Method for improving surface roughness of nickel-based superalloy casting

A method for improving nickel-based high-temperature alloy casting surface roughness using a mirror spraying device with specific abrasives and parameters achieves efficient and cost-effective results, surpassing traditional methods in both efficiency and surface finish.

CN119057702APending Publication Date: 2024-12-03NANTONG HITECH PRECISION MATERIAL CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411292976.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-14
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Existing methods for improving the surface roughness of nickel-based high-temperature alloy castings, such as manual grinding, sand blasting, vibration grinding, abrasive flow, and electrolytic polishing, are inefficient, difficult to operate, costly, or environmentally harmful, and fail to achieve the desired surface finish effectively.

Method used

A method involving measuring the casting surface, setting spraying parameters, using specific abrasives, and employing a mirror spraying device with a handheld spray gun to perform rough and fine processing, achieving a surface roughness of Ra0.6 or less.

Benefits of technology

The method significantly improves processing efficiency while reducing costs and does not require high technical skills, requiring only the ability to operate a spray gun, and achieves a surface roughness that surpasses other methods, including sandblasting and abrasive flow.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119057702A_ABST
    Figure CN119057702A_ABST
Patent Text Reader

Abstract

The invention discloses a method for improving the surface roughness of a nickel-based superalloy casting. The method comprises the following specific steps that S1, the roughness of different parts of the surface of the casting is measured, and the different parts comprise a plane area, a deep hole and a slit; s2, jet process parameters are set, the jet pressure ranges from 0.4 mpa to 0.6 mpa, the rough machining jet time ranges from 2 minutes to 3 minutes, and the finish machining jet time ranges from 3 minutes to 4 minutes; s3, grinding materials are selected, rough machining grinding materials comprise 40-mesh rubber particles and 60-mesh diamonds, and finish machining grinding materials comprise 80-mesh rubber particles and 200-mesh diamonds; s4, the workpiece is fixed, mirror face spraying equipment is operated, a spray gun is held by hand to spray the part needing to be machined, and the distance between the spray gun and the machined surface is kept to be 40-80 mm; s5, surface processing; and S6, roughness measurement. The method for improving the surface roughness of the nickel-based high-temperature alloy casting has the advantages that the cost is reduced, and meanwhile the machining efficiency is greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of improving the surface roughness of castings, and in particular to a method for improving the surface roughness of nickel-based high-temperature alloy castings. Background Art

[0002] During the processing of nickel-based high-temperature alloy castings, it is necessary to adopt a rough processing and then fine processing process to reduce the surface roughness. The existing roughness improvement technologies are as follows:

[0003] 1. Manual grinding and polishing, using sandpaper, polishing agent, felt and other materials, purely manual or hand tools for grinding and polishing;

[0004] 2. Sand blasting: In the sand blasting equipment, sand is sprayed onto the surface of the parts by air pressure for cutting and polishing;

[0005] 3. Vibration grinding: In the grinding equipment, the surface of the parts is polished by the vibration of the abrasive;

[0006] 4. Abrasive flow: In abrasive flow equipment, the abrasive is squeezed and ground on the surface of the part to polish the part;

[0007] 5.Electrolytic polishing: polishing the surface of parts through electrochemical reaction.

[0008] At the same time, this technology has the following defects:

[0009] 1. Manual grinding and polishing is inefficient and difficult to operate in small spaces;

[0010] 2. Sand blasting has poor effect on improving roughness;

[0011] 3. Vibration grinding, low efficiency;

[0012] 4. Abrasive flow, high cost of equipment, tooling and abrasives;

[0013] 5. Electrolytic polishing, environmental pollution.

[0014] To this end, we provide a method for improving the surface roughness of nickel-based high-temperature alloy castings, aiming to improve the improvement efficiency and reduce the abrasive cost. Summary of the invention

[0015] The invention discloses a method for improving the surface roughness of a nickel-based high-temperature alloy casting, aiming to solve the technical problem of how to improve the improvement efficiency and reduce the abrasive cost.

