Flow path forming device, extrusion device, and foamed plastic sheet

By optimizing the sliding properties of the flow path forming surface in the flow path forming device, and controlling the maximum drop weight of the water droplet surface from horizontal to plumb state, the thicker and poor appearance of the molded product in the prior art are solved. The problem of this achieves more stable ejection and better quality of molded products.

CN119058055APending Publication Date: 2024-12-03RICOH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410674937.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-31
Filing Date
2024-05-28
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing flow path forming device has shortcomings in suppressing the thickness of the plastic molded product and improving appearance, and it is difficult to effectively control the sliding properties of the flow path forming surface, resulting in rough surface and unstable ejection of the molded product.

Method used

By dropping water droplets on the flow path forming surface and measuring the maximum drop weight that does not slide when the dripping surface is from horizontal to plumb state, the average drop weight value of the first flow path forming surface and the second flow path forming surface is ensured. The sliding properties of the flow path forming surface are optimized to suppress the thickness of the molded product and improve the appearance.

Benefits of technology

It effectively suppresses the thickness of the molded product, improves appearance and discharge stability, enhances the freedom of flow path design, and ensures the quality and appearance of the molded product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119058055A_ABST
    Figure CN119058055A_ABST
Patent Text Reader

Abstract

The invention provides a flow path forming device, an extrusion device and a foamed plastic sheet, which can inhibit the thickness of a molded product and enable the appearance of the molded product to be good. The flow path forming device (5) has a first flow path forming member (10) and a second flow path forming member (20), and a flow path (30) for flowing a plastic composition is formed by the first flow path forming member (10) and the second flow path forming member (20). Then, water droplets are dropped within a range of 3 mm from the outlets of the flow paths (30) on the flow path forming surfaces of the first flow path forming member (10) and the second flow path forming member (20) to the upstream side in the flow direction of the plastic composition. The maximum droplet weight (G) at which the water droplets do not slip when the dripping surface of the water droplets on the flow path formation surface is inclined from a state parallel to the horizontal direction to a state parallel to the vertical direction is measured, and the average value of the maximum droplet weight (G) is 8-25 [mu] g.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a flow path forming device, an extruding device and a foamed plastic sheet. Background Art

[0002] Conventionally, there is known a flow path forming device which includes a first flow path forming member and a second flow path forming member and forms a flow path for a plastic composition to flow by the first flow path forming member and the second flow path forming member.

[0003] Patent document 1 describes a flow path forming device in which the contact angle between the flow path forming surface and the molten resin in the range of 5 mm upstream from the flow path outlet of the thermoplastic resin extrusion foaming die as the flow path forming device and 45° to 65° is set. By setting the contact angle with the molten resin to 45° to 65°, the slidability of the molten resin relative to the flow path forming surface can be made appropriate. As a result, the surface of the molded product can be prevented from becoming rough and the appearance can be improved, and the pressure near the flow path outlet can be well maintained, which can prevent the molded product from being thickened.

[0004] However, there is still room for improvement in suppressing the occurrence of uneven thickness and improving the appearance.

[0005] [Patent Document 1] (Japan) Patent No. 2896832 Summary of the invention

[0006] In order to solve the above-mentioned problems, the present invention relates to a flow path forming device, characterized in that it includes: a first flow path forming part and a second flow path forming part, and a flow path for the flow of a plastic composition is formed by the first flow path forming part and the second flow path forming part, water drops are dripped on the flow path forming surfaces of the first flow path forming part and the second flow path forming part forming the flow path within a range of 3 mm from the outlet of the flow path to the upstream side of the flow direction of the plastic composition, and the maximum droplet weight at which the water drop does not slide down when the dripping surface of the flow path forming surface is tilted from a state parallel to the horizontal direction to a state parallel to the vertical direction, and the average value of the maximum droplet weight of the flow path forming surface of the first flow path forming part and the maximum droplet weight of the flow path forming surface of the second flow path forming part is greater than 8μg and less than 25μg.

[0007] According to the present invention, uneven thickness of a molded article can be suppressed, and the appearance of the molded article can be improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0008] Figure 1 FIG. 1 is a schematic cross-sectional view of an example of the flow channel forming device according to the present embodiment.

[0009] Figure 2Shown is a schematic diagram of an example of a kneading device.

[0010] Figure 3 Shown is an exemplary diagram of an extrusion molding apparatus.

[0011] Figure 4 (a) is a graph showing the relationship between the deviation and the maximum droplet weight, and (b) is a graph showing the relationship between the appearance defect and the maximum droplet weight. DETAILED DESCRIPTION

[0012] Below, the best mode for implementing the present invention is described based on the accompanying drawings. In addition, it is easy for those skilled in the art to change and modify the present invention within the scope of the claims to form other embodiments, and these changes and modifications are included in the scope of the claims. The following description is an example of the best mode of the present invention and does not limit the scope of the claims.

[0013] Figure 1 1 is a schematic cross-sectional view of an example of the flow channel forming device 5 according to the present embodiment.

[0014] The type of the flow path forming device (hereinafter sometimes referred to as "mold", "die head", "nozzle") is not particularly limited and can be appropriately selected according to the purpose. As the flow path forming device, for example, a T die head, a flat die head, a seamless die head, a circular die head, a single heart-shaped die head, a double heart-shaped die head, a spiral die head, a bridge die head, a star-shaped die head, a tournament die head (tournament die), a hanger-shaped die head, a manifold die head, and their composite dies, etc. can be listed. Among them, from the viewpoint of using a non-flammable gas as a foaming agent to form a foamed sheet, a seamless die head is preferred, and a circular die head is more preferred.

[0015] exist Figure 1 In the example shown, the flow path forming device 5 of the present embodiment includes a first flow path forming member 10 and a second flow path forming member 20 facing the first flow path forming member 10 , and further includes other members as necessary.

[0016] The first flow path forming member 10 has a through hole, and the second flow path forming member 20 is inserted into the through hole to form an annular flow path 30 in which a plastic composition containing at least one plastic flows.

[0017] The inner peripheral surface of the through hole of the first flow path forming member 10 is a first flow path forming surface 40 forming the flow path 30 , and the outer peripheral surface of the second flow path forming member 20 is a second flow path forming surface 50 forming the flow path 30 .

[0018] In the present embodiment, a plastic composition containing at least one type of plastic is passed through the flow path 30 and the plastic composition is extruded from the outlet of the flow path 30 to form a foamed plastic sheet as a molded product.

[0019] If the flow path forming surfaces 40 and 50 have poor sliding properties with respect to the plastic composition, the surface of the molded product may be rough due to the friction between the flow path forming surfaces and the plastic composition, and the appearance may be poor. On the other hand, if the flow path forming surfaces 40 and 50 have too good sliding properties with respect to the plastic composition, the internal pressure of the flow path 30 for extrusion, i.e., the back pressure, is insufficient, and the flow of the plastic composition in the flow path 30 becomes unstable. As a result, the deviation of the ejection amount of the plastic composition ejected from the flow path outlet increases in the circumferential direction, or the ejection amount fluctuates in units of several minutes, etc., causing the ejection of the plastic composition from the flow path outlet to become unstable. As a result, the thickness of the molded product is uneven, so-called uneven thickness occurs.

[0020] If the sliding properties of the flow path forming surfaces 40, 50 relative to the plastic composition (the flow resistance of the plastic composition relative to the flow path forming surfaces) are not suitable, it is possible that the flow path may become thicker over time. In addition, if the sliding properties of the flow path forming surfaces 40, 50 relative to the plastic composition are not suitable, it is difficult to control the pressure loss of the entire flow path within the pressure resistance of the device. In addition, in order to limit the pressure loss of the entire flow path within a certain range, the gap between the lips has to be enlarged. As a result, the above gap does not match the molded product (foamed plastic sheet) to be manufactured. In addition, when a non-flammable gas is used as a foaming agent, premature foaming occurs in the flow path. As a result, a molded product in the desired state cannot be obtained. Furthermore, there is a tendency for cleaning operations of the flow path to become difficult.

[0021] Conventionally, whether the sliding property of the flow path forming surface 40, 50 with respect to the plastic composition (the flow resistance of the plastic composition with respect to the flow path forming surface) is appropriate is determined based on the contact angle between the flow path forming surface and a fluid such as water or molten resin. However, even if the contact angle of the flow path forming surface is set within a range where the sliding property is appropriate, the appearance of the sheet may not be reduced, or ejection stability may not be achieved, indicating that the sliding property of the flow path forming surface cannot be appropriately specified by the contact angle.

[0022] Therefore, in this embodiment, an in-depth study was conducted and it was found that by the following regulation, the sliding property (flow resistance of the plastic composition) of the flow path forming surface can be made within an appropriate range compared with regulation by the contact angle. Specifically, the maximum droplet weight at which the droplet does not slide off when the dripping surface dripping with water droplets is tilted from a state parallel to the horizontal direction to a state parallel to the vertical direction when water droplets are dripped on the flow path forming surface. Moreover, as shown in the verification test described later, by making the average value of the maximum droplet weight of the flow path forming surface 40 and the maximum droplet weight of the flow path forming surface 50 8 μg or more and 25 μg or less, preferably 10 μg or more and 15 μg or less, it is possible to suppress the reduction in the appearance of the molded product due to the friction between the flow path forming surface and the plastic composition, and it is possible to improve the ejection stability of the plastic composition starting from the flow path outlet, and suppress the uneven thickness of the molded product.

[0023] In addition, by controlling the average value of the maximum droplet weight within the above range and making the flow path forming surfaces 40 and 50 have appropriate sliding properties, the spraying stability starting from the flow path outlet can be achieved, thereby increasing the freedom of flow path design. As a result, it is easy to set the gap used to ensure the necessary back pressure to a flow path design that matches the molded product (foamed plastic sheet) to be manufactured. Therefore, it is easy to obtain a molded product in the required state. In addition, by increasing the freedom of flow path design, it is also possible to design a flow path that is easy to clean during production changes.

