Welding method for all-position automatic welding of corrosion-resistant pipe

Through the full-position automatic welding method and copper pad device, the problems of low welding efficiency and inconsistent quality of corrosion-resistant pipelines are solved, efficient and stable welding joint performance is achieved, and the efficient welding needs of corrosion-resistant pipelines are met.

CN119057180APending Publication Date: 2024-12-03BAOSHAN IRON & STEEL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310629207.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-31
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

In the prior art, the welding efficiency of corrosion-resistant pipelines is low, and manual welding leads to inconsistent welding quality and high labor intensity, which cannot meet the actual high efficiency needs of the project.

Method used

The full-position automatic welding method is adopted, including processing the U-shaped bevel at the welding end, and the fixed installation device uses a hexagonal boss and copper pad. The base layer, fill layer and cover layer are welded through the gas protection welding process, combining the appearance and Non-destructive testing meets the high performance requirements of welded joints.

Benefits of technology

It improves welding efficiency and quality consistency, reduces the labor intensity of welding personnel, and ensures that the tensile strength, bending and impact toughness of the welded joints meet the standard requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119057180A_ABST
    Figure CN119057180A_ABST
Patent Text Reader

Abstract

The invention discloses a welding method for all-position automatic welding of a corrosion-resistant pipe. The welding method comprises the following steps that S1, a groove is machined in the welding end of a pipe fitting; s2, the grooves of the two pipe fittings are assembled in pairs; s3, the groove of the pipe fitting is fixed through a fixing and mounting device; s4, the bottom layer, the filling layer and the covering layer of the groove are welded; and S5, appearance and nondestructive testing is conducted on the welded pipe fitting. According to the method, the welding efficiency is improved while the welding quality is guaranteed, and all performance indexes of a welding joint meet specified requirements.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to welding technology, and more specifically to a welding method for automatic full-position welding of corrosion-resistant pipes. Background Art

[0002] Nowadays, with the continuous increase in the length of pipelines, there are more and more accidents caused by pipeline failure. According to research, most of them are caused by corrosion problems. There are three main solutions to the problem of pipeline corrosion failure: (1) physical methods, such as using ultraviolet radiation to sterilize or externally scraping the biofilm; (2) chemical methods, such as using bactericides; (3) protective coatings, such as coating the surface of metal materials with antibacterial coatings, and coating anti-adhesion super-slip or super-hydrophobic coatings to make the surface less likely to be attached by microorganisms. However, the above solutions all start from the outside of the pipeline for prevention and control, and cannot fundamentally solve the corrosion problem. At present, Cu-containing pipeline steel with good corrosion resistance has been developed, but its weldability has rarely been studied, and most of the research remains on manual welding, which cannot meet the actual high efficiency requirements of the project.

[0003] Although automated welding technology has been gradually applied to the field of offshore pipe welding, manual welding is still mostly used for corrosion-resistant pipelines, especially small-diameter pipe welding. This method is inefficient, and as the welding time increases, the energy and physical strength of the welders decrease, which will also affect the welding quality. In addition, due to the differences in welders, the consistency of welding quality is difficult to ensure.

[0004] In existing patent applications, such as Chinese patent application No. 201510089418.9, a manual welding method for corrosion-resistant steel for cargo tanks of crude oil ships is disclosed. The welding method adopts two positions, horizontal and vertical, for corrosion-resistant steel plates. The horizontal groove adopts an asymmetric double-sided V-shaped groove for welding; the vertical groove adopts a symmetrical double-sided V-shaped groove for welding; when welding, the weight percentage of each component of the welding rod is: C: 0.04-0.06%, Si: 0.2-0.3%, Mn: 1.0-2.0%, Ni+Cu+Cr+Mo mixture: 0.65-1.0%, and the balance is Fe and unavoidable impurities. The above welding method can ensure that the tensile strength of the welded joint is greater than 490MPa, the impact toughness of the welded joint at -20℃ is greater than 34J, and the weld has excellent corrosion resistance. However, the patent technology is less efficient and has a greater labor intensity for workers.

