air cool them out of the furnace to obtain the forgings to be tempered.

[0026] Step 5: Quenching and tempering treatment, rough turning, flaw detection, quenching and tempering are carried out on the quenched and tempered forgings in sequence. The specific operations are as follows: a. Rough turning, flaw detection, and quenching. Rough turning is performed on the quenched and tempered forgings according to the size of the turbine rotor disk forgings (design drawings), and then flaw detection is performed on the quenched and tempered forgings according to the JB / T 5000.15 standard to ensure that the requirements of the standard Class I are met. The quenched and tempered forgings are placed in a heat treatment furnace with a temperature of ≤250℃, and the temperature is increased to 350℃ at a rate of 60℃ / h and kept warm for 2.0h; the temperature is increased to 650℃ at a rate of 30℃ / h and kept warm for 3.0h; the temperature is increased to 840℃ at a rate of 80℃ / h and kept warm. The holding time is calculated as 9.0h based on the wall thickness of the quenched and tempered forgings after rough turning; quenching cooling is performed by water-air alternating cooling, and the surface final cooling temperature is controlled to be no higher than 180℃ to complete the quenching.

[0027] b. Tempering, which includes the following three processes in sequence: process ①, the quenched forgings are placed in a heat treatment furnace with a temperature of ≤300℃, and the temperature is raised to 300℃ for isothermal treatment, and the isothermal time is 3.0h; process ②, the temperature is raised to 630℃ at a rate of 80℃ / h for tempering and insulation, and the tempering and insulation time is 13.5h calculated based on the wall thickness of the quenched and tempered forgings after rough turning; process ③, after the tempering and insulation is completed, the forgings are slowly cooled with the furnace, and the slow cooling rate is controlled to be 15-25℃ / h, and the slow cooling time is 15-30h; process ④, after the forgings are slowly cooled to the furnace temperature of 300-320℃, they are taken out of the furnace and air-cooled to obtain forging products.

[0028] Step 6: Sampling the forging product obtained in this embodiment to conduct mechanical property testing, residual stress testing and microstructure testing.

[0029] (1) Mechanical properties test: Samples were cut from the inner holes of forging products to test the mechanical properties of the forging products. The test results are shown in Table 1: Table 1 The results of the mechanical properties test of the forging products obtained in this example

[0030] (2) Residual stress detection: The residual stress of the forging product obtained in this embodiment was detected according to the method specified in GB / T 31310. The detection results are shown in Table 2: Table 2 Residual stress test results of the forging products obtained in this example

[0031] (3) Microstructure test: Take a sample from the inner hole of the forging product and observe its microstructure. The microstructure diagram is as follows: Figure 1 As shown by Figure 1 It can be seen that the forgings made by the method of the present invention have uniform microstructure after quenching and tempering, and each phase in the microstructure is uniformly dispersed without obvious segregation.

[0032] Example 2 A steam turbine rotor disc forging with an outer diameter of φ1340 mm, an inner diameter of φ550 mm, and a height of 230 mm, wherein the preparation method comprises the following steps: Step 1: Cutting and upsetting forging. The specific operations are as follows: (1) Cutting: The steel ingot is cut into square billets with a cross-sectional side length of 700 mm. Billets with a sawing height of 775 mm are used for forging this product.

[0033] (2) Forging and drawing, the square billet is heated to 1250℃ in a furnace and kept at this temperature for 10.0h. The square billet includes the following chemical compositions by mass percentage: C 0.29%, Si 0.10%, Mn 0.48%, P 0.005%, S 0.001%, Cr 1.539%, Ni3.69%, Mo 0.60%, Al 0.012%, Ti 0.002%, Cu 0.030%, V 0.16%, B 0.0003%, As 0.0041%, Sn0.0025%, Pb 0.0009%, Sb 0.0001%, Bi 0.0001%, [O]=15 ppm, [H]=1.2 ppm, and the balance is Fe and other unavoidable impurity elements.