[0024] In addition, it is preferred that water droplets are dripped onto the flow path forming surface within a range of 3 mm from the outlet of the flow path 30 to the upstream side in the flow direction of the plastic composition, and that the average value of the maximum droplet weight on the flow path forming surface 40 and the maximum droplet weight on the flow path forming surface 50 be within the above range at least within the range of 3 mm. This is because the flow resistance of the plastic composition to be foamed with respect to the flow path forming surface can be made within an appropriate range, the flow stability of the plastic composition can be maintained, and the appearance defect caused by the friction between the flow path forming surface and the sheet can be suppressed.

[0025] [Method for measuring the maximum droplet weight]

[0026] The method for measuring the maximum droplet weight at which the droplet does not slide off is not particularly limited and can be appropriately selected according to the purpose. Specifically, it is confirmed that a predetermined droplet amount can be dripped by a commercially available contact angle meter, a syringe with a micrometer tip, a pipette, etc. If necessary, the correspondence between the droplet volume and the droplet weight is determined by a commercially available electronic balance. Then, the droplet is dripped onto the flow path forming surface within a range of 3 mm from the outlet of the flow path 30 to the upstream side in the flow direction of the plastic composition.

[0027] At this time, the software attached to various contact angle meters can also be used to directly estimate the droplet volume. Before the water drops are dripped, wipe the surface of the flow path forming surface where the water drops are dripped with a solvent or alcohol with strong degreasing power or a parts cleaner. Then, it is preferred to wipe repeatedly with a clean cloth until it becomes a dry wipe state, and no more friction than necessary is applied after drying. This is to prevent changes in the measurement results due to frictional charging or changes in adsorbed substances. In addition, for the same reason, blowing after solvent wiping is not preferred.

[0028] Next, the dripping surface of the flow channel forming surface is tilted from a state parallel to the horizontal direction to a state parallel to the vertical direction. At this time, the tilting can be performed using a rotating movable table, a crane, or a tilting machine. However, it should be confirmed experimentally that no vibration that affects the measurement is applied.

[0029] In addition, by Figure 1 It can be seen that the flow path forming surface in the range of 3 mm from the outlet of the flow path 30 for dripping water to the upstream side of the flow direction of the plastic composition is roughly a curved surface. Therefore, at this time, the imaginary plane that is connected to the flow path forming surface at the center point of the droplet portion is used as the dripping surface, and it is tilted to be parallel to the vertical direction. That is, the dripping surface is regarded as a plane connected to the curved surface, and average data can be obtained. However, there is a planar area of ​​the flow path forming surface in the range of 3 mm from the outlet of the flow path 30 to the upstream side of the flow direction of the plastic composition ( Figure 1 In the case of a straight line area in the middle), water droplets are dripped onto the flat area.

[0030] Regarding the judgment of whether the droplet has slid down, it is considered to have slid down when the amount of sliding down within 1 minute after 3 seconds after reaching the vertical position is 1 mm or more. Alternatively, the image before tilting parallel to the vertical direction and the image after tilting parallel to the vertical direction can be compared, and if the movement below the part formed by the contact angle on the upper side of the vertical direction of the water droplet is confirmed, it is judged to have slid down. In addition, the method for judging whether the droplet has slid down is not limited to this, as long as it is a method that can confirm the movement of the entire droplet.

[0031] The basic measurement operation of the contact angle is in accordance with JIS R 3257. In addition, in the verification test described below, the droplet weight scanning is carried out in the form of 5μg, 8μg, 10μg, 15μg, and then increasing by 5μg each time, but the droplet weight scanning should be appropriately changed according to the error of the true value to be obtained.

[0032] In addition, the contact angle of the first flow path forming surface 40 and the second flow path forming surface 50 with respect to water is not particularly limited and can be appropriately selected according to the purpose, preferably 55° or more and less than 110°. Within this range, it can be set within the above range by relatively inexpensive processing, and there is no need to perform expensive water-repellent treatment or hydrophilic treatment on the flow path surface, such as micro-processing such as fractal processing, etc.

[0033] [Contact angle measurement method]

[0034] There is no particular limitation on the method for measuring the contact angle, and it can be appropriately selected according to the purpose. For example, it can be measured by a method based on JIS R3257. The contact angle is measured at a droplet volume in the range of about 0.5 μl to about 4 μl, and the maximum value is used when there is a peak. In the case of a small droplet volume of less than 0.5 μl, the influence of the nozzle diameter and the like may occur, resulting in an error in the contact angle being a low angle. On the other hand, in the case of a large droplet volume of more than 4 μl, there may be an impact when the liquid leaves the nozzle and an error in the contact angle being a low angle may occur.

[0035] In addition, the droplet volume at which the contact angle becomes approximately constant regardless of the droplet volume is preferably about 1.5 μl. In addition, a contact angle meter without a nozzle can also be used to measure the contact angle. The angle calculation does not necessarily have to be based on the method of JIS R3257, and can also rely on image processing of the side camera image of the droplet or the camera image of the top of the droplet within the range of ensuring consistency.

[0036] In addition, the arithmetic mean roughness Ra of the flow path forming surface of at least one of the flow path forming surface 40 and the flow path forming surface 50 is preferably less than 1.5, and the average length Rsm of the roughness curve element is preferably 60μm or more. More preferably, the arithmetic mean roughness Ra of the flow path forming surface of the flow path forming surface 40 or the flow path forming surface 50 is less than 1.3, and the average length Rsm of the roughness curve element is 67μm or more. It is particularly preferred that the arithmetic mean roughness Ra is greater than 0.2 and less than 1.3, and the average length Rsm of the roughness curve element is greater than 67μm and less than 106. Furthermore, the core height difference Rk of at least one of the flow path forming surface 40 and the flow path forming surface 50 is preferably greater than 1.0μm. Thus, the transfer of the rough shape of the molded product caused by the excessively rough flow path shape and the increase in the surface roughness of the molded product caused by this can be suppressed, and the sliding property of the flow path forming surface can be within an appropriate range.

[0037] [Measurement method of surface roughness parameters]

[0038] There is no particular limitation on the measuring method of each of the surface roughness parameters Rsm, Ra, and Rk. For example, portable roughness meters such as KEYENCE VK-X250 and Mitutoyo SJ-210 can be used for measurement. An example of the measuring conditions when measuring each of the surface roughness parameters Rsm, Ra, and Rk using KEYENCE VK-X250 is shown below. In addition, in the case of the correlation relationship based on the following measurement conditions and the presence of instrument error, it is sufficient to grasp the situation in advance, and it is not limited to this.

[0039] [Measurement conditions]

[0040] · Measuring device: KEYENCE VK-X250

[0041] Brightness: Automatic setting

[0042] Dual scan (automatic)

[0043] Measurement mode: Surface shape mode

[0044] Resolution: 1024×768

[0045] High-precision mode

[0046] RPD: No setting

[0047] ·Measurement height interval: 0.1μm

[0048] Monoscopic (no image combining)

[0049] Use X20 objective lens

[0050] [Image processing / measurement]

[0051] Plane correction: "Base plane correction (entire area)"

[0052] · Surface correction: "Surface correction strength 3"

[0053] ·Bundle point removal

[0054] ·A total of 20 vertical lines are measured (the average value of 20 points is used for line roughness, but it can also be used instead for parameters defining surface roughness)

[0055] Roughness measurement: When there is no cutoff value for λs or λc, terminal correction is performed.

[0056] It is preferred that the HRC hardness of at least one of the first flow path forming surface 40 and the second flow path forming surface 50 is 28 or more. By setting the HRC hardness to 28 or more, the sliding property of the flow path forming surface can be maintained over time. Therefore, the circumferential quality deviation and the quality deviation over time of the molded product can be maintained, and the friction between the resin and the flow path can be prevented, and the deterioration of the appearance of the molded product can be suppressed over time. Therefore, a device with low maintenance cost can be provided.

[0057] As a method for measuring HRC hardness, it can be measured by the method in accordance with JIS Z 2245. Since the HRC hardness measurement method is a destructive test, only when it is confirmed in advance that the HRC hardness of the outermost surface can be correctly estimated, can it refer to other hardness indicators, tensile test strength, or material sampling inspection values.

[0058] The materials of the first flow path forming member 10 and the second flow path forming member 20 of the flow path forming device 5 are not particularly limited and can be appropriately selected according to the purpose. Examples of the materials of the first flow path forming member 10 and the second flow path forming member 20 include metal, carbon steel, chrome steel, nickel steel, nickel-chrome steel, aluminum, plastic, stainless steel, pre-hardened steel, cemented carbide, high-speed steel, namely, S45C, S50C, S55C, A5052, S10, S400, S10, S304, S10, S316, S10, S420, SKD11, SKH51, HPM-38, SCM415, SCM435, SCM440, etc.

[0059] In addition, various coatings performed on the surfaces of the first flow path forming component 10 and the second flow path forming component 20, and on the flow path forming surfaces 40 and 50, include hard chrome plating, electroless nickel plating, acid-resistant aluminum treatment, black dyeing, Parker, carbide film, nitride film, oxide film, DLC treatment, silicon release treatment, fluorine release treatment, that is, Cr, Ni, Ni-P, amorphous alumina, crystallized alumina, zirconium oxide, TiC, TiCN, TiN, WC, PTFE, ETFE, FEP, PCTFE, PFA, PVDF, substances formed by compounding them, substances formed by compounding functional additives of plastics with them, etc.

[0060] The forming method of the material of the first flow path forming member 10 and the second flow path forming member 20 of the flow path forming device 5 is not particularly limited and can be appropriately selected according to the purpose. For example, cutting, rolling, electric discharge machining, drawing, grinding, spraying, vapor deposition, physical vapor deposition PVD, chemical vapor deposition CVD, plating, spraying, etching, etc. can be cited. Among them, spraying is excellent in efficiency when experimentally exploring various embodiments, but the products explored by spraying can also be mass-produced by other processing methods.

