Ultra-width-to-thickness-ratio slab continuous casting submersed nozzle on-line rapid replacement method
By quickly replacing the immersion water port of the ultra-wide-thickness ratio slab continuous casting, the problem of mismatch between the use time of the immersion water port and the tundra is solved, and higher production efficiency and material utilization are achieved, and cost is reduced.
Patent Information
- Application Number
- CN202410973311.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-12-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In the existing ultra-wide-thickness-biased slab continuous casting machine, the use time of the immersion water outlet does not match the use time of the intermediate tundra, resulting in low efficiency of the tundra retardant material, reducing the continuous casting production operation rate and increasing production costs.
The method of quickly changing the immersion water outlets online includes determining the replacement time according to the production time, performing pretreatment such as baking, and replacing it in a determined furnace time, controlling the pull speed change to achieve rapid replacement.
The number of continuous pouring furnaces for single tundish is increased, the downtime is reduced, the production efficiency and utilization rate of tundish are improved, and the cost of retardant materials is reduced.
Smart Images

Figure CN119057053A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of continuous casting, and in particular to a method for online rapid replacement of an immersed nozzle for continuous casting of an ultra-width-to-thickness ratio slab. Background Art
[0002] The crystallizer thickness of the ultra-width-to-thickness ratio slab continuous casting machine is generally 150mm, and the maximum width is generally 3200mm. The width-to-thickness ratio is large, and it is produced by a single submerged nozzle. The submerged nozzle refractory material has a short service life, while the tundish refractory material has a long service life. The service life of the submerged nozzle does not match the service life of the tundish, resulting in the tundish refractory material utilization efficiency not meeting the requirements, which not only reduces the continuous casting production operation rate, but also increases the production cost. Summary of the invention
[0003] The technical problem to be solved by the present invention is to overcome the disadvantages of the prior art and provide a method for online rapid replacement of an ultra-width-to-thickness ratio slab continuous casting submerged nozzle.
[0004] In order to solve the above technical problems, the technical solution of the present invention is as follows: A method for online rapid replacement of an ultra-width-to-thickness ratio slab continuous casting submerged nozzle, comprising: Determine the replacement time of the submerged nozzle according to the production time; Complete the pretreatment of the submerged nozzle before the replacement time of the submerged nozzle; Determine the furnace number for replacing the submerged nozzle, and replace the submerged nozzle in the corresponding furnace.
[0005] As a preferred solution of the method for online rapid replacement of the submerged nozzle for continuous casting of ultra-width-thickness ratio slabs of the present invention, the pretreatment of the submerged nozzle before the replacement time of the submerged nozzle includes: Bake the submerged nozzle.
[0006] As a preferred solution of the method for online rapid replacement of the submerged nozzle for continuous casting of ultra-width-thickness ratio slabs of the present invention, the baking of the submerged nozzle comprises: Place the immersion spout on the baking rack; The baking temperature is set to be greater than or equal to 900°C and the baking time is greater than or equal to 2h to bake the submerged nozzle.
[0007] As a preferred solution of the method for online rapid replacement of the submerged nozzle for continuous casting of ultra-width-thickness ratio slabs of the present invention, the method of determining the heat for replacing the submerged nozzle and replacing the submerged nozzle in the corresponding heat includes: When replacing the immersion nozzle furnace, the casting speed is reduced to 1.0m / min; Transport the pre-treated submerged nozzle to the crystallizer, open the cylinder of the tundish quick-change mechanism, and remove the blind plate; Reduce the pulling speed to 0.8 m / min; Place the submerged water inlet on the cover plate of the crystallizer; Reduce the pulling speed to 0.6 m / min; Place the submerged nozzle in the crystallizer and install it at the blind plate position of the tundish quick-change mechanism, and close the oil cylinder of the tundish quick-change mechanism; Reduce the pulling speed to 0.4 m / min; Press the quick-change button to replace the immersion nozzle.
[0008] As a preferred solution of the method for online quick replacement of the submerged nozzle for continuous casting of ultra-width-thickness ratio slab of the present invention, after the quick change button is pressed to replace the submerged nozzle, the method further comprises: Increase the pulling speed to 0.6 m / min; Clamp the replaced immersion nozzle and remove it from the crystallizer; Increase the pulling speed to 0.8 m / min; Clean the cold steel around the nozzle and increase the pulling speed to 1.0m / min; Increase the pulling speed to normal pulling speed.
