Heat treatment method for improving mechanical property of steel casting

Through heat treatment and surface treatment before and after welding repair, the problem of poor mechanical properties in the welding repair area of ​​cast steel parts is solved, and the mechanical properties of cast steel parts are restored and the stability of the welding area is improved.

CN119057387AInactive Publication Date: 2024-12-03ANHUI ANGONG MASCH MFG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411190553.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the prior art, cast steel parts are prone to local cracks and impurity defects during welding repair, resulting in a reduction in the mechanical properties of the welding repair zone, increasing the difficulty of repair, and may lead to deformation or deformation of the castings.

Method used

The surface treatment of the cast steel parts before welding repair, including PT detection, cleaning of oil and rust, decompression, repair welding and grinding, and then heating and insulation treatment in the heat treatment furnace, combining natural cooling and appropriate cooling methods to ensure that Welding area structure uniformity.

Benefits of technology

Through heat treatment before and after welding repair, the internal stress of the cast steel parts is eliminated, and the unstable quenched martensite is transformed into tempered martensite or turbanite is restored, the original mechanical properties of the welding area are improved, and the overall mechanical properties of the cast steel parts are improved. Welding strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119057387A_ABST
    Figure CN119057387A_ABST
Patent Text Reader

Abstract

The invention discloses a heat treatment method for improving the mechanical property of a steel casting. The heat treatment method specifically comprises the following steps that 1, surface defects of the steel casting are treated; 2, repairing the surface of the steel casting; 3, the repaired steel casting is placed in a heat treatment furnace, the steel casting is heated to 500 DEG C to 650 DEG C at the temperature rising speed of 50 DEG C / h to 80 DEG C / h, and heat preservation is conducted for 1 h to 1.5 h within the range of 500 DEG C to 650 DEG C; fourthly, the steel casting is taken out of the heat treatment furnace and placed in air to be naturally cooled; in the process of digging and welding the surface of the steel casting, the mechanical property of a material in a repair welding area is different from the mechanical property of the steel casting, and the internal stress of the steel casting can be eliminated by heating the steel casting before repair welding and heating and heat preservation in a heat treatment furnace after welding; and unstable quenched martensite is converted into tempered martensite, totalites or sorbite, so that the strength and hardness of a welding area of the steel casting are reduced, namely, the mechanical property of the steel casting in the original state is recovered.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of heat treatment, and in particular to a heat treatment method for improving the mechanical properties of steel castings. Background Art

[0002] The internal factors that affect the mechanical properties of steel castings include the characteristics of the material itself, such as bonding, organization, structure, and atomic nature; the external factors include the test temperature, strain rate, stress state, sample size and accuracy, sample processing method, etc. In the prior art, the patent document with announcement number CN107119176A discloses a heat treatment method for improving the mechanical properties of steel castings, wherein the steel castings are heat treated, and the heat treatment includes normalizing, rapid cooling, tempering, and furnace cooling steps. The normalizing step is to keep the temperature when the temperature of the steel casting reaches 920°C to 950°C, and the rapid cooling step is to take The steel casting is cooled by blowing air with a fan, and a water mist machine is used to spray cooling water mist onto the steel casting to ensure that the cooling rate of the steel casting reaches 10°C / min to 20°C / min; the tempering step is to heat the steel casting to 630°C to 650°C again, and the holding time is the maximum wall thickness of the steel casting multiplied by (1 to 1.5) min; and the steel casting is cooled after being taken out of the furnace. For steel castings of this type with a high residual Al content, the present invention adopts the methods of increasing the normalizing temperature, extending the normalizing holding time, increasing the normalizing cooling rate, increasing the tempering holding temperature and shortening the tempering holding time, thereby reducing the harmful effects of Al compounds in the steel casting on the organizational properties.

[0003] During PT inspection on the casting surface, cracks or impurity defects may be found in some local locations, which require excavation welding. If a large amount of welding is performed, the stress of the casting will be increased, the mechanical properties of the welding area will be reduced, or the casting will be deformed, which increases the difficulty of welding repair of defects in steel castings. Based on this, there is an urgent need to invent a more practical solution. Summary of the invention

[0004] The purpose of the present invention is to solve the shortcomings of the prior art and to propose a heat treatment method for improving the mechanical properties of steel castings.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] A heat treatment method for improving the mechanical properties of steel castings, comprising the following specific steps:

[0007] Step 1: Treatment of surface defects of steel castings: Perform PT inspection on the surface of steel castings. Clean the oil, dirt and rust on the surface of steel castings in unqualified areas, remove the defects mechanically, and then grind them into grooves.