[0061] As a spraying method, it is preferred to dilute with a solvent, but there is no problem as long as it can be processed. From the aspect of durability, it is preferred to use a coating that reacts during firing, but it is not limited to this. In order to maintain the adhesion of the coating, it is preferred to make the base as rough as possible, but it is not limited to this. Depending on the situation, there is no problem even if the base is intentionally exposed and the coating remains at the bottom of the valley.

[0062] There is no particular limitation on the finishing method of the first flow path forming member 10 and the second flow path forming member 20 of the flow path forming device 5, and they can be appropriately selected according to the purpose. As finishing methods, for example, plasma treatment, ozone treatment, heat aging treatment, chemical aging treatment, physical aging treatment, silane coupling treatment, glass coating, etc. can be cited. These can stabilize the number of cracks on the hard chrome plated surface, for example, or expand the width of the cracks. In addition, it can be used to fine-tune the maximum droplet weight G mentioned above.

[0063] The control of the surface state of the flow path forming surfaces 40 and 50 by the above-mentioned finishing method can be freely selected from the methods widely used as primer treatment or adhesion improvement treatment. In the case of metal, it is believed that the quality changes over time due to the increase in the thickness of the surface oxide layer, but in such a case, heat aging treatment is effective for stable production.

[0064] In the case of organic matter, the performance of the flow path 30 may change due to thermal degradation. Therefore, in this case, thermal aging treatment is also effective for stable production. However, it is preferred that the heat treatment temperature is higher than the processing temperature. In addition, for the same reason, although unstable flow may occur when the product is new, the performance will be stabilized after a test shot of several tons. In this case, it is also effective to perform the above-mentioned aging treatment in advance.

[0065] In the case where the maximum droplet weight or contact angle at which the droplets do not slide off is too small or too large, the surface state of the flow path forming surfaces 40 and 50 can be controlled by, for example, the following adjustment. That is, the flow path forming surface can be adjusted by gently wiping, dipping, or lightly sticking sandpaper of about #2000 on it with a solvent. However, since the direction and width that can be changed by the material will vary, it is preferred to select appropriately experimentally. In addition, as a final treatment, a method of adjusting the maximum droplet weight G or the contact angle by gently wiping, dipping, or lightly sticking sandpaper of about #2000 on the flow path forming surface can also be used. In addition, it can also be implemented as a pretreatment for improving the adhesion of various coatings performed on the surfaces of the first flow path forming component 10 and the second flow path forming component 20 and on the flow path forming surfaces 40 and 50.

[0066] The flow path 30 of the flow path forming device 5 is annular, and the shape of the annular shape is not particularly limited and can be appropriately selected according to the purpose. For example, a circular ring shape, a polygonal ring shape, a shape whose diameter increases toward the flow path outlet, etc. can be mentioned.

[0067] In addition, the size of the flow path 30 is not particularly limited and can be appropriately selected according to the purpose, but the diameter of the front end of the flow path outlet is preferably 70 mm or more and 160 mm or less regardless of the shape of the flow path 30. Thus, it is easy to manufacture a sheet having a practical foaming ratio range of about 5 to 30 times without corrugation, and the sheet width of the final product can correspond to the sheet width required by the market, that is, 300 mm or more and 1300 mm or less.

[0068] The method for forming the shape of the flow path forming surfaces 40 and 50 in the flow path forming device is not particularly limited and can be appropriately selected according to the purpose. For example, the shape of the flow path forming surfaces 40 and 50 can be formed by sandblasting, but is not limited to this, and can also be formed by electrolysis, chemical etching, lathe or other mechanical processing methods.

[0069] It is known that when sandblasting with air is used to form the shape of the flow path forming surfaces 40 and 50, the roughness of the flow path forming surfaces 40 and 50 can be controlled by controlling the construction time, the blasting pressure, the distance from the workpiece, the processing angle, the medium shape, the medium material, etc. Sandblasting may be affected by the hardness of the outermost layer of the workpiece, the structure of the processing equipment, the degree of deterioration of the medium, the nozzle shape (the shape of the flow path outlet), etc., so that the roughness of the flow path forming surfaces 40 and 50 may be uneven. However, for example, since there is a relationship that the roughness increases as the blasting pressure increases, any roughness can be obtained by repeatedly performing trial production using a test piece made of the same material as the product.

[0070] Next, the plastic composition flowing in the flow path 30 of the flow path forming device 5 will be described.

[0071] <Plastic composition>

[0072] The plastic composition is a material constituting the foamed plastic sheet molded by the flow path forming device 5. The plastic composition contains at least one plastic resin, preferably a filler (also called a foaming core material), a foaming agent, and may contain other components as required.

[0073] -Plastic resin-

[0074] There is no particular limitation on the plastic resin, and it can be appropriately selected according to the purpose. For example, as the plastic resin, there can be listed styrene homopolymers such as polystyrene and poly-p-methylstyrene, styrene-maleic anhydride copolymer, styrene-acrylonitrile copolymer, styrene-butadiene copolymer, styrene-acrylic acid copolymer, styrene-methacrylic acid copolymer, styrene resins such as mixtures of polystyrene and polyphenylene ether, polylactic acid, polyglycolic acid, poly (3-hydroxybutyrate), poly (3-hydroxybutyrate · 3-hydroxycaproate), poly (3-hydroxybutyrate · 3-hydroxyvalerate), polycaprolactone, polybutylene succinate, poly (butylene succinate · adipate) and the like. These can be used alone or in combination of two or more.

[0075] As the aliphatic polyester resin, a product synthesized from an alcohol component or a derivative thereof and an acid component or a derivative thereof may be used, or a commercially available product may be used.

[0076] Among them, aliphatic polyesters as low environmental load polymer materials are preferred, and polylactic acid as a carbon neutral material and relatively inexpensive is more preferred. In addition, polylactic acid has properties similar to those of polystyrene resins used in the past, and has a higher melting point, toughness, chemical resistance, etc. compared to other biodegradable plastics. From this point of view, polylactic acid is also preferred.

[0077] As polylactic acid, for example, copolymers of D-lactic acid and L-lactic acid, homopolymers of either D-lactic acid (D-form) or L-lactic acid (L-form), ring-opening polymers of at least one lactide selected from the group consisting of D-lactide (D-form), L-lactide (L-form) and DL-lactide, etc. can be cited. These materials can be used alone or in combination of two or more. In addition, polylactic acid can be used either by appropriate synthesis or by commercial products.

[0078] The ratio of the D-form:L-form of lactic acid constituting the polylactic acid is not particularly limited, but it is preferred that the D-form and L-form of lactic acid constituting the polylactic acid account for 95 mol% or more in the polylactic acid. Polylactic acid consisting of only one optical isomer of the D-form and the L-form may also be used. The polylactic acid falling within this range has high crystallinity, and the foamed sheet produced using such polylactic acid can be expected to have good heat resistance and is suitable for food applications, etc.

[0079] The content of the plastic resin is not particularly limited and may be appropriately selected depending on the intended purpose, but is preferably 90% by mass or more based on the total amount of the plastic composition.

[0080] The method for measuring the content of the plastic resin is not particularly limited and may be appropriately selected depending on the intended purpose. For example, the content of the plastic resin may be measured by determining the weight ratio of the resin component from the ash content determined in accordance with JIS K7250-1.

[0081] -filler-

[0082] The filler (hereinafter sometimes referred to as "foaming core material") is contained in the plastic composition for the purpose of adjusting the foaming state (cell size, amount, arrangement, etc.), reducing costs, and improving strength.

[0083] The filler is not particularly limited and may be appropriately selected depending on the purpose, and examples thereof include inorganic fillers and organic fillers, etc. These materials may be used alone or in combination of two or more.

[0084] As inorganic filler, for example, talcum, kaolin, calcium carbonate, silicate mineral, zinc carbonate, wollastonite, silicon dioxide, aluminum oxide, manganese oxide, calcium silicate, sodium aluminate, calcium aluminate, sodium aluminosilicate, magnesium silicate, glass balls, carbon black, zinc oxide, antimony trioxide, zeolite, hydrotalcite, metallic fiber, metallic whisker, ceramic whisker, potassium titanate, boron nitride, graphite, glass fiber and carbon fiber etc. can be listed.Wherein, from the viewpoint of performance and cost, silicate mineral is preferred.Or, from the affinity with the compressible fluid described later, also preferably silicon dioxide or the filler that has been surface treated with silicon dioxide.

[0085] Examples of organic fillers include naturally occurring polymers such as starch, cellulose, wood flour, soybean dregs, rice husks, and wheat bran, sorbitol compounds, benzoic acid, metal phosphates, and rosin compounds, etc. Among them, cellulose is preferred from the viewpoint of low environmental load.

[0086] - Foaming agent -

[0087] There is no particular limitation on the blowing agent, and it can be appropriately selected according to the purpose. As the blowing agent, for example, hydrocarbons such as lower alkanes such as propane, n-butane, isobutane, n-pentane, isopentane, and hexane, ethers such as dimethyl ether, halogenated hydrocarbons such as methyl chloride and ethyl chloride, and physical blowing agents such as compressed gases such as carbon dioxide and nitrogen (hereinafter sometimes referred to as "compressible fluids") can be cited. Among them, compressed gases such as carbon dioxide and nitrogen are preferred from the viewpoint of no odor, safe operation, and low environmental load.

[0088] By containing a foaming agent, a plastic foam sheet having a high foaming ratio can be obtained.

[0089] -Other components-

[0090] There is no particular limitation on other components and they may be appropriately selected according to the purpose. For example, there may be mentioned a crosslinking agent, a heat stabilizer, an antioxidant, a plasticizer, a lubricant and the like.

[0091] The crosslinking agent is not particularly limited and may be appropriately selected depending on the intended purpose. For example, at least one selected from epoxy resin compounds and isocyanate compounds is preferred, and epoxy resin compounds are more preferred.

