Method for preparing oil absorption material from waste masks and straw
By combining waste masks and straw to form efficient oil-absorbing materials, the problems of insufficient structural strength and high cost of existing oil-absorbing materials are solved, and stable oil-absorbing and reusable in fluctuating water are achieved, reducing the risk of environmental pollution.
Patent Information
- Application Number
- CN202411336550.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-24
- Publication Date
- 2024-12-03
AI Technical Summary
When dealing with oil pollution, existing oil-absorbing materials have problems such as insufficient structural strength, high cost, difficulty in reusing and poor stability in fluctuating water, and commonly used chemical methods can pollute the environment.
The polypropylene fibers of the discarded mask are combined with straw, and the flakes are treated and crushed by surfactant to form a sheet material, which improves the specific surface area and structural stability of the oil-absorbing material, and makes it reusable by extrusion.
It achieves low-cost and efficient oil absorption, the material remains stable in fluctuating water, has a high oil absorption rate and is reusable, reducing the risk of environmental pollution.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of waste resource utilization and oilfield pollutant treatment application, and in particular to a method for preparing an oil-absorbing material by using waste masks and straws. Background Art
[0002] At present, the overall level of oil spill emergency management in countries around the world is low, and the common methods for dealing with oil pollution include physical adsorption, chemical treatment, in situ combustion and biotechnology. Among these different methods, chemical methods contain toxic chemicals and will pollute the marine environment, so the use of chemical methods will waste resources. Among them, physical methods are easy to operate and have the advantages of low production cost, easy manufacturing, high selectivity, environmental friendliness and recyclability, but the recovery cost is high, and there are requirements for the thickness of the oil layer, and the oil spill treatment is not thorough. So far, different polymers have been used as oil absorbent materials, such as foam, fiber, sponge and aerogel.
[0003] Oil pollutants originate from the leakage of oil and organic solvents. They have a certain stability in organisms or environmental systems and are difficult to be decomposed and degraded, thus causing certain health problems for animals and plants. It is essential to separate oil and organic solvents from water in order to meet the emission regulations set by environmental authorities. Adsorption is considered to be one of the best processes for oil-water separation because of its low operating and capital costs and high separation efficiency. New and efficient adsorbent materials should not only have high adsorption capacity, good hydrophobicity, good suspension and good oil retention, but also be recyclable and naturally degradable.
[0004] Commonly used synthetic polymer fiber materials have strong oil absorption capacity, but they have low structural strength, are too soft, are easily broken up in fluctuating water, and have strong adsorption of oil pollutants, are not easy to reuse, and have high overall costs. Plant straw has the advantages of being natural, environmentally friendly, and low cost, but its straw fiber has weak oil absorption capacity, has a rigid loose structure, and is not easy to form a mass. If used in fluctuating water, it is easy to be broken up and difficult to collect.
[0005] Therefore, there is an urgent need to develop an oil-absorbing material that has suitable structural strength, is not easily broken up in turbulent water, has strong adsorption capacity for oil pollutants, and is low in cost. Summary of the invention
[0006] The object of the present invention is to provide a method for preparing an oil-absorbing material from discarded masks and straw by combining the advantages of polypropylene fibers of discarded masks and straw, which has good stability, is reusable and has low cost.
[0007] The present invention adopts the following technical solution: a method for preparing an oil-absorbing material using discarded masks and straw, which comprises the following steps, wherein there is no order requirement for the execution of steps 1 to 3:
[0008] Step 1: Remove the nose bridge and ear straps from the recycled discarded masks, disinfect them with 75% alcohol, dry them and cut them into 3-5cm pieces;
[0009] Step 2: At room temperature, cut the straw into 1-2 cm, soak it in 1-5% alkaline aqueous solution for more than 1 hour, remove it and dry it for later use;
[0010] Step 3: preparing a surface wetting agent aqueous solution with a total concentration of 0.5-3% by adding water to a polyether surfactant, an ammonium oxide surfactant and a quaternary ammonium salt surfactant in a mass ratio of 1:2-5:3-6;
[0011] Step 4: placing the cut mask described in step 1 in a wall breaking machine, adding the surface wetting agent aqueous solution configured in step 3, and crushing at 100-300 rpm for more than 2 minutes; then adding the cut straw described in step 2, the mass ratio of the added cut mask, the surface wetting agent aqueous solution, and the cut straw is 1:1-3:1-3, and continuing to crush at 100-300 rpm for more than 2 minutes, the obtained product is extruded at a pressure of more than 4 MPa for more than 6 minutes to form a sheet material, and the sheet material is placed at 60-75° C. and dried to obtain the oil absorption material prepared by using discarded masks and straw.