[0005] For example, Chinese patent application No. 201310726536.7 discloses a straight seam submerged arc welding method for corrosion-resistant metallurgical composite bimetallic steel pipe, comprising the following steps: pre-welding of steel pipe, welding of carbon steel layer inside pipe, welding of carbon steel layer outside pipe, welding of corrosion-resistant transition layer inside pipe, welding of corrosion-resistant layer inside pipe. The corrosion-resistant metallurgical composite bimetallic straight seam welded steel pipe provided by the present invention adopts a high-efficiency automatic submerged arc welding process, and welds each layer of metal by adopting different welding materials and welding processes, i.e., a reasonable welding sequence, so as to ensure the various properties of carbon steel layer of steel pipe and the corrosion resistance of corrosion-resistant layer. The automatic submerged arc welding process has fast welding speed, high welding efficiency, good welding quality, low technical requirements for welders, and the arc light is buried under the flux layer, without arc radiation, good working conditions, and reduced labor intensity of manual operation. However, the patent technology has more welding times and steps. Summary of the invention

[0006] In view of the defects existing in the prior art, the purpose of the present invention is to provide a welding method for all-position automatic welding of corrosion-resistant pipes, which not only ensures the welding quality but also improves the welding efficiency, and all performance indicators of the welded joints meet the specified requirements.

[0007] To achieve the above object, the present invention adopts the following technical solution:

[0008] A welding method for all-position automatic welding of corrosion-resistant pipes, comprising the following steps:

[0009] S1. Process the groove on the welding end of the pipe fitting;

[0010] S2, assembling the grooves of the two pipe fittings;

[0011] S3, fixing the groove of the pipe fitting using a fixing installation device;

[0012] S4, welding the base layer, filling layer and cover layer of the groove;

[0013] S5. Perform appearance and nondestructive testing on the welded pipe fittings.

[0014] Preferably, in the step S1, the groove is processed into a U-shaped groove;

[0015] The angle of the groove is 5°;

[0016] The blunt edge of the groove is 2±0.2 mm;

[0017] After the groove processing is completed, impurities within 30 mm on both sides of the groove are cleaned.

[0018] Preferably, in step S2, the angle variation of the groove is 0-1 mm.

[0019] Preferably, in step S3, the fixing and mounting device comprises a hexagonal boss and a copper liner provided on the side of the hexagonal boss;

[0020] Six equally divided top screw assembly holes are provided on the side surface of the hexagonal boss.

[0021] Preferably, in step S4, the base layer, the filling layer and the cover layer are all welded by gas shielded welding with a φ1.0 mm welding wire, the welding wire is Atlantic CHW-55CNH, and the gas ratio is 50% Ar+50% CO2.

[0022] Preferably, the welding current of the base layer is 240-300A, the voltage is 25-28V, the welding speed is 65-78cm / min, the swing speed is 100-150cm / min, and the swing width is 0.8-1.5mm;

[0023] The welding current of the first filling layer is 220-280A, the voltage is 22-28V, the welding speed is 70-90cm / min, the swing speed is 110-150cm / min, and the swing width is 1.5-2.5mm;

[0024] The welding current of the second filling layer is 210-250A, the voltage is 22-25V, the welding speed is 70-92cm / min, the swing speed is 130-170cm / min, and the swing width is 1.7-3.5mm;

[0025] The welding current of the cover layer is 210-250A, the voltage is 20-25V, the welding speed is 45-65cm / min, the swing speed is 160-200cm / min, and the swing width is 3.5-6.6mm.

[0026] Preferably, samples are taken from the welded pipe joints according to the DNVGL-ST-F101 standard, and the samples are subjected to tensile, bending and impact mechanical property tests;

[0027] The tensile test results of the specimens show that the tensile strength is ≥700MPa, the bending test results of the specimens show that no cracks occur when the specimens are bent to 180°, and the impact test results of the specimens show that the average and minimum impact energy values ​​of the specimens are greater than the standard values.