[0092] The foamed sheet produced by using the aliphatic polyester resin composition containing such a crosslinking agent can suppress the coalescence and breakage of cells and can increase the foaming ratio.

[0093] Next, a foamed plastic sheet (hereinafter referred to as a foamed sheet) formed by extruding a plastic composition from the outlet of the flow path 30 of the flow path forming device 5 and foaming the plastic composition will be described.

[0094] (Foam Sheet)

[0095] The foaming ratio of the foamed sheet as the foamed plastic sheet is preferably 2 to 50 times, more preferably 5 to 40 times, and further preferably 10 to 30 times. When the foaming ratio is less than 2 times, the strength is sufficient but the lightness is poor, which is not preferred. When the foaming ratio exceeds 30 times, the lightness is excellent but the strength is insufficient, which is not preferred.

[0096] The method for measuring the expansion ratio of the foam sheet is not particularly limited and can be appropriately selected according to the purpose, for example, it can be measured by a buoyancy specific gravity measuring device, etc. Alternatively, the bulk density and true density of the foam sheet can be measured to obtain the expansion ratio by the following formula.

[0097] Foaming ratio = true density [g / cm3] / bulk density [g / cm3]

[0098] In the foam sheet, it is preferred that the foam sheet does not substantially contain volatile components. By substantially containing no volatile components, in addition to improving dimensional stability, the impact on the human body or the environment can also be reduced. Examples of volatile components include foaming agents such as organic solvents and butane. In addition, the above-mentioned "substantially containing no" means that it is below the detection limit in the following analysis.

[0099] A part of the foam sheet was used as a sample, 2 parts by mass of 2-propanol was added to 1 part by mass of the sample, and after ultrasonic dispersion for 30 minutes, it was stored in a refrigerator (5°C) for more than 1 day to obtain an extract of volatile components. The extract of volatile components was analyzed by gas chromatography (GC-14A, manufactured by Shimadzu Corporation) to quantify the volatile components in the foam sheet. The measurement conditions are as follows.

[0100] [Measurement conditions]

[0101] Device: Shimadzu GC-14A

[0102] Chromatographic column: CBP20-M50-0.25

[0103] Detector: FID

[0104] Injection volume: 1μL~5μL

[0105] Carrier gas: He2.5kg / cm2

[0106] Hydrogen flow rate: 0.6kg / cm2

[0107] Air flow: 0.5kg / cm2

[0108] Chromatographic speed: 5mm / min

[0109] Sensitivity: Range101×Atten20

[0110] Column temperature: 40°C

[0111] InjectionTemp: 150℃

[0112] [Measurement]

[0113] A part of the foam sheet is dispersed in a solvent, and the volatile component extract is measured by gas chromatography under the above conditions to quantify the organic compound. When no organic compound having a boiling point of -20°C or more and less than 150°C at 1 atm is detected (below the detection limit), the foam sheet is "substantially free of" volatile components.

[0114] In order to prevent the detection of organic compounds when the foam sheet is subjected to the above measurement, as described above, by using a substance other than organic compounds such as carbon dioxide as a foaming agent, the content of volatile components (organic compounds having a boiling point of not less than -20°C and less than 150°C) can be made substantially 0% by mass. In the above measurement, by making the foam sheet in which organic compounds having a boiling point of not less than -20°C and less than 150°C (below the detection limit) are not detected, it is possible to safely handle without generating odor or the like.

[0115] As described later, carbon dioxide or the like used as a compressive fluid impregnated into the plastic resin in the kneading process can be used directly as a foaming agent without being removed after the kneading process. By using carbon dioxide as a compressive fluid impregnated into the plastic composition in the kneading process and using the compressive fluid directly as a foaming agent, it is possible to avoid using a volatile component as a foaming agent, and it is easy to make the foam sheet substantially free of volatile components.

[0116] Next, an extrusion molding device and an extrusion molding method for molding the foamed sheet (foamed plastic sheet) by extruding the plastic composition from the flow channel outlet of the flow channel forming device 5 of the present embodiment will be described.

[0117] (Extrusion molding device and extrusion molding method)

[0118] The extrusion molding method includes a kneading step and a foaming step, and also includes other steps. In addition, the kneading step and the foaming step can be carried out in one device (one extruder) or in different devices (extruders).

[0119] Extrusion molding equipment can be used Figure 3 The details will be described later. Figure 3 The extrusion molding device 110 shown in the figure includes a first extruder 110a for a kneading process and a second extruder 110b for a foaming process. In addition, the extrusion molding device 110 may also include a device for performing other processes. The first extruder 110a for the kneading process is supplied with the following Figure 2 The pelletized masterbatch (intermediate resin composition) produced by the kneading device 100 shown and the materials constituting the above-mentioned plastic composition (plastic resin, filler, other components, etc.) are then kneaded in the first extruder 110a to obtain the above-mentioned plastic composition.

[0120] The flow path forming device 5 is installed at the downstream end of the second extruder 110b in the moving direction of the plastic composition. Figure 1 The flow path 30 of the flow path forming device 5 shown is used to foam the plastic composition at the outlet of the flow path 30 to extrusion-form the foamed sheet.

[0121] Next, each step of the extrusion molding method and an apparatus for performing each step will be specifically described by taking the case where an aliphatic polyester resin (polylactic acid) is used as the plastic resin as an example.

[0122] First, the kneading step will be described.

[0123] <Mixing process>

[0124] The kneading step is to knead the aliphatic polyester resin as a plastic resin and a crosslinking agent in the presence of a compressive fluid at a temperature lower than the melting point of the aliphatic polyester resin to obtain an aliphatic polyester resin composition as a plastic composition.

[0125] There are two reasons for kneading at a temperature lower than the melting point of the aliphatic polyester resin. The first reason is that the aliphatic polyester resin has a property that the melt viscosity decreases rapidly after the melting point, so even if the additive is dispersed in the resin by kneading, the additive is difficult to aggregate.

[0126] The second reason is that when the aliphatic polyester resin and the crosslinking agent are kneaded at a high temperature, the crosslinking reaction is accelerated, the aliphatic polyester resin is polymerized, and the gel fraction of the resin composition is increased.

[0127] In order to knead the aliphatic polyester resin at a temperature lower than the melting point, the resin is impregnated with a compressive fluid. By impregnating the aliphatic polyester resin with a compressive fluid, the resin can be kneaded at a high viscosity at a temperature lower than the melting point of the aliphatic polyester resin, and additives such as unreacted crosslinking agents can be uniformly dispersed in the aliphatic polyester resin.

[0128] In the past, when kneading aliphatic polyester resin compositions, especially kneading polylactic acid and additives, polylactic acid can only be kneaded at a low viscosity below the melt viscosity at a temperature above the melting point of polylactic acid, and there are problems such as dispersibility of additives. However, in the present embodiment, as described above, by impregnating the compressible fluid, kneading can be performed well at a temperature lower than the melting point of polylactic acid even if the polylactic acid is in a high viscosity state, thereby improving the dispersibility of the additive.

[0129] Here, the compressible fluid impregnated in the aliphatic polyester resin is described. - Compressible fluid - A compressible fluid is a fluid whose density changes according to a change in pressure. For example, a supercritical fluid is a fluid that exists as a non-cohesive high-density fluid in a temperature and pressure region exceeding the limit (critical point) at which gas and liquid can coexist, and does not condense even when compressed. In addition, a liquefied gas obtained by compressing a substance that is in a gaseous state at normal temperature (25°C) and normal pressure (1 atmosphere) and a high-pressure gas (compressible gas) with a pressure of more than 1 / 2 of the critical pressure can be cited.

[0130] As substances that can be used as compressive fluids, for example, carbon monoxide, carbon dioxide, nitrous oxide, nitrogen, methane, ethane, propane, 2,3-dimethylbutane, ethylene, dimethyl ether, etc. can be listed. Among them, carbon dioxide is preferred from the following four points of view. That is, the critical pressure is about 7.4 MPa, the critical temperature is about 31°C, and a supercritical state can be easily formed (supercritical fluid can be formed). It is non-flammable and easy to use. As mentioned above, it can be used as a foaming agent. In the molded foam sheet, it is easy to become a state that does not substantially contain volatile components. These compressive fluids can be used alone or in combination of two or more.

[0131] Since the solubility of the compressive fluid varies depending on the combination of the resin type and the compressive fluid, the temperature, and the pressure, the supply amount of the compressive fluid must be appropriately adjusted.

[0132] For example, if it is a combination of polylactic acid and carbon dioxide, it is preferably 2% by mass or more and 30% by mass or less. When the supply of carbon dioxide is 2% by mass or more, the problem of limited plasticizing effect can be prevented. When the supply of carbon dioxide is 30% by mass or less, due to the problem of carbon dioxide and polylactic acid phase separation, additives such as crosslinking agents cannot be fully dispersed.

[0133] -Mixing device-

[0134] Next, a kneading device for performing the above-mentioned kneading step will be described.

[0135] As the kneading apparatus used for producing the aliphatic polyester resin composition, a continuous process or a batch process may be adopted, but it is preferred to appropriately select the reaction process in consideration of the apparatus efficiency, the characteristics and quality of the product, and the like.

[0136] As a kneading device, from the viewpoint of being able to cope with a viscosity suitable for kneading, a single-screw extruder, a twin-screw extruder, a kneader, a screwless basket-type stirring tank, BIVOLAK manufactured by Sumitomo Heavy Industries, Ltd., N-SCR manufactured by Mitsubishi Heavy Industries, Ltd., a tubular polymerization tank having a double-ring blade, a grid blade, or a Kenix-type, Sulzer-type SMLX-type static mixer manufactured by Hitachi, Ltd., etc. can be used. From the viewpoint of color tone, a finisher, N-SCR, a twin-screw extruder, etc. as a self-cleaning polymerization device can be listed. Among them, from the viewpoints of production efficiency, color tone, stability and heat resistance of the resin, a finisher and N-SCR are preferred.