[0012] The present invention uses discarded polypropylene-based masks and crop straw as basic materials to prepare low-cost, efficient oil-absorbing, and structurally stable oil-absorbing materials. On the one hand, the fine fibers of polypropylene in the mask can be attached to the rough and crude fibers of the straw, so that the polypropylene fibers can maintain a relatively fluffy state, increase the specific surface area of the oil-absorbing material, and are more conducive to the absorption and storage of oils, greatly improving the oil absorption efficiency. On the other hand, the winding of the polypropylene fibers can bind the rough and crude fibers of the straw together, solving the problem that the straw material is loose and difficult to collect, and the oil-absorbing material can still maintain a stable structure even in water under an undulating state. At the same time, the oil-absorbing material prepared by the present invention can be reused after squeezing out the oil after absorbing oil once, greatly improving the market competitiveness.
[0013] Furthermore, the discarded masks are used masks produced from polypropylene fiber non-woven fabric materials, thus realizing waste utilization.
[0014] Furthermore, the straw in step 2 is straw of one or a mixture of two or more of the following crops: wheat, rice, corn or sorghum.
[0015] Furthermore, the step 20 is included before the step 2, and the step 20 is specifically: dissolving an alkali reagent in water to prepare an alkali aqueous solution with a concentration of 1-5%, wherein the alkali reagent is sodium hydroxide or potassium hydroxide of industrial grade or higher purity, and the water used to dissolve the alkali reagent is tap water of industrial grade or higher purity, or deionized water. Since the surface of the straw is too smooth, it is not conducive to the interaction with the fiber. By soaking the straw in alkaline water, the colloid dissolved by the alkali on the surface of the straw is removed, so that the polypropylene fiber is easy to attach to the surface of the straw.
[0016] Furthermore, in step 3, the polyether surfactant is one of the following: polyethylene glycol with a degree of polymerization of 200 or more or polypropylene glycol with a degree of polymerization of 200 or more.
[0017] Furthermore, in step 3, the ammonium oxide surfactant is one of the following: dodecyl ammonium oxide, tetradecyl ammonium oxide, hexadecyl ammonium oxide, or octadecyl ammonium oxide.
[0018] Further, in step 3, the quaternary ammonium surfactant is one of the following: dodecyl trimethyl ammonium chloride, tetradecyl trimethyl ammonium chloride, hexadecyl trimethyl ammonium chloride, or octadecyl trimethyl ammonium chloride. The present invention promotes the rigid structure of the straw material and the flexible structure of the polypropylene fiber to be closely combined and entangled by adding a surfactant, thereby greatly improving the structural stability of the prepared oil-absorbing material. At the same time, the ammonium oxide surfactant can improve the hydrophobicity of the straw surface, the quaternary ammonium surfactant can improve the lipophilicity of the straw surface, and the three active materials of the polyether surfactant, the ammonium oxide surfactant and the quaternary ammonium surfactant are used in combination to enhance the oil absorption of the straw and improve the interaction between the straw and the polypropylene fiber.
[0019] Furthermore, in step 3, the water used to dissolve the surfactant is industrial grade or above tap water, or deionized water.
[0020] Furthermore, in step 4, the obtained product is squeezed at a pressure of 4-7 MPa for 6-15 minutes into a sheet material, so as to facilitate storage, transportation, use and collection of the product. At the same time, the sheet product is also convenient for covering the crude oil layer floating on the water surface, so as to facilitate the absorption of crude oil.
[0021] When used, the oil absorbing material is put into the oil-containing water. After 10-30 minutes of adsorption, the oil absorbing material is picked up, and the oil absorption effect on marine oil spills, oil field wastewater discharge, etc. can be achieved. The oil absorption rate reaches 9.0g / g (each 1g of oil absorbing material can absorb 9.0g of oil) or more.