[0008] Step 2: Repairing the surface of the steel casting: firstly, heat the steel casting to reach the welding temperature, then repair the groove of the defective part by welding, and the repair welding scar is higher than the surface of the steel casting;

[0009] Step 3, placing the repaired steel casting in a heat treatment furnace, heating the steel casting to 500°C-650°C at a heating rate of 50°C / h-80°C / h, and keeping the temperature within the range of 500°C-650°C for 1-1.5h;

[0010] Step 4: Take the steel casting out of the heat treatment furnace and place it in the air for natural cooling;

[0011] The chemical composition of the steel casting and the mass percentage of each component element are as follows: C=0.12-0.55%, Si=0.20-0.6%, Mn=0.5-1.0%, P≤0.015%, S≤0.025%, Cr≤2.20%, Mo≤0.9%, Ni≤0.3%, V≤0.01%, Cu≤0.1%, and the rest are Fe and unavoidable impurity elements.

[0012] Preferably, in step 2, the steel casting is heated to a welding repair temperature of 100°C-260°C, and heating is continued during the welding repair process. The impurities and moisture near the cracks, sand holes or bubbles of the steel casting contain impurities and moisture that are difficult to clean. The impurities and moisture inside are discharged by heating, thereby reducing the formation of defects such as pores during the welding repair process.

[0013] Preferably, in step 2, the groove is repaired by welding, and the repaired welding area higher than the surface of the cast iron part is polished until it is flush with the surface of the cast iron part, and the repaired weld is checked to ensure that defects such as lack of fusion, slag inclusion, undercut, surface pores, incomplete weld, and cracks are not allowed. If the above defects occur, repeat step S1 to ensure that the polished surface is flat and the transition is smooth.

[0014] Preferably, in step 3, the steel casting is heated to 450°C in a heat treatment furnace at a heating rate of 50°C / h-80°C / h, and then heated to 500°C-650°C at a heating rate of 80°C / h-120°C / h. The temperature is increased at a slower rate in the early stage to refine the structure of the steel casting so that it has the required mechanical properties and to prepare for subsequent heat treatment. The temperature is heated at a faster rate in the later stage, and the temperature is increased twice at different heating rates to increase the heating rate and reduce the time used.

[0015] Preferably, in step 4, the steel casting is cooled to 100°C-200°C in the heat treatment furnace together with the heat treatment furnace, and then the steel casting is taken out and placed in an aqueous solution, organic oil or air cooling box for cooling at an appropriate rate so that the components in the steel casting and the weld repair area are transformed into stable structures, thereby improving the structural uniformity of the steel casting and avoiding deformation or cracking of the casting.

[0016] The present invention has the following beneficial effects:

[0017] The heat treatment method for improving the mechanical properties of steel castings proposed in the present invention is that during the process of excavation welding on the surface of steel castings, the mechanical properties of the material in the weld repair area differ from those of the steel castings. By heating the steel castings before welding and heating and heat-insulating them in a heat treatment furnace after welding, the internal stress of the steel castings can be eliminated, and the unstable quenched martensite can be transformed into tempered martensite, troostite or troostite, so that the strength and hardness of the welding area of ​​the steel castings are reduced, that is, the mechanical properties of the steel castings are restored to their original state. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 The present invention is a schematic diagram of a heat treatment method for improving the mechanical properties of steel castings. DETAILED DESCRIPTION

[0019] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.

[0020] In the description of the present invention, it is necessary to understand that the terms "upper", "lower", "front", "back", "left", "right", "top", "bottom", "inside", "outside", etc., indicating the orientation or position relationship are based on the orientation or position relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.

[0021] Example 1

[0022] Reference Figure 1 , a heat treatment method for improving the mechanical properties of steel castings, comprising the following specific steps:

[0023] Step 1: Treatment of surface defects of steel castings: Perform PT inspection on the surface of steel castings. Clean the oil, dirt and rust on the surface of steel castings in unqualified areas, remove the defects mechanically, and then grind them into grooves.

[0024] Step 2: Repairing the surface of the steel casting: firstly, heat the steel casting to reach the welding temperature, then repair the groove of the defective part by welding, and the repair welding scar is higher than the surface of the steel casting;

[0025] Step 3, placing the repaired steel casting in a heat treatment furnace, heating the steel casting to 500°C-650°C at a heating rate of 50°C / h-80°C / h, and keeping the temperature within the range of 500°C-650°C for 1-1.5h;

[0026] Step 4: Take the steel casting out of the heat treatment furnace and place it in the air to cool naturally.

[0027] Among them, in step 2, the steel casting is heated to reach a welding temperature of 100°C-260°C, and heating is continued during the welding process. The cracks, sand holes or bubbles near the steel casting contain impurities and moisture that are difficult to clean. The impurities and moisture inside are discharged by heating, thereby reducing the formation of defects such as pores during the welding process.