[0137] Figure 2 FIG. 1 is a schematic diagram of an example of a kneading device 100 .

[0138] Figure 2 The kneading device 100 shown used a twin-screw extruder (manufactured by JSW Corporation) with a screw diameter of 42 mm, a screw length of L, and a screw diameter of D, where L / D was 48.

[0139] The kneading device 100 includes a raw material mixing / melting zone a, a compressive fluid supply zone b, a kneading zone c, a compressive fluid removal zone d, and a molding processing zone e.

[0140] -Raw material mixing / melting area a-

[0141] In the raw material mixing / melting area, as raw materials constituting the above-mentioned plastic composition, a granular aliphatic polyester resin and a crosslinking agent are supplied from the first quantitative feeder 1 and the second quantitative feeder 2. In addition, a filler or other components (thermal stabilizer, antioxidant, plasticizer and lubricant) constituting the above-mentioned plastic composition that do not react even at high temperatures may be additionally supplied.

[0142] Then, the temperature of the supplied raw material is increased in the raw material mixing / melting zone a. The heating temperature is set to be equal to or higher than the melting temperature of the aliphatic polyester resin to melt the supplied pelletized aliphatic polyester resin.

[0143] - Compressible fluid supply area b-

[0144] In the compressive fluid supplying area, the compressive fluid is supplied to the resin in a molten state by the metering pump 3 as the compressive fluid supplying unit, and the molten resin is plasticized.

[0145] -Mixing area c-

[0146] The kneading area kneads the raw materials supplied to the raw material mixing / melting area a. In the kneading area, the temperature is set to a viscosity suitable for kneading of the aliphatic polyester resin composition. The set temperature varies according to the specifications of the reaction device, the type of resin, the structure of the resin, the molecular weight, etc., and is therefore not particularly limited and can be appropriately changed. For example, in the case of commercially available polylactic acid having a weight-average molecular weight (Mw) of about 200,000, the usual kneading is carried out at the melting point of the polylactic acid + 10°C to 20°C, but in the present embodiment, the kneading can be carried out at a temperature lower than the melting point of the polylactic acid.

[0147] Thus, in the kneading device 100 of the present embodiment, kneading is performed at a temperature lower than the melting point of the aliphatic polyester resin, so that kneading can be performed at a relatively high viscosity as described above, and additives such as a crosslinking agent can be well dispersed in the resin. In addition, there is no particular limitation as long as it is a temperature lower than the melting point of the resin, but in order to suppress the crosslinking reaction of the crosslinking agent mixed in this area, in the case of commercially available polylactic acid, it is preferably set to -30°C to -80°C from the melting point of the polylactic acid.

[0148] - Compressible fluid removal area d-

[0149] In the compressive fluid removal zone d, the pressure valve provided in the extruder is opened to discharge the compressive fluid to the outside.

[0150] -Forming processing area e-

[0151] In the molding process area e, an intermediate resin composition (master batch) in which at least an aliphatic polyester resin and a crosslinking agent are mixed is molded into an appropriate arbitrary shape such as pellets.

[0152] The pressure of each area in the extruder can be appropriately set. In this embodiment, the pressure from the compressive fluid supply area b to the compressive fluid removal area d is 7 MPa.

[0153] Next, the foaming step of the extrusion molding method will be described.

[0154] <Foaming process>

[0155] The foaming process is a process of expanding the above-mentioned foaming agent to foam the aliphatic polyester resin composition. When a compressible fluid (compressed gas such as carbon dioxide or nitrogen) is used as the foaming agent, the compressible fluid is expanded and removed by opening the pressure, thereby foaming the aliphatic polyester resin composition. Specifically, the pressure is opened by extruding from the flow path outlet of the flow path forming device 5. Under the atmosphere, the compressive fluid is slowly replaced by air and removed from the foam sheet. As the temperature during the foaming process, it is preferably heated to near the melting point of the resin.

[0156] In the case of foaming when the impregnated compressive fluid is used as a foaming agent in the kneading step, in the foaming step, the solubility of the compressive fluid dissolved in the aliphatic polyester composition is reduced by reducing pressure or heating, etc., and an operation is performed to reach supersaturation. It is believed that by reducing the solubility of the compressive fluid, foaming cores are mainly formed at the interface with the foaming core material (filler), and the compressive fluid dissolved in the aliphatic polyester composition diffuses into the foaming cores, causing the foaming cores to grow into bubbles, thereby obtaining a foamed body.

[0157] Since foaming is carried out starting from the foaming core material (filler), only when the foaming core material (filler) is evenly dispersed in the resin can a foam sheet with uniform and fine foaming be manufactured. Even if a foaming core material (filler) is not used, a small amount of crystals generated in the kneading area actually acts as a foaming core material, so a foam sheet with uniform and fine foaming can be manufactured. However, if crystallization is excessive, the fluidity of the composition will be reduced, and foaming itself may become difficult, so it is preferred to add a foaming core material (filler).

[0158] Next, other steps of the extrusion molding method will be described.

[0159] <Other Processes>

[0160] The other steps are not particularly limited as long as they are steps generally performed in the production of plastic foam sheets, and can be appropriately selected depending on the purpose. Examples thereof include a molding step for processing into a sheet.

[0161] Examples of the molding process include vacuum molding, pressure molding, press molding, etc. In the present embodiment, a cylindrical masterbatch is molded, and the masterbatch is formed into a sheet shape by the molding process, thereby obtaining a foamed sheet.

[0162] Next, an extrusion molding device for molding the foamed sheet will be described.

[0163] -Extrusion molding device 1

[0164] Figure 3 Shown is an exemplary diagram of an extrusion molding device 110 .

[0165] like Figure 3 As shown, the extrusion molding device 110 includes a first extruder 110a for performing a kneading process and a second extruder 110b for performing a foaming process. A foaming device 110a is provided at the downstream end of the second extruder 110b in the direction of movement of the plastic composition. Figure 1 The flow path forming device 5 shown.

[0166] The first extruder 110a and the second extruder 110b are used Figure 2 The kneading device 100 described above is similarly a twin-screw extruder (manufactured by JSW Corporation).

[0167] The extrusion molding device 110 includes a raw material mixing / melting zone a, a compressive fluid supply zone b, a kneading zone c, and a heating zone d.

[0168] -Raw material mixing / melting area a-

[0169] In the raw material mixing / melting area a, Figure 2 The raw material mixing / melting area of ​​the kneading device shown in the figure performs the same process. That is, the raw materials are supplied from the first quantitative feeder 1 and the second quantitative feeder 2 and mixed, and the supplied raw materials are heated to melt the resin.

[0170] The raw materials supplied from the first quantitative feeder 1 and the second quantitative feeder 2 are Figure 2 The kneading device 100 shown molds a masterbatch (an intermediate resin composition in which at least an aliphatic polyester resin and a crosslinking agent are mixed), a filler or other components such as the above-mentioned heat stabilizer, antioxidant, plasticizer, lubricant, etc.

[0171] In addition, in Figure 2When the concentration of the crosslinking agent contained in the masterbatch molded by the kneading device 100 shown is high, additional resin particles are supplied to adjust the crosslinking agent concentration to an appropriate value. In addition, the type of the additionally supplied plastic resin is not particularly limited, and it is preferably an aliphatic polyester resin that is the same as the plastic resin in the masterbatch. By using the same resin as the plastic resin in the masterbatch, the resin is uniformly mixed in the kneading process, and the unreacted crosslinking agent contained is also uniformly dispersed, which is preferred. In addition, the masterbatch already contains a crosslinking agent, but the crosslinking agent can also be further supplied.

[0172] In the above, the filler as the foaming core material is added in the extrusion molding device 110, but it can also be added in Figure 2 The filler is added when molding a masterbatch (intermediate resin composition) in the kneading device 100 shown. Alternatively, the filler may be added in both the kneading step when molding the masterbatch and the kneading step when molding the foamed sheet.

[0173] - Compressible fluid supply area b-

[0174] In the compressible fluid supply area, Figure 2 Similarly, in the compressive fluid supplying region of the kneading device 100 shown, the compressive fluid is supplied to the resin in a molten state by the metering pump 3 as the compressive fluid supplying unit, thereby plasticizing the molten resin.

[0175] As the compressive fluid impregnated during the molding of the foam sheet, the compressive fluid impregnated during the molding of the masterbatch (intermediate resin composition) using the mixing device 100 can be used. As the compressive fluid impregnated during the molding of the foam sheet, carbon dioxide is preferred from the above four points of view. The compressive fluid impregnated during the molding of the foam sheet can also be used alone or in combination of two or more. By impregnating the compressive fluid, as described above, mixing can be performed well even in a high viscosity state. Thereby, the filler (foaming core material) can be evenly dispersed in the plastic resin, and a foam sheet with uniform and fine foaming can be manufactured.

[0176] In addition, in the present embodiment, the compressive fluid supplied in the compressive fluid supply area b is used as a foaming agent. By using the compressive fluid supplied in the compressive fluid supply area b as a foaming agent, kneading and foaming can be performed through a series of processes, which is more preferable as a manufacturing method from the viewpoint of reducing environmental load. Regarding the supply amount of the compressive fluid, as described above, when the aliphatic polyester resin composition is set to 100 parts by mass, the supply amount of carbon dioxide is preferably 2% by mass or more and 30% by mass or less.

[0177] In order to achieve good kneading even in a high viscosity state, a foaming agent may be used separately from the compressible fluid to be impregnated. As the foaming agent, the foaming agent described in the description of the plastic composition may be used.

[0178] -Mixing area c-

[0179] In the mixing area c, Figure 2 The kneading zone of the kneading device shown in the figure kneads the raw materials supplied to the raw material mixing / melting zone a at a temperature lower than the melting temperature of the aliphatic polyester resin.