[0022] The beneficial effects of the present invention are:
[0023] The present invention uses discarded polypropylene-based masks and crop straw as basic materials to prepare low-cost oil-absorbing materials. On the one hand, the fine fibers of polypropylene in the mask can be attached to the rough fibers of the straw, so that the polypropylene fibers can remain in a relatively fluffy state, increasing the specific surface area of the oil-absorbing material, which is more conducive to the absorption and storage of oils and greatly improving the oil absorption efficiency. On the other hand, the winding of the polypropylene fibers can bind the rough fibers of the straw together, solving the problem that the straw material is loose and difficult to collect, and the oil-absorbing material can still maintain a stable structure even in water under a fluctuating state.
[0024] The invention combines the advantages of the rigid structure of the straw material and the flexible structure of the polypropylene fiber, and utilizes the promoting effect of the surface wetting agent to make the two tightly combined and entangled, so that the prepared oil-absorbing material has good structural stability and can be reused.
[0025] The oil absorbing material prepared by the invention is simple and efficient in treating oil spills on water and is easy to salvage. After absorbing oil once, the oil can be squeezed out and reused again, and the oil absorption rate of the reused oil can be maintained at more than 60% of the original.
[0026] In summary, the oil-absorbing material prepared by compounding discarded masks and straw in the present invention has the advantages of environmental protection, good oil absorption effect, simple oil absorption operation, reusability, low cost, etc., and has strong market competitiveness. DETAILED DESCRIPTION
[0027] The present invention is further described below in conjunction with examples. These examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples that do not specify specific conditions are usually carried out according to conventional conditions in the art or according to the conditions recommended by the manufacturer; the raw materials, reagents, etc. used, unless otherwise specified, are all raw materials and reagents that can be obtained from commercial channels such as conventional markets. Any non-substantial changes and substitutions made by those skilled in the art on the basis of the present invention belong to the scope of protection claimed by the present invention.
[0028] Example 1
[0029] A method for preparing an oil-absorbing material using discarded masks and straws comprises the following steps, wherein the following steps 1-3 are in no particular order:
[0030] Step 1: Remove the nose bridge and ear straps from the collected discarded masks, disinfect them with 75% alcohol, dry and cut them into 3-5 cm pieces as spare raw materials. The discarded masks are used commercially qualified masks produced by polypropylene fiber non-woven fabric materials, and the 75% alcohol is a commercially qualified product;
[0031] Step 2: first dissolving sodium hydroxide in tap water to prepare an alkaline aqueous solution with a concentration of 1%; at room temperature, cutting the straw to 1-2 cm, soaking it in the prepared alkaline aqueous solution with a concentration of 1% for 4 hours, taking it out and drying it for later use, wherein the straw is wheat straw produced by agricultural planting;
[0032] Step 3: preparing a surface wetting agent aqueous solution with a total concentration of 0.5% by adding water to a polyether surfactant, an ammonium oxide surfactant and a quaternary ammonium salt surfactant in a mass ratio of 1:2:3, wherein the polyether surfactant is industrial-grade polyethylene glycol with a degree of polymerization of 200, the ammonium oxide surfactant is industrial-grade dodecyl ammonium oxide, the quaternary ammonium salt surfactant is industrial-grade dodecyl trimethyl ammonium chloride, and the water is tap water above industrial grade;
[0033] Step 4: placing the sterilized and cut spare masks in step 1 in a high-speed multifunctional wall breaking machine, adding the surface wetting agent aqueous solution configured in step 3, and crushing at 300 rpm for 3 minutes; then adding the cut straw in step 2, the mass ratio of the added cut mask, the surface wetting agent aqueous solution, and the cut straw is 1:1:1, and continuing to crush at 300 rpm for 2 minutes, extruding the obtained product at a pressure of 4 MPa for 8 minutes to form a sheet material, and drying the sheet material at 60° C. to obtain the oil absorption material prepared using discarded masks and straw.
[0034] When used, the oil-absorbing material prepared using discarded masks and straw is put into an oil-contaminated water source (the oil-contaminated water source can be marine oil spill water or oil field wastewater, etc.), and after adsorption for 30 minutes, the oil-absorbing material is picked up, and the oil-contaminated water source can be absorbed, and the oil absorption rate reaches 10g / g (each 1g of oil-absorbing material can absorb 9.0g of oil).