[0016] In order to achieve the above object, the present invention adopts the following technical solutions:

[0017] A method for improving the surface roughness of a nickel-based high-temperature alloy casting comprises the following specific steps: S1: measuring the roughness of different parts of the casting surface, the different parts comprising a plane area, a deep hole and a slit; S2: setting the spraying process parameters, the spraying pressure is 0.4-0.6 MPa, the roughing spraying time is 2-3 minutes, and the fine processing spraying time is 3-4 minutes; S3: selecting abrasives, the roughing abrasives are 40 mesh rubber particles plus 60 mesh diamonds, and the fine processing abrasives are 80 mesh rubber particles plus 200 mesh diamonds; S4: fixing the workpiece, running a mirror spraying device, spraying the parts to be processed with a handheld spray gun, and keeping the spray gun 40-80 mm away from the processing surface; S5: surface processing, using the mirror spraying device to perform rough processing on the surface once and then fine processing on the surface once; S6: measuring the roughness and comparing it with the roughness before processing.

[0018] This method for improving the surface roughness of nickel-based high-temperature alloy castings is simple to operate and does not require high technical skills for the operator. It only requires starting the spray gun and aiming it at the surface to be processed for sandblasting. Compared with manual grinding, abrasive flow and electrolytic polishing, the operating skills required are lower. At the same time, it can greatly improve the processing efficiency while reducing costs. Compared with other methods, the processing time can be greatly shortened, while the processing time of manual grinding, abrasive flow and vibration grinding is longer, which is 5-10 times that of this spray processing method. At the same time, the surface roughness of nickel-based high-temperature alloy castings improved by this method is good, and the roughness after processing can reach below Ra0.6, which cannot be achieved by sandblasting, vibration grinding and abrasive flow.

[0019] In a preferred embodiment, the mirror spraying equipment in S4 includes an equipment shell, and a window and a glove are arranged on one side of the equipment shell, a sealing door is arranged on the inner wall on the same side of the equipment shell, a clamping mechanism and a cleaning mechanism are arranged in the equipment shell at the same time, and the clamping mechanism and the cleaning mechanism are connected, a guide groove is fixedly connected to the bottom end of the equipment shell, the guide groove is located at the bottom end of the clamping mechanism and the cleaning mechanism, a negative pressure pipe is arranged in the middle position of the guide groove, and a spray gun is connected to the top of the negative pressure pipe, a support frame is fixedly connected to the inner wall of one side of the equipment shell, and the spray gun is clamped on the support frame, the clamping mechanism includes two clamping frames, and grid plates are inserted in the middle of the two clamping frames at the same time, and the opposite sides of the grid plates are respectively fixedly connected to the inner wall of the equipment shell through a connecting frame, and the inner walls of the opposite sides of the two clamping frames are respectively provided with clamping seats, and the two clamping seats are fitted and clamped on both sides of the workpiece, and the bottom end of each of the clamping frames is respectively fixedly connected to a side support plate, and the outer walls of the opposite sides of the two side support plates are respectively connected to The cam is provided with a plurality of grooves on one side of the inner wall of the arc surface and a plurality of grooves on the other side of the arc surface, and a plurality of grooves are provided in the grooves.

[0020] By connecting an arc-surface rebound plate and a bottom rebound plate on the same side of the clamping frame, the abrasive rebounded during the grinding process can be rebounded back to the workpiece surface for a second time, thereby improving the grinding efficiency. When the arc-surface rebound plate is vertical, it can be used for regular workpieces with smooth surfaces. The rebounded abrasive pops out laterally and rebounds to the side of the workpiece through the arc-surface rebound plate for a second time. When the arc-surface rebound plate is inclined inward, it can be used for irregular workpieces or workpieces with uneven surfaces. The abrasive rebounded through the concave part pops out upward and rebounds back to the workpiece surface after contacting the arc-surface rebound plate obliquely above, thereby optimizing the adaptability of the arc-surface rebound plate.