[0180] - Heating area d

[0181] The aliphatic polyester resin kneaded in the kneading area c of the first extruder 110a is supplied to the heating area d of the second extruder 110b. In the heating area d, the aliphatic polyester resin supplied from the first extruder 110a is further kneaded. As the set temperature of the heating area d, it is preferably set so that the temperature of the plastic composition when extruded from the flow path outlet of the flow path forming device 5 is lower than the melting point of the plastic composition.

[0182] By making the temperature of the plastic composition when extruded from the flow channel outlet of the flow channel forming device 5 lower than the melting point of the plastic composition, the viscosity of the plastic composition can be increased, and thus a foamed plastic having a high expansion ratio can be obtained.

[0183] The aliphatic polyester resin further kneaded in the heating zone d is extruded into the flow path 30 of the flow path forming device 5 installed at the downstream end of the second extruder 110b in the moving direction of the plastic composition. Figure 1 The flow path 30 of the flow path forming device shown in the figure is opened, and the pressure is released at the outlet of the flow path 30 to expand and remove the compressible fluid as the foaming agent, thereby extruding and foaming the aliphatic polyester resin composition. The extrusion-foamed foamed sheet 4 is wound around a mandrel.

[0184] In this embodiment, as the flow path forming device 5, a Figure 1 The flow path forming device 5 described above. Specifically, the flow path forming device 5 is used in which the average value of the maximum droplet weight G within the range of 3 mm from the flow path outlet of the first flow path forming surface 40 and the second flow path forming surface 50 is 8 μg or more and 25 μg or less. As a result, the flow resistance of the aliphatic polyester resin composition to be foamed to the flow path forming surface can be made within an appropriate range. As a result, as described above, the flow stability of the aliphatic polyester resin composition to be foamed can be maintained and the foam sheet 4 with suppressed thickness can be obtained. In addition, the friction between the flow path forming surface and the aliphatic polyester resin composition is suppressed, and the roughness of the surface is suppressed, and a foam sheet with good appearance can be obtained.

[0185] In this embodiment, by Figure 2 The kneading device 100 shown molds the intermediate resin composition (masterbatch), and kneads the intermediate resin composition and additives such as fillers through the first extruder 110a of the extrusion molding device 110 to produce an aliphatic polyester resin composition. However, this structure is not limited to this. The aliphatic polyester resin composition may be produced in the kneading process of the extrusion molding device 110 without molding the intermediate resin composition (masterbatch).

[0186] <Artifacts>

[0187] The foam sheet obtained by this embodiment can be used directly or as a manufactured product. The foam sheet of this embodiment is light and heat-resistant, so it is suitable for use as a food container or tableware. In addition, although it is suitable as a heat-resistant food container, it is not limited to such use. In addition, it can also be used by directly printing on the foam sheet.

[0188] In addition, there is no particular restriction on the manufactured product using the obtained foam sheet, and it can be appropriately changed. The manufactured product includes the foam sheet and contains other components as required. As other components, as long as they are components used in common resin products, there is no particular restriction, and they can be appropriately selected according to the purpose.

[0189] The obtained foamed sheet can also be processed as the product of the present invention. There is no particular restriction on the processing of the foamed sheet, and for example, a process using a mold to process and obtain a product can be used. There is no particular restriction on the processing method of the sheet using the mold, and a conventional method of thermoplastic resin can be used, for example, vacuum forming, pressure forming, vacuum pressure forming, pressurization forming, etc. can be cited.

[0190] Manufactured products (also called consumer materials) include, for example, packaging containers, trays, tableware, cutlery, etc. The concept of manufactured products includes not only manufactured products as a single unit, but also parts composed of manufactured products such as a handle of a tray, products including manufactured products such as a tray with a handle, etc. In addition, manufactured products include bags, stationery, daily necessities, etc.

[0191] The amount of crosslinking in the obtained foamed sheet varies depending on the molecular weight of the resin used and the molecular weight distribution of the resin. In particular, when a biodegradable resin is used as the aliphatic polyester resin, it is preferably adjusted to 3% by mass or less in order not to impair the biodegradability.

[0192] In addition, the amount of the foaming core material (filler) in the foam sheet is preferably adjusted to 10 parts by mass or less. If it exceeds 10 parts by mass, the physical properties of the foam sheet may become hard and brittle. In particular, when a biodegradable resin is used as the aliphatic polyester resin, it is preferred that the content of the foaming core material with poor biodegradability is less, and more preferably adjusted to 1 part by mass or less.

[0193] In addition, when using a biodegradable resin as the aliphatic polyester resin, from the viewpoint of biodegradability and recyclability (easy recycling), it is preferred that the biodegradable resin is 90% by mass or more relative to the total amount of organic matter in the foamed sheet. More preferably, it is 98% by mass or more. If it is 90% by mass or more, even if the polylactic acid is biodegraded, the problem of other components remaining that are not biodegraded can be prevented. If it is less than 90% by mass, good biodegradability cannot be obtained.

[0194] The organic matter in the foamed sheet mainly includes biodegradable resins such as polylactic acid, and the substances other than polylactic acid include, for example, organic core materials, crosslinking agents, etc. When an inorganic core material is used as the foaming core material, the inorganic core material does not belong to the organic matter.

[0195] -Method for measuring the content ratio of polylactic acid-

[0196] The content ratio of polylactic acid in the foamed sheet can be calculated from the ratio of the added materials (the raw materials supplied in the raw material mixing / melting area a of the extrusion molding device). If the material ratio is unknown, for example, the following GCMS analysis can be performed to determine the composition by comparing with a known polylactic acid as a standard sample. If necessary, the area ratio of the spectrum measured by NMR or other analytical methods can also be combined for calculation.

[0197] [Measurement by GCMS analysis]

[0198] GCMS: QP2010 manufactured by Shimadzu Corporation; auxiliary equipment Frontier Laboratories LtdPy3030D

[0199] Separation column: Frontier Laboratories Ltd Ultra ALLOY UA5-30M-0.25F

[0200] Sample heating temperature: 300℃

[0201] Column oven temperature: 50°C (hold for 1 minute) ~ temperature rise 15°C / minute ~ 320°C (6 minutes)

[0202] ·Ionization method: Electron Ionization (EI) method

[0203] Detection mass range: 25~700(m / z)

[0204] As a supplement, the content ratio of polylactic acid in the foamed sheet can be obtained, for example, by analyzing using a gas chromatography mass spectrometer (GC-MS) and using a known polylactic acid as a standard sample to obtain a calibration curve in advance, thereby obtaining the ratio of polylactic acid in the foamed sheet. In addition, at this time, when an organic nucleating agent is identified by library retrieval of a mass spectrum, the amount of addition can also be quantified by making a calibration curve. If necessary, it can also be calculated by combining the area ratio of the spectrum measured by NMR or other analytical methods.

[0205] Next, a verification experiment performed by the technicians of the present invention will be described.

[0206] [Verification test]

[0207] First, the flow channel forming devices of Examples 1 to 5 and Comparative Examples 1 to 3 used in the verification test will be described.

[0208] [Example 1]

[0209] The first flow path forming member 10 and the second flow path forming member 20 made of S45C (manufactured by Misumi Co., Ltd.) were processed by sandblasting (using alumina abrasive media for sandblasting manufactured by MonotaRO, with a processing angle of about 45 degrees) to form a Figure 1 Then, a silicone release coating of about 100 μm is sprayed on the flow channel forming surfaces 40 and 50 processed by sandblasting, and then fired.

[0210] Then, an aging treatment was performed at 220° C., and then the flow path forming surfaces 40 and 50 were wiped with toluene and finally processed with #2000 sandpaper to manufacture the first flow path forming surface 40 and the second flow path forming surface 50 .

[0211] Water was dripped onto the first flow path forming surface 40 and the second flow path forming surface 50 within a range of 3 mm from the outlet of the flow path 30, and the maximum drop weight G was measured by the above-mentioned method of measuring the maximum drop weight G at which the drop does not slide off. Both measurements were 10 μg, and the average value of the maximum drop weight was 10 μg.

[0212] In addition, the contact angle was measured by the contact angle measurement method described above. The contact angle measurement method described above is a measurement method in which the measurement error is not zero. Therefore, the first flow path forming surface 40 and the second flow path forming surface 50 are measured three times while changing the position within a range of 3 mm from the flow path 30 outlet to confirm the change mode. When the change is outside the specified range, the number of measurements is further increased. Then, the average value of these measured values ​​is calculated to obtain the contact angle. The obtained contact angle is 88.2°.

[0213] In addition, the arithmetic mean roughness Ra and the average length Rsm of the roughness curve element of the first flow path forming surface 40 and the second flow path forming surface 50 within a range of 3 mm from the outlet of the flow path 30 are measured by the measurement method of the above-mentioned surface roughness parameters Rsm, Ra, and Rk. The measurement method of the above-mentioned surface roughness parameters Rsm, Ra, and Rk is also a measurement method in which the measurement error is not zero. Therefore, similarly to the contact angle, the position is changed while measuring 3 times to confirm the change mode. When the change is large, the number of measurements is further increased. Then, the average values ​​of these measured values ​​are calculated to obtain the arithmetic mean roughness Ra and the average length Rsm of the roughness curve element. The arithmetic mean roughness Ra is 1.29μm, and the average length Rsm of the roughness curve element is 91.6μm.

[0214] In addition, depending on the shape of the flow path, if the range of 3 mm from the outlet of the flow path 30 is not suitable for the measurement of the maximum droplet weight G, contact angle, surface roughness Rsm, and Ra, the same treatment as that near the flow path outlet of the flow path forming surface (within the range of 3 mm from the outlet of the flow path 30) can be implemented, and the measurement can be performed at a position where the surface state is equivalent to that near the flow path outlet. In addition, a test piece that has been treated the same as that near the flow path outlet (within the range of 3 mm from the outlet of the flow path 30) can be prepared for substitute measurement. In addition, for the flow path forming surface of one of the first flow path forming surface 40 and the second flow path forming surface 50, if the measurement near the flow path outlet can be performed, the first flow path forming surface 40 and the second flow path forming surface 50 can be processed in the same batch, and only the measurement value of one side can be used as a substitute.