[0035] The oil absorbing material prepared in this embodiment can be reused after absorbing oil once and then squeezing out the oil. According to tests, the oil absorption rate of the reused material for more than 5 times can maintain 66% of the oil absorption rate of the first use.
[0036] Example 2
[0037] A method for preparing an oil-absorbing material using discarded masks and straws comprises the following steps, wherein the following steps 1-3 are in no particular order:
[0038] Step 1: Remove the nose bridge and ear straps from the collected discarded masks, disinfect them with 75% alcohol, dry them, and cut them into 3-5 cm pieces as spare raw materials. The discarded masks are used commercially qualified masks produced from polypropylene fiber non-woven fabrics, and the 75% alcohol is a commercially qualified product.
[0039] Step 2: first dissolve potassium hydroxide in deionized water to prepare an alkaline aqueous solution with a concentration of 2%; cut the straw to 1-2 cm at room temperature, soak it in the prepared alkaline aqueous solution for 3 hours, fish it out and dry it for standby use, the straw is rice straw produced by agricultural planting;
[0040] Step 3: preparing a surface wetting agent aqueous solution with a total concentration of 1% by adding water to a polyether surfactant, an ammonium oxide surfactant and a quaternary ammonium salt surfactant in a mass ratio of 1:3:5, wherein the polyether surfactant is industrial-grade polypropylene glycol with a degree of polymerization of 1000, the ammonium oxide surfactant is tetradecyl ammonium oxide, the quaternary ammonium salt surfactant is hexadecyl trimethyl ammonium chloride, and the water used to dissolve the surfactant is industrial-grade deionized water;
[0041] Step 4: placing the sterilized and cut spare masks in step 1 in a high-speed multifunctional wall breaking machine, adding the surface wetting agent aqueous solution configured in step 3, and crushing at 250 rpm for 2 minutes; then adding the cut straw in step 2, the mass ratio of the added cut mask, the surface wetting agent aqueous solution, and the cut straw is 1:2:1.5, and continuing to crush at 250 rpm for 5 minutes, extruding the obtained product at a pressure of 5 MPa for 15 minutes to form a sheet material, and drying the sheet material at 65° C. to obtain the oil absorption material prepared using discarded masks and straw.
[0042] When used, the oil-absorbing material prepared using discarded masks and straw is put into an oil-contaminated water source (the oil-contaminated water source can be marine oil spill water or oil field wastewater, etc.), and after adsorption for 25 minutes, the oil-absorbing material is picked up, and the oil-contaminated water source can be absorbed, and the oil absorption rate reaches 11.5g / g.
[0043] The oil absorbing material prepared in this embodiment can be reused after absorbing oil once and then squeezing out the oil. According to tests, the oil absorption rate of the reused material for more than 6 times can maintain 63% of the oil absorption rate of the first use.
[0044] Example 3
[0045] A method for preparing an oil-absorbing material using discarded masks and straws comprises the following steps, wherein the following steps 1-3 are not performed in any order:
[0046] Step 1: Remove the nose bridge and ear straps from the collected discarded masks, disinfect them with 75% alcohol, dry them, and cut them into 3-5 cm pieces as spare raw materials. The discarded masks are used commercially qualified masks produced from polypropylene fiber non-woven fabrics, and the 75% alcohol is a commercially qualified product.