[0034] The square billet is upset twice and drawn twice in the following order: first drawn to a square billet with a cross-sectional side length of 560 mm and a height of 1185 mm, then upset to a square billet with a cross-sectional side length of 815 mm and a height of 560 mm, and the upsetting ratio of the first upsetting is about 2.12; the square billet that has completed the first upsetting is pulled to a square billet with a cross-sectional side length of 560 mm and a height of 1185 mm, then upset to a square billet with a cross-sectional side length of 815 mm and a height of 560 mm, and the upsetting ratio of the second upsetting is about 2.12; the square billet that has completed the second upsetting is pulled to a round billet with a diameter of 750 mm and a height of 840 mm and returned to the furnace.

[0035] Step 2: Punching and expanding, the round blank is returned to the furnace and heated to 1230℃ and kept warm for 2.0h. After being taken out of the furnace, it is upset to a round blank with a height of 290mm. The upsetting ratio of the third upsetting is controlled to be about 2.9. A φ240mm punch is used to punch the round blank with a height of 290mm, and the hole is expanded to φ300mm to obtain a preform, which is returned to the furnace.

[0036] Step 3: Ring rolling forming, the preform is returned to the furnace and heated to 1200℃ and kept warm for 2.0 hours. After it is taken out of the furnace, it is ring rolled to the preset size to obtain a formed forging.

[0037] Step 4: Post-forging treatment, sequentially perform post-forging cooling, post-forging annealing, normalizing + tempering on the formed forgings to obtain the forgings to be quenched and tempered. The specific operations are as follows: (1) Post-forging cooling and post-forging annealing: First, place the formed forging in a slow cooling furnace, slowly cool it to the surface temperature of the formed forging at 200°C, then take it out of the furnace and air cool it to room temperature. Then, place the formed forging in a heat treatment furnace with a temperature of ≤250°C, heat it to 350°C at a rate of 60°C / h and keep it at that temperature for 3.0h; heat it to 650°C at a rate of 30°C / h and keep it at that temperature for 3.0h; heat it to 920°C at a rate of 80°C / h and keep it at that temperature for 12.0h calculated according to the wall thickness of the formed forging; take it out of the furnace and air cool it to the surface temperature of 600°C, then return it to the furnace for isothermal treatment. The isothermal temperature is 600°C and the isothermal time is 30.0h calculated according to the wall thickness of the formed forging. After the isothermal treatment is completed, take it out of the furnace and air cool it to room temperature to complete the post-forging annealing.

[0038] (2) Normalizing + tempering: Place the forgings that have been annealed after forging in a heat treatment furnace with a temperature of ≤250℃, heat them to 350℃ at a rate of ≤120℃ / h and keep them at that temperature for 3.0h; heat them to 650℃ at a rate of 30℃ / h and keep them at that temperature for 5.0h; heat them to 870℃ at a rate of 80℃ / h and keep them at that temperature for 12.0h calculated based on the wall thickness of the forgings; air cool them out of the furnace until the surface temperature of the forgings reaches 200℃, and return them to the furnace for tempering; heat them to 300℃ and keep them at that temperature for 5.0h; heat them to 650℃ at a rate of 60℃ / h and keep them at that temperature for 20.0h calculated based on the wall thickness of the forgings. After the insulation is completed, cool the forgings with the furnace until the furnace temperature is ≤300℃, then air cool them out of the furnace to obtain the forgings to be tempered.

[0039] Step 5: Quenching and tempering treatment, rough turning, flaw detection, quenching and tempering are carried out on the quenched and tempered forgings in sequence. The specific operations are as follows: a. Rough turning, flaw detection, and quenching. Rough turning is performed on the quenched and tempered forgings according to the size of the turbine rotor disk forgings (design drawings), and then flaw detection is performed on the quenched and tempered forgings according to the JB / T 5000.15 standard to ensure that the requirements of the standard Class I are met. The quenched and tempered forgings are placed in a heat treatment furnace with a temperature of ≤250℃, and the temperature is increased to 350℃ at a rate of 60℃ / h and kept warm for 2.0h; the temperature is increased to 650℃ at a rate of 30℃ / h and kept warm for 3.0h; the temperature is increased to 840℃ at a rate of 80℃ / h and kept warm. The holding time is calculated as 9.0h based on the wall thickness of the quenched and tempered forgings after rough turning; quenching cooling is performed by water-air alternating cooling, and the surface final cooling temperature is controlled to be no higher than 180℃ to complete the quenching.