[0021] In a preferred embodiment, the cleaning mechanism includes an inclined groove, and the outer wall of the inclined groove is fixedly connected to a plurality of slide seats, each of the slide seats is movably connected to a slide rail, and the slide rail is fixed to the inner wall of the equipment housing, the inner wall of the inclined groove is fixedly connected to two gear rods, and the gear rod arranged on the outer side is lower than the gear rod on the inner side, one side outer wall of the inclined groove is fixedly connected to a linkage plate, and an L-shaped clamping groove is arranged at the bottom end of the linkage plate, a clamping frame is movably clamped in the L-shaped clamping groove, and the clamping frame is installed on one side of the collet basket, one side outer wall of the linkage plate is fixedly connected to a second support rod, and one end of the second support rod is hinged to a first hinged rod, the other end of the first hinged rod is hinged to a second hinged rod, and the second hinged rod is movably connected to the second support plate, and one side of the second support plate is fixedly connected to a stepping motor The machine is a machine, and the output end of the stepping motor is connected to the second hinge rod through the second support plate, the outer wall of the second support plate is fixedly connected to the limiting sleeve, and the limiting sleeve is movably sleeved on the outside of the second support rod, the outer walls on the opposite sides of the collet basket are respectively fixedly connected to the third support plates, and the third support plate is inlaid with a permanent magnet block, wherein the positive pole of the permanent magnet block faces upward and the negative pole faces downward, the inner wall of the device shell is fixedly connected to two second mounting frames, and the two second mounting frames are respectively located on both sides of the collet basket, the upper and lower inner walls of the second mounting frames are respectively inlaid with guide electromagnetic blocks, and the positive pole of the guide electromagnetic block faces downward and the negative pole faces upward, the guide electromagnetic block is composed of a plurality of electromagnet blocks, the magnetic force of the upper guide electromagnetic block decreases from the middle to both ends, and the magnetic force of the lower guide electromagnetic block increases from the middle to both ends.

[0022] A cleaning mechanism is provided, wherein the cleaning mechanism is used for cleaning abrasives on the workpiece. Through the setting of the gear lever, the workpiece can be turned over, and the abrasives blocked on different surfaces can be made to fall down, thereby realizing multi-faceted cleaning. At the same time, under the rotation of the stepper motor, the inclined slot and the collet basket can be driven to reciprocate at the same time, so that during the falling process of the workpiece, the stuck abrasive can be better separated from the groove of the workpiece through shaking and impact. The guiding electromagnet is composed of a plurality of electromagnet blocks. During the shaking process of the collet basket, based on the setting of the permanent magnet blocks on both sides of the collet basket, the permanent magnet blocks and the electromagnet blocks can be made not to contact each other, while ensuring that the stepper motor drives the collet basket to translate smoothly, it also prevents the abrasives from clogging the sliding path and causing jamming. In addition, the magnetic force of the electromagnet block is set to increase or decrease. During the translation process, as the magnetic force changes, the collet basket can also be shaken up and down to increase the vibration intensity, thereby better realizing the filtering of the abrasive in the collet basket.

[0023] From the above, it can be seen that a method for improving the surface roughness of a nickel-based high-temperature alloy casting includes the following specific steps: S1: measuring the roughness of different parts of the casting surface, including plane areas, deep holes, and slits; S2: setting the spraying process parameters, the spraying pressure is 0.4-0.6 MPa, the roughing spraying time is 2-3 minutes, and the finishing spraying time is 3-4 minutes; S3: selecting abrasives, roughing abrasives: 40 mesh rubber particles plus 60 mesh diamonds, finishing abrasives: 80 mesh rubber particles plus 200 mesh diamonds; S4: fixing the workpiece, running the mirror spraying equipment, spraying the parts to be processed with a handheld spray gun, and keeping the spray gun 40-80 mm away from the processing surface; S5: surface processing, using the mirror spraying equipment to roughen the surface once, and then finish the surface once; S6: roughness measurement, and comparing with the roughness before processing. The method for improving the surface roughness of a nickel-based high-temperature alloy casting provided by the present invention has the technical effect of greatly improving the processing efficiency while reducing the cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 The present invention provides an overall flow chart of a method for improving the surface roughness of a nickel-based high-temperature alloy casting.

[0025] Figure 2 A schematic diagram of the overall appearance structure of a mirror spraying device for a method of improving the surface roughness of a nickel-based high-temperature alloy casting proposed in the present invention.

[0026] Figure 3 A schematic diagram of the internal structure of a mirror spraying device for a method of improving the surface roughness of a nickel-based high-temperature alloy casting proposed in the present invention.

[0027] Figure 4 A schematic diagram of the connection structure of a clamping mechanism and a cleaning mechanism of a mirror spraying device for a method for improving the surface roughness of a nickel-based high-temperature alloy casting proposed by the present invention.

[0028] Figure 5 A schematic structural diagram of a clamping mechanism of a mirror spraying device for a method of improving the surface roughness of a nickel-based high-temperature alloy casting proposed in the present invention.

[0029] Figure 6 A schematic diagram of the disassembled structure of the clamping mechanism of the mirror spraying equipment for the method of improving the surface roughness of nickel-based high-temperature alloy castings proposed by the present invention.

