Process method for improving airtight qualified rate of hemodialysis dry powder barrel

By using ultrasonic welding and injection molding in the production of hemodialysis dry powder barrels, combining the addition of nucleating agent and acetylated di-starch phosphate, and integrating the filter screen with the barrel lid, the poor sealing of the barrel lid and the barrel body is solved. The problem of this paper improves the product's air-tight pass rate and tensile strength, and reduces labor costs.

CN119058133AInactive Publication Date: 2024-12-03SHANGHAI JIQI BIOTECHNOLOGY CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202311479062.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-11-08
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

During use, the hemodialysis dry powder bucket is not sealed firmly between the barrel lid and the barrel body, which leads to water leakage, affecting the air-tight pass rate.

Method used

Ultrasonic welding process combined with injection molding process, by adding nucleating agent and acetylated di-starch phosphate during the injection molding process, the crystallinity and uniformity of the plastic are improved, and the filter mesh and the barrel lid are formed integrally to reduce clogging and optimize welding. Parameters to improve sealing.

Benefits of technology

It improves the air-tight pass rate of hemodialysis dry powder barrels, reduces labor costs, and enhances the tensile strength and sealing properties of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004537543450000011
    Figure HDA0004537543450000011
Patent Text Reader

Abstract

The invention belongs to the technical field of dry powder barrel production, and discloses a process method for improving the airtight qualified rate of a hemodialysis dry powder barrel, and the process method comprises the steps of material taking and mixing, heating and plasticizing, injection molding, cooling and forming, mold opening and welding. According to the dry powder barrel, the additive is added in the injection molding process, so that the barrel body and the barrel cover have excellent mechanical properties, the stability of subsequent ultrasonic welding is improved, and then the airtight qualification rate of the finished dry powder barrel is increased; the filter screen and the barrel cover are integrally formed, so that the blocking phenomenon can be effectively avoided, the qualified rate of products is increased, and the labor cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of dry powder barrel production, and more specifically, to a process method for improving the airtight qualification rate of hemodialysis dry powder barrels. Background Art

[0002] The dialysis dry powder barrel is a disposable product used in hemodialysis machines. The main structure of the dialysis dry powder barrel usually includes a barrel body and a barrel cover. The barrel body and the barrel cover are generally injection molded, and a filter screen is usually fixedly connected between the barrel body and the barrel cover.

[0003] In the production process of hemodialysis dry powder barrels, the barrel cover is usually welded to the upper end of the barrel body. However, in the actual production process, there is a phenomenon that the seal between the barrel cover and the barrel body is not firm, which indirectly leads to the problem of hemodialysis dry powder contacting with impurities in the air. Hemodialysis dry powder barrels need to be pressurized and filled with water during use. If the seal between the barrel cover and the barrel body is not firm, water leakage will occur, which seriously affects normal use. Therefore, how to improve the airtight qualification rate of hemodialysis dry powder barrels is an urgent problem to be solved in the current production of dry powder barrels. Summary of the invention

[0004] In order to solve the above problems, the present application provides a process method for improving the airtight qualification rate of hemodialysis dry powder barrels.

[0005] The present application provides a process for improving the airtight qualification rate of hemodialysis dry powder barrels using the following technical solutions:

[0006] A process for improving the airtight qualification rate of hemodialysis dry powder barrels comprises the following steps:

[0007] S1. Take the materials and mix them. Weigh the PP particles and additives and mix them evenly.

[0008] S2, heating and plasticizing, adding the mixed material into the injection molding machine for heating and plasticizing to form a molten plastic fluid;

[0009] S3, injection molding, pressurizing the molten plastic fluid and injecting it into the corresponding mold, maintaining the pressure at 80 bar for 20 seconds;

[0010] S4, cooling molding, using cooling water to cool the mold, wherein the cooling time of the barrel mold is 20s, and the cooling time of the barrel cover mold is 15s;

[0011] S5, opening the mold to obtain the formed barrel body and barrel cover;

[0012] S6. Welding: The barrel cover and the barrel mouth of the barrel body are welded and formed by ultrasonic welding.

[0013] Furthermore, the additives in S1 include a nucleating agent, a dispersing agent and acetylated distarch phosphate, the nucleating agent is a sorbitol nucleating agent, and the dispersing agent is stearamide.

[0014] Through the above technical scheme, the nucleating agent helps to improve the crystallinity of the injection molded product; the addition of acetylated distarch phosphate can reduce the surface tension of the PP particle melt on the one hand, and improve the compatibility of the nucleating agent with the PP particle melt; on the other hand, the acetylated distarch phosphate has strong adhesiveness, which enables the nucleating agent to better adhere to the dispersant, and improves the dispersion of the nucleating agent in the PP particle melt during the melting of the raw materials, thereby improving the crystallinity and uniformity of the injection molded product, making each part have the same shrinkage rate, reducing the thermal stress generated during the cooling molding process, and improving the tensile strength of the injection molded product.