[0009] As a preferred solution of the method for online rapid replacement of the submerged nozzle for continuous casting of ultra-width-thickness ratio slabs of the present invention, before replacing the submerged nozzle heat and reducing the casting speed to 1.0 m / min, it also includes: Improve the superheat of the molten steel in the previous furnace of the replacement of the submerged nozzle furnace.
[0010] As a preferred solution of the method for online rapid replacement of submerged nozzles for continuous casting of ultra-width-to-thickness ratio slabs of the present invention, the superheat degree of the molten steel is greater than or equal to 30°C.
[0011] The beneficial effects of the present invention are: The present invention realizes the online replacement of the submerged nozzle, can increase the number of continuous casting furnaces of a single tundish, reduce the downtime for continuous casting and group change, and improve production efficiency. At the same time, it increases the use time of a single tundish, increases the utilization rate of a single tundish, and reduces the use cost of refractory materials for the tundish. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative labor.
[0013] Figure 1 A schematic diagram of a process for online rapid replacement of an ultra-width-to-thickness ratio slab continuous casting submerged nozzle provided by the present invention; Figure 2 Schematic diagram of the change in pulling speed during the process of replacing the submerged nozzle. DETAILED DESCRIPTION
[0014] In order to make the content of the present invention more clearly understood, the present invention is further described in detail below according to specific implementation modes and in combination with the accompanying drawings.
[0015] Figure 1 A schematic diagram of a method for online rapid replacement of an ultra-wide-to-thickness ratio slab continuous casting submerged nozzle provided in an embodiment of the present application. The method comprises the following steps: Step S101: Determine the replacement time of the submerged nozzle according to the production time.
[0016] Specifically, first, according to the production plan requirements, it is determined whether the submerged nozzle of the continuous casting machine crystallizer needs to be quickly replaced. If it is determined that it needs to be quickly replaced, the replacement time of the submerged nozzle is determined according to the production time.
[0017] Step S102: completing pretreatment of the submerged nozzle before the submerged nozzle is replaced.
[0018] Specifically, the unused immersion nozzle is baked. The immersion nozzle is placed on a baking rack. Then, the baking temperature is set to be greater than or equal to 900°C, and the baking time is greater than or equal to 2 hours, and the immersion nozzle is baked. After the baking is completed, the pretreatment of the immersion nozzle is achieved.
[0019] Step S103: Determine the heat for replacing the submerged nozzle, and replace the submerged nozzle in the corresponding heat.
[0020] Specifically, determine the heat order for replacing the submerged nozzle. After determining the heat order, contact the operator of the previous process to appropriately increase the superheat of the molten steel. In this embodiment, the superheat of the molten steel is greater than or equal to 30°C. After that, perform the following steps in sequence to achieve the replacement of the submerged nozzle.
[0021] Step S103a: Based on the temperature of the tundish, the pulling speed of the continuous casting machine crystallizer is slowly reduced to 1.0 m / min.
[0022] Step S103b: The baked immersion nozzle is transported to the side of the crystallizer using a special tool, and at the same time, the cylinder of the tundish quick-change mechanism is opened and the blind plate is removed.
[0023] Step S103c: slowly reduce the pulling speed of the continuous casting machine crystallizer to 0.8 m / min.
[0024] Step S103d: clean the fiber blanket wrapped around the unused immersion nozzle, clamp the neck of the immersion nozzle with a special clamping tool, and lift the immersion nozzle onto the cover plate next to the crystallizer.
[0025] Step S103e: Slowly reduce the pulling speed to 0.6 m / min.
[0026] Step S103f: Place the submerged water inlet in the crystallizer and install it at the blind plate position of the tundish quick-change mechanism, and close the tundish quick-change mechanism cylinder.
[0027] Step S103g: Slowly reduce the pulling speed to 0.4 m / min.
[0028] Step S103h: Press the quick-change button to replace the immersion nozzle.
[0029] Step S103i: slowly increase the pulling speed to 0.6 m / min.
[0030] Step S103j: clamping the replaced immersion nozzle and removing it from the crystallizer; Step S103k: slowly increase the pulling speed to 0.8 m / min.