[0030] Figure 7 A schematic diagram of the disassembled structure of a cleaning mechanism of a mirror spraying device for a method of improving the surface roughness of a nickel-based high-temperature alloy casting proposed in the present invention.

[0031] Figure 8This is a schematic diagram of the other side of the disassembled structure of the cleaning mechanism of the mirror spraying equipment of the method for improving the surface roughness of nickel-based high-temperature alloy castings proposed by the present invention.

[0032] Fig. 9 A schematic diagram of the guiding electromagnet structure of a mirror spraying device for a method for improving the surface roughness of a nickel-based high-temperature alloy casting proposed in the present invention.

[0033] In the figure: 1, equipment housing; 2, window; 3, clamping mechanism; 4, cleaning mechanism; 5, sealing door; 6, gloves; 7, grid plate; 8, connecting frame; 9, guide groove; 10, negative pressure pipe; 11, support frame; 12, spray gun; 301, arc rebound plate; 302, outer cover; 303, bottom rebound plate; 304, connecting block; 305, clamping frame; 306, side support plate; 307, two-way gas rod; 308, first mounting frame; 309, clamping seat; 310, damping connecting rod group; 311, handle; 312, groove; 313, limit slide groove; 314, limit slide block; 315, first support rod; 316, curved fixing plate; 317, fixing groove; 318, screw; 401, second support plate; 402, first hinge rod; 403, second hinge rod; 404, stepper motor; 405, second support rod; 406, inclined groove; 407, shift rod; 408, second mounting bracket; 409, guide electromagnet; 410, third support plate; 411, collet basket; 412, permanent magnet block; 413, slide rail; 414, slide seat; 415, clamping frame; 416, L-shaped clamping groove; 417, limit sleeve; 418, linkage plate; 419, electromagnet block. DETAILED DESCRIPTION

[0034] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.

[0035] A method for improving the surface roughness of a nickel-based high-temperature alloy casting disclosed in the present invention is mainly used in the scenario of improving the surface roughness of a nickel-based high-temperature alloy casting.

[0036] Reference Figure 1A method for improving the surface roughness of a nickel-based high-temperature alloy casting comprises the following specific steps: S1: measuring the roughness of different parts of the casting surface, the different parts including a plane area, a deep hole, and a slit; S2: setting the spraying process parameters, the spraying pressure is 0.4-0.6 MPa, the roughing spraying time is 2-3 minutes, and the fine processing spraying time is 3-4 minutes; S3: selecting abrasives, the roughing abrasives are 40 mesh rubber particles plus 60 mesh diamonds, and the fine processing abrasives are 80 mesh rubber particles plus 200 mesh diamonds; S4: fixing the workpiece, running the mirror spraying equipment, spraying the parts to be processed with a handheld spray gun, and keeping the spray gun 40-80 mm away from the processing surface; S5: surface processing, using the mirror spraying equipment to perform rough processing on the surface once and then fine processing on the surface once; S6: roughness measurement, and comparing with the roughness before processing.

[0037] Reference Figure 2-Figure 4 In a preferred embodiment, the mirror spraying device in S4 includes an equipment housing 1, and a window 2 and a glove 6 are provided on one side of the equipment housing 1, a sealing door 5 is provided on the inner wall on the same side of the equipment housing 1, a clamping mechanism 3 and a cleaning mechanism 4 are provided in the equipment housing 1, and the clamping mechanism 3 and the cleaning mechanism 4 are connected, and a guide groove 9 is fixedly connected to the bottom end of the equipment housing 1, and the guide groove 9 is located at the bottom end of the clamping mechanism 3 and the cleaning mechanism 4.

[0038] Reference Figure 2-Figure 4 In a preferred embodiment, a negative pressure pipe 10 is provided in the middle position of the guide groove 9, and a spray gun 12 is connected to the top end of the negative pressure pipe 10, a support frame 11 is fixedly connected to the inner wall of one side of the equipment housing 1, and the spray gun 12 is clamped on the support frame 11.

[0039] Reference Figure 4 and Figure 5 In a preferred embodiment, the clamping mechanism 3 includes two clamping frames 305, and a grid plate 7 is inserted in the middle of the two clamping frames 305. The opposite sides of the grid plate 7 are fixedly connected to the inner wall of the equipment housing 1 through a connecting frame 8. The inner walls of the opposite sides of the two clamping frames 305 are respectively provided with clamping seats 309, and the two clamping seats 309 are clamped on both sides of the workpiece. The bottom end of each clamping frame 305 is respectively fixedly connected with a side support plate 306, and the outer walls of the opposite sides of the two side support plates 306 are respectively connected to the two output ends of the bidirectional gas rod 307, and the middle section of the bidirectional gas rod 307 is fixedly connected to the bottom end of the grid plate 7 through a first mounting frame 308.