[0028] The present invention provides a corrosion-resistant pipe full-position automatic welding method, which not only provides technical support for welding corrosion-resistant pipelines, but also can greatly reduce the labor intensity of welders and improve welding efficiency while completing welding joints that meet requirements. The use of automated welding means is more conducive to ensuring the consistency of welding quality. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 It is a schematic flow chart of the welding method of the present invention;

[0030] Figure 2 It is a schematic diagram of the base layer, the filling layer and the cover layer in the welding method of the present invention;

[0031] Figure 3 is a schematic diagram of a fixed installation device in the welding method of the present invention;

[0032] Figure 4 Schematic diagram of a U-shaped groove in the welding method of the present invention;

[0033] Figure 5 Schematic diagram of the metallographic structure of the pipe joint in the embodiment of the welding method of the present invention. DETAILED DESCRIPTION

[0034] In order to better understand the above technical solution of the present invention, the technical solution of the present invention is further described below in conjunction with the accompanying drawings and embodiments.

[0035] Combination Figure 1 As shown, the present invention provides a method for all-position automatic welding of corrosion-resistant pipes, comprising the following steps:

[0036] S1. Welding preparation: Process the welding end of the pipe into a U-shaped groove, such as Figure 4 As shown, the angle 8 of the groove is 5°, and the blunt edge 9 of the groove is 2±0.2 mm.

[0037] After the groove processing is completed, clean the impurities (oil stains, oxide layer, etc.) within 30mm on both sides of the groove.

[0038] S2. Bevel assembly: Manually assemble the bevels of the two pipe fittings and fix them by spot welding at three points on the inner circumference of the pipe. Then, grind the excess height at the spot welding point with a grinder to make it smooth.

[0039] The misalignment of the groove is 0-1mm, and the angle of the groove after alignment is 5°.

[0040] S3. Installation of fixed installation device: Use the top screw nut and the hexagonal boss to make the copper gasket fit tightly to the bottom of the circular groove.

[0041] like Figure 3 As shown, the fixing and mounting device 5 includes a hexagonal boss and a copper pad arranged on the side of the hexagonal boss.

[0042] Six equally divided top screw assembly holes 6 are provided on the side surface of the hexagonal boss.

[0043] A mounting platform 7 for mounting a copper liner is provided on the side of the hexagonal boss.

[0044] S4. The base layer, filling layer and cover layer of the groove are welded using φ1.0mm gas shielded welding process. The welding wire is Atlantic CHW-55CNH and the gas ratio is 50% Ar + 50% CO2.

[0045] like Figure 2 As shown, the welding current of the base layer 4 is 240-300A, the voltage is 25-28V, the welding speed is 65-78cm / min, the swing speed is 100-150cm / min, and the swing width is 0.8-1.5mm;

[0046] The welding current of the first filling layer 3 is 220-280A, the voltage is 22-28V, the welding speed is 70-90cm / min, the swing speed is 110-150cm / min, and the swing width is 1.5-2.5mm;

[0047] The welding current of the second filling layer 2 is 210-250A, the voltage is 22-25V, the welding speed is 70-92cm / min, the swing speed is 130-170cm / min, and the swing width is 1.7-3.5mm;

[0048] The welding current of the cover layer 1 is 210-250A, the voltage is 20-25V, the welding speed is 45-65cm / min, the swing speed is 160-200cm / min, and the swing width is 3.5-6.6mm.

[0049] S5. Carry out appearance inspection and non-destructive testing such as ultrasonic and X-ray flaw detection on the welded pipe fittings.

[0050] The welding method of the present invention adopts an efficient full-position automatic welding method, combined with a simple copper liner installation device designed independently, to ensure that the single-sided weld back of the base welding is forced to form. A complete set of welding process specifications has been established for the automatic welding of corrosion-resistant pipes, which ensures the welding quality and welding efficiency while ensuring that the various properties of corrosion-resistant pipe joints meet relevant standards. On the basis of using corrosion-resistant pipes, corrosion-resistant welding wires are further selected, and combined with more mature full-position automatic welding technology for pipelines, the base layer, filling layer and cover layer are all fully automatically welded, which can not only improve the corrosion resistance of the pipeline and the filling material itself, but also ensure the welding efficiency of the oil and gas pipeline at the same time.