[0047] Step 2: First, chemically pure sodium hydroxide is dissolved in tap water to prepare an alkaline aqueous solution with a concentration of 3%; at room temperature, the straw is cut short to 1-2 cm, soaked in the prepared alkaline aqueous solution with a concentration of 3% for 3 hours, and then taken out and dried for use, wherein the straw is corn straw produced by agricultural planting;
[0048] Step 3: preparing a surface wetting agent aqueous solution with a total concentration of 3% by adding water to a polyether surfactant, an ammonium oxide surfactant and a quaternary ammonium salt surfactant in a mass ratio of 1:3:6, wherein the polyether surfactant is polyethylene glycol with a chemically pure degree of polymerization of 2000, the ammonium oxide surfactant is hexadecyl ammonium oxide, the quaternary ammonium salt surfactant is hexadecyl trimethyl ammonium chloride, and the water used to dissolve the surfactant is industrial grade deionized water;
[0049] Step 4: placing the sterilized and cut spare masks in step 1 in a high-speed multifunctional wall breaking machine, adding the surface wetting agent aqueous solution configured in step 3, and crushing at 100 rpm for 3 minutes; then adding the cut straw in step 2, the mass ratio of the added cut mask, the surface wetting agent aqueous solution, and the cut straw is 1:3:3, and continuing to crush at 100 rpm for 6 minutes, extruding the obtained product at a pressure of 6 MPa for 12 minutes to form a sheet material, and drying the sheet material at 75° C. to obtain the oil absorption material prepared using discarded masks and straw.
[0050] When used, the oil-absorbing material prepared using discarded masks and straw is put into an oil-containing contaminated water source (the oil-containing contaminated water source can be marine oil spill water or oil field wastewater, etc.), and after adsorption for 30 minutes, the oil-absorbing material is picked up, and the oil-containing contaminated water source can be absorbed, and the oil absorption rate reaches 12.5g / g.
[0051] The oil absorbing material prepared in this embodiment can be reused after absorbing oil once and then squeezing out the oil. According to tests, the oil absorption rate of the reused material for more than three times can maintain 71% of the oil absorption rate of the first use.
[0052] Example 4
[0053] A method for preparing an oil-absorbing material using discarded masks and straws comprises the following steps, wherein the following steps 1-3 are not performed in any order:
[0054] Step 1: Remove the nose bridge and ear straps from the collected discarded masks, disinfect them with 75% alcohol, dry them, and cut them into 3-5 cm pieces as spare raw materials. The discarded masks are used commercially qualified masks produced from polypropylene fiber non-woven fabrics, and the 75% alcohol is a commercially qualified product.
[0055] Step 2: first dissolving analytical pure potassium hydroxide in deionized water to prepare a 4% alkaline aqueous solution; at room temperature, cutting the straw to 1-2 cm, soaking it in a 4% alkaline aqueous solution for 4 hours, fishing it out and drying it for later use, wherein the straw is sorghum straw produced by agricultural planting;
[0056] Step 3: preparing a surface wetting agent aqueous solution with a total concentration of 2% by adding water to a polyether surfactant, an ammonium oxide surfactant and a quaternary ammonium salt surfactant in a mass ratio of 1:4:5, wherein the polyether surfactant is polypropylene glycol with an analytically pure degree of polymerization of 4000, the ammonium oxide surfactant is octadecyl ammonium oxide, and the quaternary ammonium salt surfactant is octadecyl trimethyl ammonium chloride;
[0057] Step 4: placing the sterilized and cut spare masks in step 1 in a high-speed multifunctional wall breaking machine, adding the surface wetting agent aqueous solution configured in step 3, and crushing at 200 rpm for 3 minutes; then adding the cut straw in step 2, the mass ratio of the added cut mask, the surface wetting agent aqueous solution, and the cut straw is 1:2:2.5, and continuing to crush at 300 rpm for 5 minutes, extruding the obtained product at a pressure of 4 MPa for 10 minutes to form a sheet material, and drying the sheet material at 70° C. to obtain the oil absorption material prepared using discarded masks and straw.
[0058] When used, the oil-absorbing material prepared using discarded masks and straw is put into an oil-contaminated water source (the oil-contaminated water source can be marine oil spill water or oil field wastewater, etc.), and after adsorption for 30 minutes, the oil-absorbing material is picked up, and the oil-contaminated water source can be absorbed, and the oil absorption rate reaches 9.6g / g.
[0059] The oil absorbing material prepared in this embodiment can be reused after absorbing oil once and then squeezing out the oil. According to tests, the oil absorption rate of the reused material for more than 4 times can maintain 80% of the oil absorption rate of the first use.
[0060] Example 5
[0061] A method for preparing an oil-absorbing material using discarded masks and straws comprises the following steps, wherein the following steps 1-3 are not performed in any order:
[0062] Step 1: Remove the nose bridge and ear straps from the collected discarded masks, disinfect them with 75% alcohol, dry them, and cut them into 3-5 cm pieces as spare raw materials. The discarded masks are used commercially qualified masks produced from polypropylene fiber non-woven fabrics, and the 75% alcohol is a commercially qualified product.