[0215] [Example 2]

[0216] Example 2 is the same as Example 1 except that the coating material of the first flow path forming surface 40 and the second flow path forming surface 50 is changed from a silicone release coating to a fluorine release coating. The maximum droplet weight G of each flow path forming surface 40 and 50 is measured in the same way as in Example 1, and the result is that the average value of the maximum droplet weight G is 10μg. In addition, the average value of the contact angle is 83.3°, the average value of the arithmetic mean roughness Ra is 1.26μm, and the average value of the roughness curve element average length Rsm is 105μm.

[0217] [Example 3]

[0218] Example 3 is the same as Example 1 except that the material of each flow path forming member 10, 20 is changed from S45C to hard chrome plating. The maximum drop weight G of each flow path forming surface 40, 50 is measured in the same manner as in Example 1, and the result is that the average value of the maximum drop weight G is 15 μg. In addition, the average value of the contact angle is 60.3°, the average value of the arithmetic mean roughness Ra is 0.21 μm, and the average value of the roughness curve element average length Rsm is 67.7 μm.

[0219] [Example 4]

[0220] Example 4 is the same as Example 2 except that the wiping operation after aging is performed using a solvent equivalent to hexane. The maximum droplet weight G of each flow path forming surface 40, 50 is measured in the same way as in Example 1, and the result is that the average value of the maximum droplet weight is 8μg. In addition, the average value of the contact angle is 106.6°, the average value of the arithmetic mean roughness Ra is 1.35μm, and the average value of the roughness curve element average length Rsm is 122.8μm.

[0221] [Example 5]

[0222] Example 5 is the same as Example 1 except that the #2000 sandpaper treatment is performed for a longer time than Example 1. The maximum droplet weight G of each flow path forming surface 40, 50 is measured in the same manner as in Example 1, and the result is that the average value of the maximum droplet weight G is 25 μg. In addition, the average value of the contact angle is 57.6°, the average value of the arithmetic mean roughness Ra is 1.02 μm, and the average value of the roughness curve element average length Rsm is 138.0 μm.

[0223] [Comparative Example 1]

[0224] Comparative Example 1 is the same as Example 2 except that the coating is not treated after firing (aging treatment, sandpaper treatment) and the new product state is maintained. The maximum droplet weight G of each flow path forming surface 40, 50 is measured in the same way as in Example 1, and the result is that the average value of the maximum droplet weight G is 5μg. In addition, the average value of the contact angle is 102°, the average value of the arithmetic mean roughness Ra is 1.24μm, and the average value of the roughness curve element average length Rsm is 99.4μm.

[0225] [Comparative Example 2]

[0226] Comparative Example 2 is the same as Example 1 except that the #2000 sandpaper treatment is changed to the #1000 sandpaper treatment. The maximum droplet weight G of each flow path forming surface 40, 50 is measured in the same manner as in Example 1, and the result is that the average value of the maximum droplet weight G is 30 μg. In addition, the average value of the contact angle is 91.2°, the average value of the arithmetic mean roughness Ra is 1.57 μm, and the average value of the roughness curve element average length Rsm is 75.2 μm.

[0227] [Comparative Example 3]

[0228] Comparative Example 3 is an example of manufacturing the first flow path forming surface 40 and the second flow path forming surface 50 by sandblasting only the portion of the first flow path forming component 10 and the second flow path forming component 20 of material S45C. The maximum droplet weight G was measured for each flow path forming surface 40 and 50 in the same manner as in Example 1, and the result was that the average value of the maximum droplet weight G was 60 μg. In addition, the average value of the contact angle was 121°, the average value of the arithmetic mean roughness Ra was 2.07 μm, and the average value of the roughness curve element average length Rsm was 52.4 μm.

[0229] The verification test was carried out by installing the flow path forming devices of the above-mentioned embodiments 1 to 5 and comparative examples 1 to 3 on Figure 3 The foamed sheet was molded on the extrusion molding device 110 shown, and the bulk density, deviation, and appearance were measured and evaluated.

[0230] The mixing conditions in the verification test are as follows.

[0231] Plastic resin: Polylactic acid A (manufactured by Nature Works, 4032D, melting point 168°C)

[0232] Filler: Magnesite (manufactured by Kamishima Chemical Industry Co., Ltd., MS-S, number average particle size 1.2 μm)

[0233] Total flow rate of polylactic acid and filler: 10 kg / hr (polylactic acid: 9 kg / hr, filler: 1 kg / hr)

[0234] Compressible fluid: Carbon dioxide (flow rate: 0.9 kg / h (equivalent to 10% by mass relative to polylactic acid))

[0235] The temperature of each zone is: raw material mixing / melting zone a and compressive fluid supply zone b: 190°C, kneading zone c: 130°C, compressive fluid removal zone d: 190°C, and molding processing zone e: 190°C. The pressure of each zone is 10.0 MPa from the compressive fluid supply zone b to the kneading zone c, and the pressure of the compressive fluid removal zone d is 0.5 MPa, and an intermediate resin composition is obtained. The molding of the foam sheet is carried out at a total flow rate of 30 kg / hr, of which 1.5 kg / hr is carbon dioxide and 20 kg / hr is polylactic acid A. The zones a, b, and c are at the same temperature as the kneading. The zone d is 150°C, and the pressure of the flow path 30 of the flow path forming device 5 is 5 MPa to mold a foam sheet with a thickness of 1000 μm. Then, the obtained foam sheet is evaluated for bulk density, deviation and appearance.

[0236] <Bulk density>

[0237] The bulk density is measured as follows. Specifically, the foamed sheet is left to stand for more than 24 hours in an environment adjusted to a temperature of 23°C and a relative humidity of 50%, and a 50 mm × 50 mm test piece is cut out. The bulk density of the cut sample is obtained by the in-liquid weighing method using an automatic specific gravity meter (DSG-1, manufactured by Toyo Seiki Seisakusho Co., Ltd.). This is calculated by accurately weighing the weight (g) of the foamed sheet in the atmosphere, and then accurately weighing the weight (g) of the foamed sheet in water using the following formula.

[0238] Bulk density [g / cm 3 ] = weight of sample in the atmosphere [g] / {(weight of sample in the atmosphere [g] - weight in liquid [g]) × liquid density [g / cm 3 ]}

[0239] <Appearance>

[0240] The appearance of the foamed sheet was evaluated as follows.

[0241] The surface and back of the obtained foamed sheet are analyzed by image processing, and an index that quantifies the poor appearance is used. The poor appearance has the following tendency: the larger the size and width of the solid foreign matter on the surface of the sheet, and the greater the difference in light and dark with the background, the worse the visual evaluation. Therefore, about 100 samples are visually evaluated by humans in advance, and the samples with poor appearance are given a sequence in terms of sensory perception. The image processing algorithm is fitted in a way with the highest consistency to quantify the poor appearance. Even the previous visual grade evaluation has no problem in essence, but from the perspective of efficiency and reproducibility, this index is used in the evaluation.

[0242] [Appearance evaluation]

[0243] The image processing described above is used to analyze and numerically represent the appearance defects. The appearance is then evaluated based on whether the value is less than 16, which is a range that can be used as a product.

[0244] <deviation>

[0245] The evaluation of the deviation was performed as follows.

[0246] The foam sheet was left to stand for more than 24 hours in an environment adjusted to a temperature of 23°C and a relative humidity of 50%, and a 50 mm × 50 mm test piece was cut out. For the cut test piece, the weight (g) of the foam sheet in the atmosphere was accurately weighed and divided by the sheet area of ​​50 mm × 50 mm to obtain the sheet weight per unit area. The standard deviation of 12 data obtained by measuring at 12 locations in the TD direction (the width direction of the foam sheet, the orthogonal direction of the extrusion direction) was divided by the 12-point average value, and the resulting value was taken as the deviation.

[0247] The deviation is evaluated based on whether it is less than 0.16, which is a range that can be used as a product. The deviation of the foamed sheet is more preferably less than 0.10, and further preferably less than 0.08.

[0248] As long as it is a parameter that reflects the deviation state of the flow in the TD direction (circumferential direction of the flow path 30), it is not necessary to stick to the sheet weight per unit area, and it can also be evaluated by foaming ratio, thickness, etc. In addition, the spatial resolution does not need to be 12 points, and as long as the resolution that can correctly identify the phenomenon and estimate the value of the product is set in advance, it can be replaced by a smaller number of measurements.

[0249] Then, the case where the number of appearance defects was less than 16 and the variation was less than 0.16 was evaluated as “○”, and the case where the number of appearance defects was more than 16 and the variation was more than 0.16 was evaluated as “×”.

[0250] The results of the verification test are shown in Table 1 below, Figure 4 It is a graph of the verification test results.

[0251] Table 1

[0252]

[0253] As shown in Table 1, in Comparative Example 1, in which the average value of the maximum droplet weight G was 5 μg, the appearance defect was 8.3, and although a very good result was obtained in the appearance evaluation, the deviation was 0.16 or more, and the deviation evaluation did not meet the standard.

[0254] This is considered to be because the average value of the maximum droplet weight G is 5 μg, and the plastic composition is in an excessively slippery state relative to the flow path forming surface. Therefore, it is considered that the back pressure in the flow path is reduced, the plastic composition cannot be extruded well, and the flow rate of the plastic composition extruded from the flow path outlet becomes unstable due to the spread in the direction orthogonal to the extrusion direction in the flow path. Therefore, it is considered that even if the contact angle is as high as 102°, the plastic composition cannot be stably ejected from the flow path outlet. As a result, it is considered that the thickness of the molded foam sheet cannot be suppressed, and the deviation exceeds 0.16.