[0051] The welding method of the present invention is aimed at the characteristics of corrosion-resistant pipes. Based on the full-position automatic welding means, a set of full-position automatic welding process specifications for corrosion-resistant pipes is developed. The difference between its welding process specifications and ordinary pipes is mainly in the matching coordination between welding process parameters and the automatic adjustment of the welding gun inclination angle, which is specifically reflected in the following two aspects: first, the fluidity of the molten metal in the weld is poor, especially in the overhead welding area of ​​the pipeline welding, the molten metal has a more obvious falling phenomenon, presenting a "peak shape"; second, in the vertical welding area of ​​the pipeline, the bottom layer is prone to incomplete penetration. In view of the above problems, through theoretical analysis and practical verification, a set of full-position automatic welding process parameter adjustment specifications for corrosion-resistant pipes is obtained, and the adjustment of welding parameters follows the matching relationship of multiple parameters. The welding process specifications of the present invention adjust the above four welding process parameters by reducing the wire feeding speed and welding speed within a certain range in the overhead welding area, increasing the swing speed and edge residence time, and at the same time increasing the welding gun inclination angle by 10° in the vertical welding area, so that the weld formation in all areas of the pipeline at all positions finally meets the standard requirements.

[0052] It should be noted that the base layer is particularly important in the full-position automated welding of pipelines. The quality of the base layer directly affects the forming quality of the subsequent welds of the weld. The present invention adopts a forced forming base layer scheme on the back of the copper liner. Through scheme analysis, the following scheme is designed: Figure 3 The copper liner installation device shown in the figure. The device is designed to match the pipe diameter size, and the device consists of 6 arc trapezoidal copper liners and a copper liner placement rack. The arc copper liner trapezoidal offset design can adapt to a certain range of pipe inner diameters. The copper liner placement rack is designed with an initial area for copper liner placement, and the boss edge required for copper liner installation is specially reserved in the initial area for placement, which is convenient for adjusting the position of the copper liner. In each initial area, a hexagonal threaded hole is designed, and six round head screws are screwed into the screw holes. By tightening the six screws, the six-petal copper liner in the initial area can be tightly fitted to the bottom circumference of the groove, and it can be ensured that the six-petal copper liner is tightly connected end to end on the circumference after installation, forming a complete copper liner ring, which can ensure the smooth implementation of forced forming of the copper liner during welding. The copper liner installation device is novel and innovative in design. The device is simple to process, easy to operate and install, and quick and convenient to disassemble. It can assist the pipeline full-position external welding machine to complete forced forming welds with good quality.

[0053] The welding method of the present invention can be applied to gas metal arc welding (GMAW) of pipeline steel, and its main application prospects include the following industries: oil pipelines, chemical pipes and the like.

[0054] Example

[0055] Select X65Q pipeline steel with a specification of φ219*12mm, use a lathe to process the U-shaped groove, and grind and clean the oxide layer, oil stains and other impurities within 30mm on both sides of the groove with a grinder. The groove form is as follows: Figure 3 As shown, the groove angle is 5° and the blunt edge is 2±0.2mm. After cleaning, manual assembly is performed to ensure that the error is within the range of 0-1mm. Use a magnetic seat to fix the groove on the circumference, and then take three points at the bottom of the groove inside the circumference for spot welding. After spot welding, use a grinder to grind it flat to complete the assembly process. Install the copper liner through the hexagonal top screw nut device. The device is as follows Figure 2 As shown, ensure that the copper liner fits tightly with the bottom of the groove. Install the guide rail and welding trolley, use φ1.0mm welding wire and gas shielded welding with a gas ratio of 50% Ar + 50% CO2 to weld the base layer, filling layer and cover layer. The welding parameters of each layer are shown in Tables 1, 2, 3, and 4.

[0056] Table 1 Base layer welding process parameters

[0057]

[0058] Table 2 Welding process parameters of the first filling layer

[0059]

[0060] Table 3 Welding process parameters of the second filling layer

[0061]

[0062] Table 4 Cover layer welding process parameters

[0063]

[0064] According to DNVGL-ST-F101 standard, 2 tensile specimens, 3 bending specimens and 6 notched impact specimens were taken from the pipe joints, and mechanical properties tests such as tensile, bending and impact were carried out on the specimens. The test data are shown in Tables 5, 6 and 7.

[0065] Table 5 Tensile test

[0066] Sample No. Sample thickness (mm) Sample width (mm) Fracture location Tensile strength(Mpa) Test results L1 12 37 Base Material 704 qualified L2 12 37 Base Material 721 qualified

[0067] The tensile test results in Table 5 show that the tensile strength is 535 MPa and the test fracture occurs at the parent material, which meets the requirements of DNVGL-ST-F101 standard.