[0028] In step 2, the groove is repaired by welding, and the repaired welding area higher than the surface of the cast iron part is polished until it is flush with the surface of the cast iron part. The repaired weld is checked to ensure that there are no defects such as lack of fusion, slag inclusion, undercut, surface pores, incomplete welding of welds, and cracks. If the above defects occur, repeat step S1 to ensure that the polished surface is flat and the transition is smooth.

[0029] In step 3, the steel casting is heated to 450°C in a heat treatment furnace at a heating rate of 50°C / h-80°C / h, and then heated to 500°C-650°C at a heating rate of 80°C / h-120°C / h. The temperature is increased at a slower rate in the early stage to refine the structure of the steel casting so that it has the required mechanical properties and prepare for subsequent heat treatment. The temperature is heated at a faster rate in the later stage, and the temperature is increased twice at different heating rates to increase the heating rate and reduce the time used.

[0030] Step 4, the steel casting is cooled to 100°C-200°C in the heat treatment furnace together with the heat treatment furnace, then the steel casting is taken out and placed in an aqueous solution, organic oil or air cooling box for cooling, and cooled at an appropriate rate so that the components in the steel casting and the weld repair area are transformed into stable structures, thereby improving the uniformity of the structure of the steel casting and avoiding deformation or cracking of the casting.

[0031] In this embodiment, the chemical composition of the steel casting used and the mass percentage of each component element are as follows: C=0.12%, Si=0.20%, Mn=0.5%, P≤0.015%, S≤0.025%, Cr≤2.20%, Mo≤0.9%, Ni≤0.3%, V≤0.01%, Cu≤0.1%, and the rest are Fe and unavoidable impurity elements. The welding material used is the same as the material of the steel casting. The mechanical properties of the steel casting tested are tensile strength Rm=600~660MPa, yield strength Rp0.2=420~450MPa, elongation A=20%~24%, and cross-sectional shrinkage Z=43%~50%.

[0032] Example 2

[0033] A heat treatment method for improving the mechanical properties of steel castings, comprising the following specific steps:

[0034] Step 1: Treatment of surface defects of steel castings: Perform PT inspection on the surface of steel castings. Clean the oil, dirt and rust on the surface of steel castings in unqualified areas, remove the defects mechanically, and then grind them into grooves.

[0035] Step 2: Repairing the surface of the steel casting: firstly, heat the steel casting to reach the welding temperature, then repair the groove of the defective part by welding, and the repair welding scar is higher than the surface of the steel casting;

[0036] Step 3, placing the repaired steel casting in a heat treatment furnace, heating the steel casting to 500°C-650°C at a heating rate of 50°C / h-80°C / h, and keeping the temperature within the range of 500°C-650°C for 1-1.5h;

[0037] Step 4: Take the steel casting out of the heat treatment furnace and place it in the air to cool naturally.

[0038] Among them, in step 2, the steel casting is heated to reach a welding temperature of 100°C-260°C, and heating is continued during the welding process. The cracks, sand holes or bubbles near the steel casting contain impurities and moisture that are difficult to clean. The impurities and moisture inside are discharged by heating, thereby reducing the formation of defects such as pores during the welding process.

[0039] In step 2, the groove is repaired by welding, and the repaired welding area higher than the surface of the cast iron part is polished until it is flush with the surface of the cast iron part. The repaired weld is checked to ensure that there are no defects such as lack of fusion, slag inclusion, undercut, surface pores, incomplete welding of welds, and cracks. If the above defects occur, repeat step S1 to ensure that the polished surface is flat and the transition is smooth.

[0040] In step 3, the steel casting is heated to 450°C in a heat treatment furnace at a heating rate of 50°C / h-80°C / h, and then heated to 500°C-650°C at a heating rate of 80°C / h-120°C / h. The temperature is increased at a slower rate in the early stage to refine the structure of the steel casting so that it has the required mechanical properties and prepare for subsequent heat treatment. The temperature is heated at a faster rate in the later stage, and the temperature is increased twice at different heating rates to increase the heating rate and reduce the time used.

[0041] Step 4, the steel casting is cooled to 100°C-200°C in the heat treatment furnace together with the heat treatment furnace, then the steel casting is taken out and placed in an aqueous solution, organic oil or air cooling box for cooling, and cooled at an appropriate rate so that the components in the steel casting and the weld repair area are transformed into stable structures, thereby improving the uniformity of the structure of the steel casting and avoiding deformation or cracking of the casting.