[0255] In addition, the appearance and thickness variation of Comparative Examples 2 and 3, in which the average value of the maximum droplet weight G was 30 μg or more, did not meet the standards. This is because the average value of the maximum droplet weight G was 30 μg or more, so the plastic composition had difficulty sliding on the flow path forming surface, and the flow resistance of the plastic in the flow path to the flow path forming surface was large. As a result, the plastic composition could not be ejected smoothly from the flow path outlet, the surface rubbed against the flow path forming surface, the surface roughness was serious, the value of poor appearance was 16 or more, and the appearance did not meet the standards.

[0256] In addition, since the plastic composition has difficulty sliding relative to the flow path forming surface, the balance of flow resistance in the flow path is destroyed, and the flow rate of the plastic composition extruded from the flow path outlet becomes unstable. As a result, the deviation is also more than 0.16, which does not meet the standard.

[0257] In contrast, Examples 1 to 5, in which the average value of the maximum droplet weight G was 8 μg to 25 μg, all satisfied the standard in terms of variation and appearance and were evaluated as "○". Figure 4 The graph shown also confirms that if the average value of the maximum droplet weight G is 8μg to 25μg, the deviation and appearance meet the standard. This is because Examples 1 to 5 can make the sliding of the flow path forming surface relative to the plastic composition within an appropriate range, can suppress the reduction of the back pressure in the flow path, and can maintain the flow resistance in the flow path at a constant level. As a result, the flow rate of the plastic composition extruded from the flow path outlet is stable, the occurrence of uneven thickness is suppressed, and the deviation meets the standard (less than 0.16).

[0258] In addition, by making the sliding of the flow path forming surface relative to the plastic composition within an appropriate range, the friction between the plastic composition and the flow path forming surface at the flow path outlet is suppressed, the plastic composition is discharged smoothly, and the roughness of the surface of the foam sheet can be suppressed. As a result, the value of the poor appearance can meet the standard (less than 16).

[0259] In addition, in Examples 1 to 5, the arithmetic mean roughness Ra of the flow path forming surface is less than 1.5, the roughness curve element average length Rsm is 60 μm or more, and the surface roughness of the flow path forming surface is suppressed. As a result, since the surface roughness of the flow path forming surface can suppress the roughness of the surface of the foam sheet due to transfer to the surface of the foam sheet, the value of the poor appearance can meet the standard (less than 16).

[0260] In Examples 1 to 3, in which the average value of the maximum droplet weight G was 10 μg to 15 μg, the variation was suppressed to 0.08 or less, and uneven thickness of the molded product was suppressed well.

[0261] Although preferred embodiments of the present invention have been described above, the present invention is not limited to the above-mentioned specific embodiments, and various modifications and changes can be made within the scope of the concept of the present invention as described in the scope of rights unless otherwise specified in the above description.

[0262] The above description is just an example, and the following various methods all have unique effects.

[0263] (Method 1)

[0264] A flow path forming device 5, characterized in that it includes: a first flow path forming component 10 and a second flow path forming component 20, and a flow path 30 for a plastic composition to flow is formed by the first flow path forming component 10 and the second flow path forming component 20, water drops are dripped on the flow path forming surface of the first flow path forming component 10 and the second flow path forming component 20 within a range of 3 mm from the outlet of the flow path 30 to the upstream side of the flow direction of the plastic composition, and the maximum droplet weight G at which the water droplets do not slide down when the dripping surface of the flow path forming surface is tilted from a state parallel to the horizontal direction to a state parallel to the vertical direction is measured, and the average value of the maximum droplet weight of the flow path forming surface of the first flow path forming component and the maximum droplet weight of the flow path forming surface of the second flow path forming component is greater than 8μg and less than 25μg.

[0265] Patent Document 1 specifies the contact angle between the flow path forming surface and the plastic composition such as molten resin, and although the occurrence of uneven thickness of the molded product is suppressed and the appearance of the molded product is improved, even if the contact angle is adjusted to an appropriate range, the pressure near the flow path outlet cannot be well maintained, and sometimes the uneven thickness of the molded product is deteriorated, or the surface of the molded product is rough and the appearance is deteriorated. This can be considered that the above contact angle is not sufficient as an indicator value representing the slidability of the flow path forming surface.

[0266] Therefore, in the first embodiment, as an index value indicating the slidability of the flow path forming surface, the maximum droplet weight G that prevents the water droplet from sliding down when the water droplet landing surface of the flow path forming surface is tilted from a state parallel to the horizontal direction to a state parallel to the vertical direction is used. If the flow path forming surface is easy to slide, the water droplet is easy to slide down, and the maximum droplet weight G becomes light. On the other hand, if it is difficult to slide, the water droplet is difficult to slide down, and the maximum droplet weight G becomes heavy. Therefore, by defining the above-mentioned maximum droplet weight G, the slidability of the flow path forming surface with respect to the plastic composition can be made within a more appropriate range compared to the case of defining it by the contact angle.

[0267] Furthermore, as described in the above verification test, by setting the average value of the maximum droplet weight G to 8 μg or more and 25 μg or less, uneven thickness of the molded product can be suppressed and the appearance of the molded product can be improved.

[0268] (Method 2)

[0269] In Embodiment 1, the average value of the maximum droplet weight G is not less than 10 μg and not more than 15 μg.

[0270] Thereby, as shown in the verification test, the variation can be suppressed to 0.08 or less, and uneven thickness of the molded product can be suppressed favorably.

[0271] (Method 3)

[0272] In the embodiment 1 or 2, the contact angle between the flow channel forming surface of at least one of the first flow channel forming member 10 and the second flow channel forming member 20 and water is 55° or more and less than 110°.

[0273] Thus, the flow path forming surface can be formed by relatively inexpensive processing.

[0274] (Method 4)

[0275] In any of the first to third aspects, the flow channel forming surface of at least one of the first flow channel forming member 10 and the second flow channel forming member 20 has an arithmetic mean roughness Ra of less than 1.5 and a roughness curve element average length Rsm of 60 μm or more.

[0276] As described in the embodiment, this can suppress roughening of the surface of the molded product due to the transfer of the roughness of the flow channel forming surface to the molded product such as the foamed sheet, and can suppress degradation of the appearance of the molded product.

[0277] (Method 5)

[0278] In the extruder having the flow path forming device 5 and extruding the plastic composition from the flow path outlet of the flow path forming device 5, the flow path forming device of any one of the embodiments 1 to 4 is used as the flow path forming device.

[0279] This makes it possible to perform extrusion molding of a molded product with suppressed uneven thickness and good appearance.

[0280] (Method 6)

[0281] In the fifth embodiment, a plastic composition containing at least one incombustible gas and at least one plastic is extruded from an outlet of a flow path of a flow path forming device at a temperature lower than the melting point of the plastic to produce a foamed plastic.

[0282] Thereby, as described in the embodiment, a foaming core material such as a filler can be uniformly dispersed in a plastic resin, and a foamed sheet having uniform and fine foaming can be produced.

[0283] (Method 7)

[0284] In the embodiment 5 or 6, the plastic composition is extruded from the flow channel outlet of the flow channel forming device to produce a molded article containing 90% by weight or more of a biodegradable resin.

[0285] Thereby, as described in the embodiment, a molded article having good biodegradability can be produced.

[0286] (Method 8)

[0287] In Embodiment 7, the biodegradable resin is polylactic acid.

[0288] Thereby, as described in the embodiment, a molded product having a higher melting point, toughness, chemical resistance, etc. than other biodegradable plastics can be obtained.

[0289] (Method 9)

[0290] The foamed plastic sheet is formed by an extrusion device in any one of Modes 6 to 8.

[0291] Thereby, as described in the embodiment, it is possible to form a foamed plastic sheet with suppressed uneven thickness and good appearance.

Claims

1. A flow path forming device, characterized in that include: a first flow path forming member and a second flow path forming member, and The first flow path forming member and the second flow path forming member form a flow path for the plastic composition to flow. Water drops are dripped on the flow path forming surfaces of the first flow path forming member and the second flow path forming member forming the flow path within a range of 3 mm from the outlet of the flow path to the upstream side in the flow direction of the plastic composition, and the maximum drop weight at which the water drops do not slide down is measured when the dripping surface of the flow path forming surface is tilted from a state parallel to the horizontal direction to a state parallel to the vertical direction, An average value of the maximum droplet weight on the flow channel forming surface of the first flow channel forming member and the maximum droplet weight on the flow channel forming surface of the second flow channel forming member is 8 μg or more and 25 μg or less.

2. The flow path forming device according to claim 1, characterized in that: The average value of the maximum droplet weight is 10 μg or more and 15 μg or less.

3. The flow path forming device according to claim 1, characterized in that: A contact angle between a flow channel forming surface of at least one of the first flow channel forming member and the second flow channel forming member and water is equal to or greater than 55° and less than 110°.

4. The flow path forming device according to claim 1, characterized in that: The flow channel forming surface of at least one of the first flow channel forming member and the second flow channel forming member has an arithmetic mean roughness Ra of less than 1.5 and a roughness curve element average length Rsm of 60 μm or more.

5. An extrusion device having a flow path forming device, and extruding a plastic composition from an outlet of a flow path of the flow path forming device, characterized in that: As the flow path forming device, the flow path forming device according to claim 1 is used.

6. The extrusion device according to claim 5, characterized in that: A plastic composition containing at least one incombustible gas and at least one plastic is extruded from an outlet of the flow path of the flow path forming device at a temperature lower than the melting point of the plastic to produce a foamed plastic.

7. The extrusion device according to claim 5, characterized in that: The plastic composition is extruded from the outlet of the flow path of the flow path forming device to produce a molded article containing 90% by mass or more of a biodegradable resin.

8. The extrusion device according to claim 7, characterized in that: The biodegradable resin is polylactic acid.

9. A foamed plastic sheet, characterized in that: The molding is performed by the extrusion device according to claim 6.