[0068] Table 6 Bending test

[0069]

[0070] The bending test results in Table 6 show that the specimen can be bent to 180° without any cracks, which meets the requirements of DNVGL-ST-F101 standard.

[0071] Table 7 Impact test

[0072]

[0073] The impact test results in Table 7 show that the average and minimum impact energy of the samples are greater than the standard values, which meets the requirements of DNVGL-ST-F101 standard.

[0074] Metallographic sampling was performed on the pipe joint, and macroscopic observation was performed as follows: Figure 5 As shown in the figure, the thickness of each welding layer is moderate, the interlayer fusion is good, and no visible defects are generated.

[0075] Those skilled in the art should recognize that the above embodiments are only used to illustrate the present invention, and are not intended to limit the present invention. As long as they are within the spirit of the present invention, any changes or modifications to the above embodiments will fall within the scope of the claims of the present invention.

Claims

1. A welding method for all-position automatic welding of corrosion-resistant pipes. It is characterized in that The following steps are involved: S1. Process the groove on the welding end of the pipe fitting; S2, assembling the grooves of the two pipe fittings; S3, fixing the groove of the pipe fitting using a fixing installation device; S4, welding the base layer, filling layer and cover layer of the groove; S5. Perform appearance and nondestructive testing on the welded pipe fittings.

2. The welding method for all-position automatic welding of corrosion-resistant pipe according to claim 1, Features: In the step S1, the groove is processed into a U-shaped groove; The angle of the groove is 5°; The blunt edge of the groove is 2±0.2 mm; After the groove processing is completed, impurities within 30 mm on both sides of the groove are cleaned.

3. The welding method for all-position automatic welding of corrosion-resistant pipe according to claim 1, Features: In the step S2, the angle between the groove and the groove is 0 to 1 mm.

4. The welding method for all-position automatic welding of corrosion-resistant pipes according to claim 1, Features: In step S3, the fixing and mounting device includes a hexagonal boss and a copper liner provided on the side of the hexagonal boss; Six equally divided top screw assembly holes are provided on the side surface of the hexagonal boss.

5. The welding method for all-position automatic welding of corrosion-resistant pipe according to claim 1, Features: In step S4, the base layer, the filling layer, and the cover layer are all welded by gas shielded welding with a diameter of 1.0 mm. The welding wire is Atlantic CHW-55CNH, and the gas ratio is 50% Ar + 50% CO 2 .

6. The welding method for all-position automatic welding of corrosion-resistant pipe according to claim 5, Features: The welding current of the base layer is 240-300A, the voltage is 25-28V, the welding speed is 65-78cm / min, the swing speed is 100-150cm / min, and the swing width is 0.8-1.5mm; The welding current of the first filling layer is 220-280A, the voltage is 22-28V, the welding speed is 70-90cm / min, the swing speed is 110-150cm / min, and the swing width is 1.5-2.5mm; The welding current of the second filling layer is 210-250A, the voltage is 22-25V, the welding speed is 70-92cm / min, the swing speed is 130-170cm / min, and the swing width is 1.7-3.5mm; The welding current of the cover layer is 210-250A, the voltage is 20-25V, the welding speed is 45-65cm / min, the swing speed is 160-200cm / min, and the swing width is 3.5-6.6mm.

7. The welding method for all-position automatic welding of corrosion-resistant pipes according to claim 6, Features: According to DNVGL-ST-F101 standard, samples are taken from welded pipe joints and subjected to tensile, bending and impact mechanical performance tests. The tensile test results of the specimens show that the tensile strength is ≥700MPa, the bending test results of the specimens show that no cracks occur when the specimens are bent to 180°, and the impact test results of the specimens show that the average and minimum impact energy values ​​of the specimens are greater than the standard values.

Citation Information

Patent Citations

  • Pipeline welding method

    CN104014909A

  • Liner structure for abutting steel pipe and welding method

    CN104889530A

  • Non-backing type full-automatic butt welding technology for girth weld of seabed carbon steel pipeline

    CN106112222A

  • Welding method for slope pipeline

    CN108098110A

  • MAG welding process for austenitic stainless steel pipeline

    CN110695499A