[0040] b. Tempering, which includes the following three processes in sequence: process ①, the quenched forgings are placed in a heat treatment furnace with a temperature of ≤300℃, and the temperature is raised to 300℃ for isothermal treatment, and the isothermal time is 3.0h; process ②, the temperature is raised to 630℃ at a rate of 80℃ / h for tempering and insulation, and the tempering and insulation time is 13.5h calculated based on the wall thickness of the quenched and tempered forgings after rough turning; process ③, after the tempering and insulation is completed, the forgings are slowly cooled with the furnace, and the slow cooling rate is controlled to be 15-25℃ / h, and the slow cooling time is 15-30h; process ④, after the forgings are slowly cooled to the furnace temperature of 300-320℃, they are taken out of the furnace and air-cooled to obtain forging products.

[0041] Step 6: Sampling the forging product obtained in this embodiment to conduct mechanical property testing, residual stress testing and microstructure testing.

[0042] (1) Mechanical properties test: The forging products obtained in this example were sampled and subjected to mechanical properties test. The test results are shown in Table 3: Table 3 The results of the mechanical properties test of the forging products obtained in this example

[0043] (2) Residual stress detection: The residual stress of the forging product obtained in this embodiment was detected according to the method specified in GB / T 31310. The detection results are shown in Table 4: Table 4 Residual stress test results of the forging products obtained in this example

[0044] (3) Microstructure test: Take a sample from the inner hole of the forging product and observe its microstructure. The microstructure diagram is as follows: Figure 2 As shown by Figure 2 It can be seen that the forgings made by the method of the present invention have uniform microstructure after quenching and tempering, and each phase in the microstructure is uniformly dispersed without obvious segregation.

[0045] Although the present invention has been described in detail with reference to the accompanying drawings and in combination with the preferred embodiments, the present invention is not limited thereto. Without departing from the spirit and essence of the present invention, a person of ordinary skill in the art may make various equivalent modifications or substitutions to the embodiments of the present invention, and these modifications or substitutions shall be within the scope of the present invention. Any person of ordinary skill in the art may easily think of changes or substitutions within the technical scope disclosed by the present invention, and these shall be within the scope of protection of the present invention.

Claims

1. A method for preparing a steam turbine rotor disc forging, characterized in that: The steps include: Step 1: Upsetting and drawing forging, heating the billet to 1230-1250℃ and keeping it warm, then performing two upsetting and three drawing to obtain a round billet, wherein the holding time is 0.8-2.0min / mm calculated based on the average thickness; Step 2: Punching and expanding, heating the round blank to 1210-1240°C and keeping it warm for 1-2 hours, and then upsetting, punching and expanding it again to obtain a preform; Step 3: Ring rolling forming, heating the preform to 1180-1200℃ and keeping it warm for 1-2h, then ring rolling forming to obtain a formed forging; Step 4: Post-forging treatment, sequentially performing post-forging cooling, post-forging annealing, normalizing + tempering on the formed forgings to obtain the forgings to be quenched and tempered; Step 5: Quenching and tempering treatment, rough turning, flaw detection, quenching and tempering are carried out on the quenched and tempered forgings in sequence.