[0015] Furthermore, the heating temperature in S2 is 200°C.

[0016] Furthermore, the mold temperature in S3 is 80°C.

[0017] Through the above technical solution, the mold is preheated before injection molding, which reduces the temperature difference between the molten liquid and the mold, reduces the thermal stress inside the plastic product, and improves the tensile strength of the product.

[0018] Furthermore, the barrel cover and the filter screen in S3 are formed by an integrated mold.

[0019] Through the above technical solution, the filter screen and the barrel cover are formed in one piece, which can effectively avoid clogging, improve the product qualification rate and reduce labor costs.

[0020] Furthermore, the temperature of the cooling water in S4 is 18°C.

[0021] Further, the welding process in S6 includes the following steps:

[0022] S601, debug ultrasonic welding machine;

[0023] S602, process the welding fixture to match the product surface;

[0024] S603, placing the injection molded barrel into the mold of the welding machine, and checking the dust condition at the edge of the barrel mouth;

[0025] S604, place the barrel cover on the barrel body, push it into place manually, confirm that the barrel cover fits the barrel body, and then start the ultrasonic welding machine to complete the welding.

[0026] S605. Check the sealing effect. There should be no overflow and no damage to the packaging material. Complete the welding of the barrel cover and the barrel body.

[0027] Through the above technical solution, the ultrasonic vibration welding head transmits ultrasonic energy to the welding surface of the plastic material. The friction between the molecules causes the bonding surface to generate high heat, causing the plastic to melt and join.

[0028] Furthermore, debugging the ultrasonic welding machine in S601 includes: pulling down the welding head when the air pressure is zero, observing whether the welding head can fully contact the workpiece placed in the bottom mold or slightly lower than the plastic part, and ensuring that the parts can be easily taken in and out; using a horizontal plate and an adjusting screw to adjust it horizontally, and using carbon paper and white paper to check; adjusting welding parameters includes time, pressure, descending speed, trigger pressure, amplitude and holding time.

[0029] Furthermore, the processing of the welding fixture in S602 includes: polishing the bottom fixture of the fixture to extend the service life of the ultrasonic fixture and avoid scratches on the appearance of the finished product; adjusting the ultrasonic fixture to surround the bottom of the product to be melted to avoid displacement of plastic parts caused by vibration waves during the melting process.

[0030] In summary, the present application includes at least one of the following beneficial technical effects:

[0031] (1) The present application adds additives during the injection molding process, so that the barrel body and barrel cover have excellent mechanical properties, improve the stability of subsequent ultrasonic welding, and thus improve the airtight qualification rate of the finished dry powder barrel;

[0032] (2) By integrating the filter screen with the barrel cover, blockage can be effectively avoided, the product qualification rate can be improved, and labor costs can be reduced. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 This is a flowchart of the application; DETAILED DESCRIPTION

[0034] The technical solutions in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application; obviously, the described embodiments are only part of the embodiments of the present application, rather than all the embodiments, and all other embodiments obtained by ordinary technicians in this field based on the embodiments in the present application without making creative work are within the scope of protection of the present application.

[0035] Embodiment 1:

[0036] The present application embodiment discloses a process for improving the airtight qualification rate of a hemodialysis dry powder barrel, comprising the following steps:

[0037] S1. Take the materials and mix them. Weigh the PP particles and additives and mix them evenly.

[0038] S2, heating and plasticizing, adding the mixed material into the injection molding machine for heating and plasticizing to form a molten plastic fluid;

[0039] S3, injection molding, pressurizing the molten plastic fluid and injecting it into the corresponding mold, maintaining the pressure at 80 bar for 20 seconds;

[0040] S4, cooling molding, using cooling water to cool the mold, wherein the cooling time of the barrel mold is 20s, and the cooling time of the barrel cover mold is 15s;

[0041] S5, opening the mold to obtain the formed barrel body and barrel cover;

[0042] S6. Welding: The barrel cover and the barrel mouth of the barrel body are welded and formed by ultrasonic welding.

[0043] Furthermore, the additives described in S1 include nucleating agents, dispersing agents and acetylated distarch phosphate, wherein the nucleating agent is a sorbitol nucleating agent, and the dispersing agent is stearamide. The nucleating agent helps to improve the crystallinity of the injection molded product; the addition of acetylated distarch phosphate can reduce the surface tension of the PP particle melt on the one hand, and improve the compatibility between the nucleating agent and the PP particle melt on the other hand, the acetylated distarch phosphate has strong adhesiveness, so that the nucleating agent can be better attached to the dispersing agent, and in the process of melting the raw materials, the dispersion of the nucleating agent in the PP particle melt is improved, the crystallinity and uniformity of the injection molded product are improved, and each part has the same shrinkage rate, which reduces the thermal stress generated during the cooling molding process, improves the tensile strength of the injection molded product, and then improves the strength of subsequent welding and the airtightness after molding.