[0063] Step 2: First, dissolve analytical pure sodium hydroxide in tap water to prepare an alkaline aqueous solution with a concentration of 3.5%; at room temperature, cut the straw to 1-2 cm, soak it in the prepared alkaline aqueous solution with a concentration of 3.5% for 6 hours, fish it out and dry it for use, the straw is wheat straw produced by agricultural planting;
[0064] Step 3: prepare a surface wetting agent aqueous solution with a total concentration of 1.5% by mixing a polyether surfactant, an ammonium oxide surfactant and a quaternary ammonium salt surfactant with a mass ratio of 1:5:3 with water, wherein the polyether surfactant is analytically pure polyethylene glycol with a degree of polymerization of 1000, the ammonium oxide surfactant is hexadecyl ammonium oxide, the quaternary ammonium salt surfactant is hexadecyl trimethyl ammonium chloride, and the water used to dissolve the surfactant is industrial grade deionized water;
[0065] Step 4: placing the sterilized and cut spare masks in step 1 in a high-speed multifunctional wall breaking machine, adding the surface wetting agent aqueous solution configured in step 3, and crushing at 100 rpm for 5 minutes; then adding the cut straw in step 2, the mass ratio of the added cut mask, the surface wetting agent aqueous solution, and the cut straw is 1:3:3, and continuing to crush at 300 rpm for 5 minutes, extruding the obtained product at a pressure of 7 MPa for 6 minutes to form a sheet material, and drying the sheet material at 75° C. to obtain the oil absorption material prepared using discarded masks and straw.
[0066] When used, the oil-absorbing material prepared using discarded masks and straw is put into an oil-containing contaminated water source (the oil-containing contaminated water source can be marine oil spill water or oil field wastewater, etc.), and after adsorption for 30 minutes, the oil-absorbing material is picked up, and the oil-containing contaminated water source can be absorbed, and the oil absorption rate reaches 9.0g / g.
[0067] The oil absorbing material prepared in this embodiment can be reused after absorbing oil once and then squeezing out the oil. According to tests, the oil absorption rate of the reused material for more than 6 times can maintain 63% of the oil absorption rate of the first use.
[0068] Example 6
[0069] A method for preparing an oil-absorbing material using discarded masks and straws comprises the following steps, wherein the following steps 1-3 are not performed in any order:
[0070] Step 1: Remove the nose bridge and ear straps from the collected discarded masks, disinfect them with 75% alcohol, dry them, and cut them into 3-5 cm pieces as spare raw materials. The discarded masks are used commercially qualified masks produced from polypropylene fiber non-woven fabrics, and the 75% alcohol is a commercially qualified product.
[0071] Step 2: first dissolve industrial-grade potassium hydroxide in tap water to prepare an alkaline aqueous solution with a concentration of 5%; at room temperature, cut the straw to 1-2 cm, soak it in the prepared alkaline aqueous solution with a concentration of 5% for more than 6 hours, remove it and dry it for use, the straw is corn straw produced by agricultural planting;
[0072] Step 3: prepare a surface wetting agent aqueous solution with a total concentration of 2% by adding water to a polyether surfactant, an ammonium oxide surfactant and a quaternary ammonium salt surfactant in a mass ratio of 1:2:6, wherein the polyether surfactant is industrial-grade polypropylene glycol with a degree of polymerization of 1500, the ammonium oxide surfactant is octadecyl ammonium oxide, the quaternary ammonium salt surfactant is octadecyl trimethyl ammonium chloride, and the water used to dissolve the surfactant is industrial-grade deionized water;
[0073] Step 4: placing the sterilized and cut spare masks in step 1 in a high-speed multifunctional wall breaking machine, adding the surface wetting agent aqueous solution configured in step 3, and crushing at 300 rpm for 2 minutes; then adding the cut straw in step 2, the mass ratio of the added cut mask, the surface wetting agent aqueous solution, and the cut straw is 1:2.2:3, and continuing to crush at 300 rpm for 5 minutes, extruding the obtained product at a pressure of 5 MPa for 15 minutes to form a sheet material, and drying the sheet material at 70°C to obtain the oil absorption material prepared using discarded masks and straw.