[0040] Reference Figure 5 and Figure 6In a preferred embodiment, the outer wall of the same side of each clamping frame 305 is fixedly connected with a fixing groove 317 through a connecting block 304, and a plurality of screw holes are provided on one side of the fixing groove 317, each screw hole is respectively engaged with a screw 318, and each fixing groove 317 is respectively clamped with an arc surface fixing plate 316, and one end of the screw 318 is pressed on one side of the arc surface fixing plate 316. The two clamping frames 305 are driven to move inward to clamp the workpiece by the telescopic movement of the bidirectional gas rod 307 in the clamping mechanism 3, and By replacing the clamping seat 309, it can adapt to the use of workpieces of different specifications. By connecting the arc rebound plate 301 and the bottom rebound plate 303 on the same side of the clamping frame 305, the abrasive rebounded during the grinding process can be rebounded back to the workpiece surface for a second time, thereby improving the grinding efficiency. The arc fixing plate 316 is clamped by the screw 318, and the arc fixing plate 316 is clamped by the fixing groove 317. The position of the entire rebound structure can be changed according to different workpiece diameters to ensure the normal use of the rebound structure.

[0041] Reference Figure 5 and Figure 6 In a preferred embodiment, the top of the arc fixed plate 316 is fixedly connected to the bottom rebound plate 303, the top of the bottom rebound plate 303 is fixedly connected to multiple first support rods 315, and the two ends of each first support rod 315 are respectively fixedly connected to the limiting slider 314, and the top of the bottom rebound plate 303 is movably connected to the arc rebound plate 301.

[0042] Reference Figure 5 and Figure 6 In a preferred embodiment, a plurality of grooves 312 are arranged on the inner wall of one side of the arc rebound plate 301, and a limiting slide groove 313 is arranged in the groove 312, and a limiting slide block 314 is movably connected to the limiting slide groove 313, and each groove 312 is respectively covered with an outer cover 302, and the outer wall of the same side of the arc rebound plate 301 and the bottom rebound plate 303 is hinged with a damping link group 310 at the same time, and a handle 311 is arranged at the hinge of the damping link group 310. In addition, under the support and clamping action of the first support rod 315 and the setting of the back damping link group 310, the arc The arc rebound plate 301 can be pulled up and the angle of the damping link group 310 can be changed to make the arc rebound plate 301 tilted inward. Therefore, when the arc rebound plate 301 is vertical, it can be used for regular and smooth workpieces. The abrasive that is rebounded will pop out laterally and rebound to the side of the workpiece through the arc rebound plate 301 for a second time. When the arc rebound plate 301 is tilted inward, it can be used for irregular or uneven workpieces. The abrasive that rebounds through the concave part will pop out upward and rebound to the surface of the workpiece after contacting the arc rebound plate 301 obliquely above, thereby optimizing the adaptability of the arc rebound plate 301.

[0043] Reference Figure 7and Figure 8 In a preferred embodiment, the cleaning mechanism 4 includes an inclined groove 406, and the outer wall of the inclined groove 406 is fixedly connected to a plurality of slide seats 414, each slide seat 414 is movably connected to a slide rail 413, and the slide rail 413 is fixed to the inner wall of the device housing 1, and the inner wall of the inclined groove 406 is fixedly connected to two gear rods 407, and the gear rod 407 arranged on the outer side is lower than the gear rod 407 on the inner side, and the outer wall of one side of the inclined groove 406 is fixedly connected to a linkage plate 418, and the bottom end of the linkage plate 418 is provided with an L-shaped card The connecting groove 416 has a connecting frame 415 movably connected in the L-shaped connecting groove 416, and the connecting frame 415 is installed on one side of the collet 411, wherein the cleaning mechanism is used for cleaning the abrasive on the workpiece, and through the setting of the shift rod 407, when the workpiece is polished and removed and placed on the inclined groove 406, it moves downward along the inclined surface of the inclined groove 406, and when it contacts the shift rod 407, it can be turned over under the action of the shift rod 407, so that during the turning process, the abrasive blocked on different surfaces can fall down, thereby realizing multi-faceted cleaning.