[0044] Furthermore, the heating temperature in S2 is 200° C., and the mold temperature in S3 is 80° C. Preheating the mold before injection molding reduces the temperature difference between the molten liquid and the mold, reduces the thermal stress inside the plastic product, and improves the tensile strength of the product.

[0045] Furthermore, the barrel cover and the filter screen in S3 are formed in one piece, which can effectively avoid blockage, improve the product qualification rate and reduce labor costs.

[0046] Furthermore, the temperature of the cooling water in S4 is 18°C.

[0047] Further, the welding process in S6 includes the following steps:

[0048] S601, debug ultrasonic welding machine;

[0049] S602, process the welding fixture to match the product surface;

[0050] S603, placing the injection molded barrel into the mold of the welding machine, and checking the dust condition at the edge of the barrel mouth;

[0051] S604, place the barrel cover on the barrel body, push it into place manually, confirm that the barrel cover fits the barrel body, and then start the ultrasonic welding machine to complete the welding.

[0052] S605. Check the sealing effect. There should be no overflow and no damage to the packaging material. Complete the welding of the barrel cover and the barrel body.

[0053] The ultrasonic vibration welding head transmits ultrasonic energy to the welding surface of the plastic material. The friction between the molecules generates high heat on the bonding surface, causing the plastic to melt and join.

[0054] Furthermore, debugging the ultrasonic welding machine in S601 includes: pulling down the welding head when the air pressure is zero, observing whether the welding head can fully contact the workpiece placed in the bottom mold or slightly lower than the plastic part, and ensuring that the parts can be easily taken in and out; using a horizontal plate and an adjusting screw to adjust it horizontally, and using carbon paper and white paper to check; adjusting welding parameters includes time, pressure, descending speed, trigger pressure, amplitude and holding time.

[0055] Furthermore, the processing of the welding fixture in S602 includes: polishing the bottom fixture of the fixture to extend the service life of the ultrasonic fixture and avoid scratches on the appearance of the finished product; adjusting the ultrasonic fixture to surround the bottom of the product to be melted to avoid displacement of plastic parts caused by vibration waves during the melting process.

[0056] The process method for improving the airtight qualification rate of a hemodialysis dry powder barrel described in the present invention mainly comprises injection molding and welding. PP particles are molded by injection molding. Different process parameters have different effects on the size of the dry powder barrel molded by injection molding. By continuously adjusting the parameters, the sizes of the barrel cover and the barrel body can achieve the best effect of ultrasonic welding. The injection molding machine is equipped with a cooler, and the temperature is controlled by cooling water. For the barrel cover, the injection molding cooling time is adjusted from 12S to 15S, and the temperature is adjusted from 12℃-17℃ to 18℃. After the parameters are adjusted, the barrel cover is 0.05mm larger. For the barrel body, the injection molding cooling time is adjusted from 12S to 20S. After the parameters are adjusted, the outer diameter of the barrel body is 0.2mm larger. The injection molding parameters of the barrel cover are adjusted. This parameter is the optimal parameter and has the best effect in ultrasonic welding.

[0057] In terms of product structure, we increase the R angle design, optimize the sheet rib structure design, optimize the welding rib size, and add spark patterns in the corresponding area of ​​the welding rib to reduce overflow, increase strength, and increase sealing. The traditional barrel cover and filter are assembled separately after injection molding. The assembled cover will be blocked. The gas inspection process is modified to modify the product structure to form the small filter and barrel cover into one piece to solve the blockage problem, improve the pass rate, and reduce labor costs.

[0058] The injection molded barrel cover and barrel body are sealed by ultrasonic welding. Before welding, pull down the welding head when the air pressure is zero to observe whether the welding head can fully contact the workpiece placed in the bottom mold or slightly lower than the plastic part, and whether it can ensure convenient access to the workpiece. Use the horizontal plate and adjusting screws to adjust it horizontally, and use carbon paper and white paper for inspection. When welding, weld it evenly under pressure. In order to prevent the surface of the workpiece from being crushed by the pressure, the mold needs to be realigned. The adjustment of welding parameters is: time, pressure, descent speed, trigger pressure, amplitude, holding time and other parameters to meet the welding requirements.