[0031] Step S1031: clean the cold steel around the nozzle and slowly increase the pulling speed to 1.0 m / min.
[0032] Step S103m: slowly increase the pulling speed to the normal pulling speed.
[0033] See the schematic diagram of the change of casting speed during the replacement of the submerged nozzle in the above steps. Figure 2 .
[0034] By adopting the above method, the online replacement of the submerged nozzle is realized, the number of continuous casting furnaces of a single tundish can be increased, the downtime for continuous casting and changing groups can be reduced, and production efficiency can be improved. At the same time, the use time of a single tundish is increased, the utilization rate of a single tundish is increased, and the use cost of refractory materials for the tundish is reduced.
[0035] In addition to the above embodiments, the present invention may also have other implementation modes; any technical solutions formed by equivalent replacement or equivalent transformation shall fall within the protection scope required by the present invention.
Claims
1. A method for online rapid replacement of an ultra-width-thickness ratio slab continuous casting immersion nozzle, characterized in that: include: Determine the replacement time of the submerged nozzle according to the production time; Complete the pretreatment of the submerged nozzle before the replacement time of the submerged nozzle; Determine the furnace number for replacing the submerged nozzle, and replace the submerged nozzle in the corresponding furnace.
2. The method for online rapid replacement of submerged nozzles for continuous casting of ultra-width-thickness ratio slabs according to claim 1 is characterized in that: The pretreatment of the submerged nozzle before the submerged nozzle replacement time includes: Bake the submerged nozzle.
3. The method for online rapid replacement of submerged nozzles for continuous casting of ultra-width-thickness ratio slabs according to claim 2 is characterized in that: The baking of the submerged nozzle comprises: Place the immersion spout on the baking rack; The baking temperature is set to be greater than or equal to 900°C and the baking time is greater than or equal to 2h to bake the submerged nozzle.
4. The method for online rapid replacement of submerged nozzles for continuous casting of ultra-width-thickness ratio slabs according to claim 1 is characterized in that: The step of determining the heat for replacing the submerged nozzle and replacing the submerged nozzle in the corresponding heat includes: When replacing the immersion nozzle furnace, the casting speed is reduced to 1.0m / min; Transport the pre-treated submerged nozzle to the crystallizer, open the cylinder of the tundish quick-change mechanism, and remove the blind plate; Reduce the pulling speed to 0.8 m / min; Place the submerged water inlet on the cover plate of the crystallizer; Reduce the pulling speed to 0.6 m / min; Place the submerged nozzle in the crystallizer and install it at the blind plate position of the tundish quick-change mechanism, and close the oil cylinder of the tundish quick-change mechanism; Reduce the pulling speed to 0.4 m / min; Press the quick-change button to replace the immersion nozzle.
5. The method for online rapid replacement of submerged nozzles for continuous casting of ultra-width-thickness ratio slabs according to claim 4 is characterized in that: After the quick-change button is pressed to replace the submerged nozzle, the method further includes: Increase the pulling speed to 0.6 m / min; Clamp the replaced immersion nozzle and remove it from the crystallizer; Increase the pulling speed to 0.8 m / min; Clean the cold steel around the nozzle and increase the pulling speed to 1.0m / min; Increase the pulling speed to normal pulling speed.
6. The method for online rapid replacement of submerged nozzles for continuous casting of ultra-width-thickness ratio slabs according to claim 4 is characterized in that: Before replacing the submerged nozzle furnace and reducing the casting speed to 1.0 m / min, the process also includes: Improve the superheat of the molten steel in the previous furnace of the replacement of the submerged nozzle furnace.
7. The method for online rapid replacement of submerged nozzles for continuous casting of ultra-width-to-thickness ratio slabs according to claim 6 is characterized in that: The superheat degree of the molten steel is greater than or equal to 30°C.
Citation Information
Patent Citations
Continuous casting tundish submerged nozzle on-line roasting apparatus and roasting method
CN101879590A
Method for increasing success rate of heat exchange of continuous casting machine tundish
CN103464699A
Continuous casting tundish nozzle replacement process
CN113084145A
Method for reducing slag entrapment by replacing submersed nozzle in square billet continuous casting
CN114619022A
Nozzle exchange apparatus for tundish
KR1020040031309A