2. The method for preparing a steam turbine rotor disk forging according to claim 1, characterized in that: In step 1, the blank includes the following chemical compositions by mass percentage: C 0.26%-0.30%, Si ≤0.10%, Mn 0.30%-0.60%, P ≤0.010%, S ≤0.003%, Cr 1.35%-1.75%, Ni 3.30%-3.90%, Mo 0.50%-0.80%, V 0.10%-0.20%, Al 0.010%-0.020%, Ti≤0.003%, B≤0.0005%, Cu≤0.10%, N≤0.007%, [O] ≤15 ppm, [H]≤1.5 ppm, As ≤0.010%, Sn ≤0.005%, Sb ≤0.002%, Pb ≤0.010%, Bi ≤0.010%, the balance is Fe and other inevitable impurity elements.

3. The method for preparing a steam turbine rotor disk forging according to claim 1, characterized in that: In step 1, the upsetting ratios of the first upsetting and the second upsetting are controlled to be 2.0-3.0 respectively.

4. The method for preparing a steam turbine rotor disk forging according to claim 1, characterized in that: In step 2, the upsetting ratio of the second upsetting is controlled to be 2.5-3.0, and the punch specification is not less than φ200mm.

5. The method for preparing a steam turbine rotor disk forging according to claim 1, characterized in that: In step 4, the formed forging is slowly cooled in a slow cooling furnace to a surface temperature of ≤300°C and then taken out of the furnace and air-cooled to room temperature.

6. The method for preparing a steam turbine rotor disk forging according to claim 1, characterized in that: In step 4, the post-forging annealing includes the following five stages in sequence: the first stage, heating to 350°C and keeping warm for 1-4h; the second stage, heating to 650°C and keeping warm for 1-4h; the third stage, heating to 880-930°C and keeping warm, and the holding time is 30-50mm / h calculated according to the wall thickness of the forging; the fourth stage, air cooling to the surface temperature of 600-650°C after being taken out of the furnace; the fifth stage, returning to the furnace to isothermal, the isothermal temperature is 550-650°C, the isothermal time is 15-30mm / h calculated according to the wall thickness of the forging, and after the isothermal is completed, the furnace is air cooled to room temperature.

7. The method for preparing a steam turbine rotor disk forging according to claim 1, characterized in that: In step 4, normalizing + tempering includes the following six processes in sequence: process 1, heating to 350℃ and keeping warm for 1-4h; process 2, heating to 650℃ and keeping warm for 1-5h; process 3, heating to 840-900℃ and keeping warm, and the holding time is 30-50mm / h calculated according to the wall thickness of the forging; process 4, air cooling to the surface temperature of 200-300℃ after being taken out of the furnace, and returning to the furnace for tempering; process 5, heating to 300℃ and isothermal, and the isothermal time is 3-6h; process 6, heating to 650℃ and keeping warm, and the holding time is 20-40mm / h calculated according to the wall thickness of the forging. After the insulation is completed, it is taken out of the furnace and air cooled.

8. The method for preparing a steam turbine rotor disk forging according to claim 1, characterized in that: In step five, quenching includes the following four processes in sequence: process a, heating to 350°C and keeping warm for 1-4h; process b, heating to 650°C and keeping warm for 1-4h; process c, heating to 830-860°C and keeping warm, and the holding time is 30-50mm / h calculated according to the wall thickness of the forging after rough turning; process d, quenching cooling is carried out by water-air alternating cooling.

9. The method for preparing a steam turbine rotor disk forging according to claim 1, characterized in that: In step five, tempering includes the following three processes in sequence: process ①, heating to 300℃ and isothermal, the isothermal time is 1-4h; process ②, heating to 600-650℃ and tempering, the tempering holding time is 20-40mm / h calculated according to the wall thickness of the forging after rough turning; process ③, after the tempering and holding is completed, slow cooling with the furnace, controlling the slow cooling speed to 15-25℃ / h, and the slow cooling time is 15-30h; process ④, after the forging is slowly cooled to 300-320℃, it is air-cooled out of the furnace.

Citation Information

Patent Citations

  • Forging and machining process of special marine rear pipe body forge piece

    CN112024798A

  • Manufacturing method of gear ring forge piece for wind power speed increasing box

    CN114289675A

  • Manufacturing method of high-performance 30Cr2Ni4MoV wheel disc forge piece for gas turbine

    CN114472791A