[0059] Place the injection-molded barrel into the mold and check whether there is dust on the edge of the barrel mouth. If there is dust, wipe it clean. Put the barrel cover on the barrel mouth and push it into place manually / press the handle to put it into place. After confirming that the barrel cover fits the barrel body, press the start button and the ultrasonic welding machine will automatically complete the welding. The ultrasonic vibration welding head transmits ultrasonic energy to the welding surface of the plastic material. The friction between molecules causes high heat to be generated on the bonding surface, causing the plastic to melt and join. During the ultrasonic welding operation, check the sealing effect. There should be no overflow and the packaging material should not be damaged.

[0060] The contact surface shape of the ultrasonic fixture itself is best matched with the product surface to avoid damage to the gap between the two welded parts. For easy placement, 10 threads are reserved. In order to extend the service life of the ultrasonic fixture and avoid scratches on the finished product, the bottom fixture is polished. The ultrasonic fixture surrounds the bottom and surroundings of the product to be melted, providing better support and avoiding displacement of plastic parts caused by vibration waves during the melting process.

[0061] The welding qualification rate is improved through injection molding process, product structure and welding tooling, and continuous debugging proves that this process method has a good welding qualification rate.

[0062] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.

Claims

1. A process for improving the airtight qualification rate of hemodialysis dry powder barrels, characterized in that: The following steps are involved: S1. Take the materials and mix them. Weigh the PP particles and additives and mix them evenly. S2, heating and plasticizing, adding the mixed material into the injection molding machine for heating and plasticizing to form a molten plastic fluid; S3, injection molding, pressurizing the molten plastic fluid and injecting it into the corresponding mold, maintaining the pressure at 80 bar for 20 seconds; S4, cooling molding, using cooling water to cool the mold, wherein the cooling time of the barrel mold is 20s, and the cooling time of the barrel cover mold is 15s; S5, opening the mold to obtain the formed barrel body and barrel cover; S6. Welding: The barrel cover and the barrel mouth of the barrel body are welded and formed by ultrasonic welding.

2. The process for improving the airtight qualification rate of hemodialysis dry powder barrels according to claim 1 is characterized in that: The additives in S1 include a nucleating agent, a dispersing agent and acetylated distarch phosphate, wherein the nucleating agent is a sorbitol nucleating agent and the dispersing agent is stearamide.

3. The process for improving the airtight qualification rate of hemodialysis dry powder barrels according to claim 1 is characterized in that: The heating temperature in S2 is 200°C.

4. The process for improving the airtight qualification rate of hemodialysis dry powder barrels according to claim 1 is characterized in that: The mold temperature in S3 was 80°C.

5. The process for improving the airtight qualification rate of hemodialysis dry powder barrels according to claim 1 is characterized in that: The barrel cover and filter screen of S3 are formed by one-piece mold.

6. The process for improving the airtight qualification rate of hemodialysis dry powder barrels according to claim 1 is characterized in that: The temperature of the cooling water in S4 is 18°C.

7. The process for improving the airtight qualification rate of hemodialysis dry powder barrels according to claim 1, characterized in that: The welding process in S6 includes the following steps: S601, debug ultrasonic welding machine; S602, process the welding fixture to match the product surface; S603, placing the injection molded barrel into the mold of the welding machine, and checking the dust condition at the edge of the barrel mouth; S604, place the barrel cover on the barrel body, push it into place manually, confirm that the barrel cover fits the barrel body, and then start the ultrasonic welding machine to complete the welding. S605. Check the sealing effect. There should be no overflow and no damage to the packaging material. Complete the welding of the barrel cover and the barrel body.

8. The process for improving the airtight qualification rate of hemodialysis dry powder barrels according to claim 6 is characterized in that: Debugging the ultrasonic welding machine in S601 includes: pulling down the welding head when the air pressure is zero, observing whether the welding head can fully contact the workpiece placed in the bottom mold or slightly lower than the plastic part, and ensuring that the parts can be easily taken in and out; using the horizontal plate and adjusting screws to adjust it horizontally, and using carbon paper and white paper to check; adjusting the welding parameters includes time, pressure, descending speed, trigger pressure, amplitude and holding time.

9. The process for improving the airtight qualification rate of hemodialysis dry powder barrels according to claim 6, characterized in that: The processing of the welding fixture in S602 includes: polishing the bottom fixture of the fixture; adjusting the ultrasonic fixture to surround the bottom of the product to be melted to avoid displacement of plastic parts caused by vibration waves during the melting process.

Citation Information

Patent Citations

  • Injection molding process for dialysis dry powder bucket

    CN109676886A

  • PP material injection molding process and bottle cap prepared by same

    CN111892766A

  • Online B-powder device for hemodialysis and hemofiltration

    CN202096520U

  • Method for manufacturing container

    JP2008238437A