[0042] In this embodiment, the chemical composition of the steel casting used and the mass percentage of each component element are: C=0.55%, Si=0.6%, Mn=1.0%, P≤0.015%, S≤0.025%, Cr≤2.20%, Mo≤0.9%, Ni≤0.3%, V≤0.01%, Cu≤0.1%, and the rest are Fe and unavoidable impurity elements. The welding material used is the same as the material of the steel casting. The mechanical properties of the steel casting tested are tensile strength Rm=620~680MPa, yield strength Rp0.2=422~470MPa, elongation A=25%~28%, and cross-sectional shrinkage Z=50%~65%.

[0043] The heat treatment method for improving the mechanical properties of steel castings proposed in the present invention is that during the process of excavation welding on the surface of steel castings, the mechanical properties of the material in the weld repair area differ from those of the steel castings. By heating the steel castings before welding and heating and heat-insulating them in a heat treatment furnace after welding, the internal stress of the steel castings can be eliminated, and the unstable quenched martensite can be transformed into tempered martensite, troostite or troostite, so that the strength and hardness of the welding area of ​​the steel castings are reduced, that is, the mechanical properties of the steel castings are restored to their original state.

[0044] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A heat treatment method for improving the mechanical properties of steel castings, characterized in that: Including the following details: Step 1: Treatment of surface defects of steel castings: Perform PT inspection on the surface of steel castings. Clean the oil, dirt and rust on the surface of steel castings in unqualified areas, remove the defects mechanically, and then grind them into grooves. Step 2: Repairing the surface of the steel casting: firstly, heat the steel casting to reach the welding temperature, then repair the groove of the defective part by welding, and the repair welding scar is higher than the surface of the steel casting; Step 3, placing the repaired steel casting in a heat treatment furnace, heating the steel casting to 500°C-650°C at a heating rate of 50°C / h-80°C / h, and keeping the temperature within the range of 500°C-650°C for 1-1.5h; Step 4: Take the steel casting out of the heat treatment furnace and place it in the air for natural cooling; The chemical composition of the steel casting and the mass percentage of each component element are as follows: C=0.12-0.55%, Si=0.20-0.6%, Mn=0.5-1.0%, P≤0.015%, S≤0.025%, Cr≤2.20%, Mo≤0.9%, Ni≤0.3%, V≤0.01%, Cu≤0.1%, and the rest are Fe and unavoidable impurity elements.

2. A heat treatment method for improving the mechanical properties of steel castings according to claim 1, characterized in that: In the step 2, the steel casting is heated to a welding temperature of 100° C. to 260° C., and the heating is continued during the welding process.

3. A heat treatment method for improving the mechanical properties of steel castings according to claim 2, characterized in that: In step 2, the groove is repaired by welding, and the repaired welding area higher than the surface of the cast iron part is polished until it is flush with the surface of the cast iron part. The repaired weld is checked to ensure that no defects such as lack of fusion, slag inclusion, undercut, surface pores, incomplete welding of weld nodules, and cracks are allowed. If the above defects occur, repeat step S1.

4. A heat treatment method for improving the mechanical properties of steel castings according to claim 3, characterized in that: In the step 3, the steel casting is heated to 450°C in a heat treatment furnace at a heating rate of 50°C / h-80°C / h, and then heated to 500°C-650°C at a heating rate of 80°C / h-120°C / h.

5. A heat treatment method for improving the mechanical properties of steel castings according to claim 4, characterized in that: In the step 4, the steel casting is cooled to 100° C.-200° C. in the heat treatment furnace together with the heat treatment furnace, and then the steel casting is taken out and placed in an aqueous solution, organic oil or air cooling box to cool down.

6. A heat treatment method for improving the mechanical properties of steel castings according to claim 5, characterized in that: The chemical composition of the steel casting and the mass percentage of each component element are as follows: C=0.12%, Si=0.20%, Mn=0.5%, P≤0.015%, S≤0.025%, Cr≤2.20%, Mo≤0.9%, Ni≤0.3%, V≤0.01%, Cu≤0.1%, and the rest are Fe and unavoidable impurity elements. The mechanical properties of the steel casting are tensile strength Rm=600-660MPa, yield strength Rp0.2=420-450MPa, elongation A=20%-24%, and section shrinkage Z=43%-50%.

7. A heat treatment method for improving the mechanical properties of steel castings according to claim 5, characterized in that: The chemical composition of the steel casting and the mass percentage of each component element are as follows: C=0.55%, Si=0.6%, Mn=1.0%, P≤0.015%, S≤0.025%, Cr≤2.20%, Mo≤0.9%, Ni≤0.3%, V≤0.01%, Cu≤0.1%, and the rest are Fe and unavoidable impurity elements. The mechanical properties of the steel casting are tensile strength Rm=620-680MPa, yield strength Rp0.2=422-470MPa, elongation A=25%-28%, and section shrinkage Z=50%-65%.