[0044] Reference Figure 7 and Figure 8 In a preferred embodiment, a second support rod 405 is fixedly connected to an outer wall of one side of the linkage plate 418, and one end of the second support rod 405 is hinged to the first hinge rod 402, and the other end of the first hinge rod 402 is hinged to the second hinge rod 403, and the second hinge rod 403 is movably connected to the second support plate 401, a stepper motor 404 is fixedly connected to one side of the second support plate 401, and the output end of the stepper motor 404 passes through the second support plate 401 and is connected to the second hinge rod 403, the outer wall of the second support plate 401 is fixedly connected to a limiting sleeve 417, and the limiting sleeve 417 is movably sleeved on the outside of the second support rod 405, and at the same time Under the rotation action of the stepper motor 404, the second hinged rod 403 is driven to rotate, and at the same time, through the hinge with the first hinged rod 402, the displacement of the other end of the first hinged rod 402 is used to drive the second support rod 405 to move forward and backward along the limit sleeve 417, and then through the connection of the linkage plate 418, the inclined groove 406 and the collet basket 411 are driven to reciprocate at the same time, so that during the falling process of the workpiece, the stuck abrasive can be better separated from the workpiece groove through shaking and impact. The connection with the collet basket 411 is established by means of the L-shaped clamping groove 416, which can facilitate the installation of the collet basket 411 and also assist the subsequent use of the guiding electromagnet 409.

[0045] Reference Figure 7 and Fig. 9In a preferred embodiment, the outer walls of the two opposite sides of the collet basket 411 are respectively fixedly connected with the third support plate 410, and the third support plate 410 is inlaid with a permanent magnet block 412, wherein the positive pole of the permanent magnet block 412 faces upward and the negative pole faces downward, and the inner wall of the device housing 1 is fixedly connected with two second mounting frames 408, and the two second mounting frames 408 are respectively located on both sides of the collet basket 411, and the upper and lower inner walls of the second mounting frames 408 are respectively inlaid with guide electromagnetic blocks 409, and the positive pole of the guide electromagnetic block 409 faces downward and the negative pole faces upward. The guide electromagnetic block 409 is composed of a plurality of electromagnet blocks 419, and the magnetic force of the guide electromagnetic block 409 located at the top is from the middle to both ends. The magnetic force of the guiding electromagnet block 409 located at the bottom increases from the middle to both ends. Based on the fact that the guiding electromagnet 409 is composed of a plurality of electromagnet blocks 419, during the shaking of the collet basket 411, based on the setting of the permanent magnet blocks 412 on both sides of the collet basket, the permanent magnet blocks 412 and the electromagnet blocks 419 can be prevented from contacting each other, while ensuring that the stepper motor 404 drives the collet basket 411 to translate smoothly, it also prevents the abrasive from being blocked in the sliding path and causing jamming. In addition, the magnetic force of the electromagnet block 419 is set to increase or decrease. During the translation process, as the magnetic force changes, the collet basket 411 can also be shaken up and down to increase the vibration intensity, thereby better realizing the filtering of the abrasive in the collet basket 411.

[0046] Example:

[0047] Fix the workpiece, use the mirror spray equipment to rough-process the surface once, and then fine-process the surface once. For rough processing, use 40-mesh rubber particles plus 60-mesh diamonds. Set the spray process parameters to spray pressure 0.4-0.6mpa and spray time 2-3 minutes;

[0048] For finishing, 80-mesh rubber particles and 200-mesh diamonds were used, and the spraying process parameters were set to spray pressure 0.4-0.6 MPa and spray time 3-4 minutes;

[0049] The roughness was measured and compared with the roughness before processing. The comparison results are as follows: The roughness of the workpiece before spraying was Ra0.9-1.3, and after spraying it reached Ra0.4-0.5, which is a significant improvement.

[0050] Location 1 2 3 4 5 Before injection Ra1.1 Ra0.9 Ra1.3 Ra1.1 Ra0.9 After injection Ra0.4 Ra0.4 Ra0.5 Ra0.4 Ra0.5

[0051] The following is the data of abrasive flow machining of workpieces made of the same material:

[0052] Location 1 2 3 4 5 Before injection Ra1.2 Ra1.3 Ra1.0 Ra0.9 Ra0.9 After injection Ra0.7 Ra0.7 Ra0.6 Ra0.7 Ra0.5

[0053] Comparison conclusion:

[0054] Using workpieces of the same material and surface roughness, the total time for jetting is 10 minutes, and the total time for abrasive flow machining is 60 minutes. Jet machining can achieve better roughness effect.