[0074] When used, the oil-absorbing material prepared using discarded masks and straw is put into an oil-contaminated water source (the oil-contaminated water source can be marine oil spill water or oil field wastewater, etc.), and after adsorption for 25 minutes, the oil-absorbing material is picked up, and the oil-contaminated water source can be absorbed, and the oil absorption rate reaches 13.5g / g.
[0075] The oil absorbing material prepared in this embodiment can be reused after absorbing oil once and then squeezing out the oil. According to tests, the oil absorption rate of the oil absorbing material can be maintained at 69% of the first use after being reused for more than 7 times.
[0076] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A method for preparing an oil-absorbing material using discarded masks and straw, characterized in that: The method comprises the following steps, wherein there is no order requirement for executing step 1 to step 3: Step 1: Remove the nose bridge and ear straps from the recycled discarded masks, disinfect them with 75% alcohol, dry them and cut them into 3-5cm pieces; Step 2: At room temperature, cut the straw into 1-2 cm, soak it in 1-5% alkaline aqueous solution for more than 1 hour, remove it and dry it for later use; Step 3: preparing a surface wetting agent aqueous solution with a total concentration of 0.5-3% by adding water to a polyether surfactant, an ammonium oxide surfactant and a quaternary ammonium salt surfactant in a mass ratio of 1:2-5:3-6; Step 4: placing the cut mask described in step 1 in a wall breaking machine, adding the surface wetting agent aqueous solution configured in step 3, and crushing at 100-300 rpm for more than 2 minutes; then adding the cut straw described in step 2, the mass ratio of the added cut mask, the surface wetting agent aqueous solution, and the cut straw is 1:1-3:1-3, and continuing to crush at 100-300 rpm for more than 2 minutes, extruding the obtained product at a pressure of more than 3MPa for more than 6 minutes to form a sheet material, and drying the sheet material at 60-75°C to obtain the oil absorption material prepared by using discarded masks and straw.
2. The method for preparing an oil absorbing material using discarded masks and straw according to claim 1, characterized in that: The discarded masks are used masks produced using polypropylene fiber non-woven fabric materials.
3. The method for preparing an oil absorbing material using discarded masks and straw according to claim 1, characterized in that: The straw in step 2 is one or a mixture of two or more of the following crops: wheat, rice, corn or sorghum.
4. The method for preparing an oil absorbing material using discarded masks and straw according to claim 1, characterized in that: The method also includes step 20 before step 2, and the specific steps of step 20 are as follows: dissolving an alkali reagent in water to prepare an alkali aqueous solution with a concentration of 1-5%, wherein the alkali reagent is sodium hydroxide or potassium hydroxide of industrial grade or higher purity, and the water used to dissolve the alkali reagent is tap water of industrial grade or higher purity, or deionized water.
5. The method for preparing an oil absorbing material using discarded masks and straw according to claim 1, characterized in that: In the step 3, the polyether surfactant is one of the following: polyethylene glycol with a degree of polymerization of more than 200 or polypropylene glycol with a degree of polymerization of more than 200.
6. The method for preparing an oil absorbing material using discarded masks and straw according to claim 1, characterized in that: In step 3, the ammonium oxide surfactant is one of the following: dodecyl ammonium oxide, tetradecyl ammonium oxide, hexadecyl ammonium oxide, or octadecyl ammonium oxide.
7. The method for preparing an oil absorbing material using discarded masks and straw according to claim 1, characterized in that: In the step 3, the quaternary ammonium salt surfactant is one of the following: dodecyltrimethylammonium chloride, tetradecyltrimethylammonium chloride, hexadecyltrimethylammonium chloride, or octadecyltrimethylammonium chloride.
8. The method for preparing an oil absorbing material using discarded masks and straw according to claim 1, characterized in that: In step 3, the water used to dissolve the surfactant is industrial grade or above tap water, or deionized water.
9. The method for preparing an oil absorbing material using discarded masks and straw according to claim 1, characterized in that: In the step 4, the obtained product is extruded at a pressure of 4-7 MPa for 6-15 minutes into a sheet material.