[0055] Working principle: This method of improving the surface roughness of nickel-based high-temperature alloy castings is simple to operate and does not require high technical skills for operators. You only need to start the spray gun and aim it at the surface to be processed for sandblasting. Compared with manual grinding, abrasive flow and electrolytic polishing, it requires lower operating skills. By mixing rubber particles with diamonds as abrasives, when the abrasive acts on the workpiece surface under the action of the spray gun, the mixed rubber particles and diamonds are evenly ejected. When they come into contact with the surface of the nickel-based high-temperature alloy casting, in addition to rebounding on the surface of the nickel-based high-temperature alloy casting, during the rebound process, the rubber particles come into contact with the diamonds. Under the action of rubber particles, diamonds can be provided with a certain resilience, so that part of the diamonds can act on the surface of nickel-based high-temperature alloy castings for a second time, thereby greatly improving processing efficiency while reducing costs. Compared with other methods, the processing time can be greatly shortened, while manual grinding, abrasive flow, and vibration grinding have a longer processing time, which is 5-10 times that of this jet processing method. At the same time, the surface roughness of nickel-based high-temperature alloy castings improved by this method is good, and the roughness after processing can reach below Ra0.6, which cannot be achieved by sandblasting, vibration grinding, and abrasive flow.

[0056] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for improving the surface roughness of nickel-based high-temperature alloy castings, It is characterized in that The specific steps include: S1: Measure the roughness of different parts of the casting surface, including flat areas, deep holes, and narrow gaps; S2: Set the injection process parameters, injection pressure 0.4-0.6 MPa, roughing injection time 2-3 minutes, and finishing injection time 3-4 minutes; S3: Select abrasives, rough processing abrasives: 40 mesh rubber particles plus 60 mesh diamonds, fine processing abrasives: 80 mesh rubber particles plus 200 mesh diamonds; S4: Fix the workpiece, operate the mirror spraying equipment, hold the spray gun to spray the part to be processed, and keep the spray gun 40-80mm away from the processing surface; S5: Surface processing, using mirror spraying equipment to rough-process the surface once and then fine-process the surface once; S6: Roughness measurement, compared with the roughness before processing.

2. A method for improving the surface roughness of a nickel-based high-temperature alloy casting according to claim 1, It is characterized in that The mirror spraying device in S4 comprises a device housing (1), and a window (2) and a glove (6) are arranged on one side of the device housing (1); a sealing door (5) is arranged on the inner wall on the same side of the device housing (1); a clamping mechanism (3) and a cleaning mechanism (4) are arranged in the device housing (1), and the clamping mechanism (3) and the cleaning mechanism (4) are connected; a guide groove (9) is fixedly connected to the bottom end of the device housing (1), and the guide groove (9) is located at the bottom ends of the clamping mechanism (3) and the cleaning mechanism (4).

3. A method for improving the surface roughness of a nickel-based high-temperature alloy casting according to claim 2, It is characterized in that A negative pressure pipe (10) is arranged in the middle of the guide groove (9), and a spray gun (12) is connected to the top end of the negative pressure pipe (10); a support frame (11) is fixedly connected to an inner wall of one side of the device housing (1), and the spray gun (12) is clamped on the support frame (11).

4. A method for improving the surface roughness of a nickel-based high-temperature alloy casting according to claim 2, It is characterized in that The clamping mechanism (3) comprises two clamping frames (305), and a grid plate (7) is inserted in the middle of the two clamping frames (305). The opposite sides of the grid plate (7) are fixedly connected to the inner wall of the equipment housing (1) through a connecting frame (8). The inner walls of the two clamping frames (305) on the opposite sides are respectively provided with clamping seats (309), and the two clamping seats (309) are clamped on the two sides of the workpiece. The bottom end of each clamping frame (305) is respectively fixedly connected to a side support plate (306), and the outer walls on the opposite sides of the two side support plates (306) are respectively connected to the two output ends of the bidirectional gas rod (307), and the middle section of the bidirectional gas rod (307) is fixedly connected to the bottom end of the grid plate (7) through a first mounting frame (308).

5. A method for improving the surface roughness of a nickel-based high-temperature alloy casting according to claim 4, It is characterized in that The outer wall of the same side of each clamping frame (305) is fixedly connected to a fixing groove (317) via a connecting block (304), and a plurality of screw holes are provided on one side of the fixing groove (317), each of which is respectively engaged with a screw (318), and each of which is respectively clamped with an arc-surface fixing plate (316), and one end of the screw (318) is pressed against one side of the arc-surface fixing plate (316).

6. A method for improving the surface roughness of a nickel-based high-temperature alloy casting according to claim 5, It is characterized in that The top of the arc surface fixed plate (316) is fixedly connected to the bottom rebound plate (303), the top of the bottom rebound plate (303) is fixedly connected to a plurality of first support rods (315), and both ends of each first support rod (315) are respectively fixedly connected to a limiting slider (314), and the top of the bottom rebound plate (303) is movably connected to the arc surface rebound plate (301).

7. A method for improving the surface roughness of a nickel-based high-temperature alloy casting according to claim 6, It is characterized in that A plurality of grooves (312) are arranged on an inner wall of one side of the arc rebound plate (301), and a limiting slide groove (313) is arranged in the groove (312), the limiting slider (314) is movably connected in the limiting slide groove (313), and each groove (312) is respectively covered with an outer cover (302), and a damping connecting rod group (310) is hingedly connected to the outer wall of the same side of the arc rebound plate (301) and the bottom rebound plate (303), and a handle (311) is arranged at the hinge of the damping connecting rod group (310).

8. A method for improving the surface roughness of a nickel-based high-temperature alloy casting according to claim 2, It is characterized in that The cleaning mechanism (4) comprises an inclined groove (406), and the outer wall of the inclined groove (406) is fixedly connected to a plurality of slide seats (414), each of the slide seats (414) is movably connected to a slide rail (413), and the slide rail (413) is fixed to the inner wall of the equipment housing (1), the inner wall of the inclined groove (406) is fixedly connected to two shift rods (407), and the shift rod (407) arranged on the outer side is lower than the shift rod (407) on the inner side, one side outer wall of the inclined groove (406) is fixedly connected to a linkage plate (418), and the bottom end of the linkage plate (418) is provided with an L-shaped clamping groove (416), and a clamping frame (415) is movably clamped in the L-shaped clamping groove (416), and the clamping frame (415) is installed on one side of the drain basket (411).

9. A method for improving the surface roughness of a nickel-based high-temperature alloy casting according to claim 8, It is characterized in that A second support rod (405) is fixedly connected to an outer wall of one side of the linkage plate (418), and one end of the second support rod (405) is hinged to a first hinge rod (402), and the other end of the first hinge rod (402) is hinged to a second hinge rod (403), and the second hinge rod (403) is movably connected to the second support plate (401), and a stepper motor (404) is fixedly connected to one side of the second support plate (401), and the output end of the stepper motor (404) passes through the second support plate (401) and is connected to the second hinge rod (403), and the outer wall of the second support plate (401) is fixedly connected to a limiting sleeve (417), and the limiting sleeve (417) is movably sleeved outside the second support rod (405).

10. A method for improving the surface roughness of a nickel-based high-temperature alloy casting according to claim 9, It is characterized in that The outer walls of the colander (411) on both sides facing each other are fixedly connected with third support plates (410), and the third support plates (410) are embedded with permanent magnet blocks (412), wherein the positive pole of the permanent magnet block (412) faces upward and the negative pole faces downward. The inner wall of the device housing (1) is fixedly connected with two second mounting frames (408), and the two second mounting frames (408) are respectively located on both sides of the colander (411). The upper and lower inner walls of the second mounting frames (408) are respectively embedded with guide electromagnetic blocks (409), and the positive pole of the guide electromagnetic block (409) faces downward and the negative pole faces upward. The guide electromagnetic block (409) is composed of a plurality of electromagnet blocks (419) spliced ​​together. The magnetic force of the upper guide electromagnetic block (409) decreases from the middle to both ends, and the magnetic force of the lower guide electromagnetic block (409) increases from the middle to both ends.

Citation Information

Patent Citations

  • Method and system for improving surface roughness of casting

    CN112276800A

  • Method for improving surface smoothness of artificial joint casting

    CN113305740A

  • Composite diamond wheel system in lens processing machine

    KR102309539B1

  • Method for surface treatment of workpiece made from hard-brittle material

    US20190283212A1