Bamboo charcoal plate for reinforcing layer of composite floor of railway wagon and preparation method of bamboo charcoal plate
Through the close composite of bamboo charcoal board and wood pellet foamed polyurethane, the problems of high density and non-renewable material of the existing railway truck composite floor reinforcement layer are solved, and lightweight and environmentally friendly composite board preparation is achieved, reducing vehicle weight and manufacturing costs. It also improves the nailing ability and maintenance efficiency of the structure.
Patent Information
- Application Number
- CN202411225223.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-12-03
AI Technical Summary
The reinforcement layer materials of existing railway truck composite floors have problems such as high density, non-environmentality, non-renewable, difficult to recycle and degrade, high cost and difficult to nail in, which affects cargo loading and reinforcement and leads to damage to the structure.
Bamboo charcoal board is used as the reinforcement layer of railway truck composite flooring, bamboo charcoal board is prepared through the charcoalization and hot pressing process of bamboo materials, and is closely composited with the foamed polyurethane material reinforced by wood particles to form a lightweight and environmentally friendly composite board.
It reduces the overall quality and density of composite sheets, provides renewable materials to solve recycling problems, reduces manufacturing costs, bamboo charcoal boards are easy to nail in and are not easy to separate from the load-bearing layer, and improves vehicle weight and maintenance efficiency.
Smart Images

Figure CN119058181A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of bamboo and wood material processing, and in particular relates to a bamboo charcoal board used for a reinforcement layer of a composite floor of a railway freight car and a preparation method thereof. Background Art
[0002] In order to solve the problems of easy decay, flammability and short life of wooden floors in railway freight cars (also known as "railway flat cars"), relevant research institutes have successively developed glass fiber reinforced composite floors and wood particle reinforced composite floors. These two types of composite floors are mainly composed of a wear-resistant layer, a load-bearing layer (or foaming layer) and a reinforcing layer. Among them, the reinforcing layer is placed at the bottom of the composite floor. It is one of the important structures to ensure and improve the overall mechanical properties of the composite floor. It is mainly made of metal materials or composite materials. The Chinese invention patent "A composite sheet for railway flat cars and its preparation method and application" with patent number ZL202111226707.0 (authorization announcement date October 31, 2023) discloses a composite sheet with the above structure, in which the reinforcing layer (ie "reinforcement layer") is a metal material or continuous fiber (such as glass fiber) reinforced PU, PE, PP, PVC and other materials. Fiber-reinforced polymer sheets, such as the long glass fiber reinforced polyurethane pultruded sheets (commonly known as "glass reinforced plastics") used in practice, have problems such as high density, environmental protection, non-renewable, difficult to recycle and degrade, and high cost. In addition, when trucks are transporting goods, they often need to nail the composite floor to reinforce the goods. When the nails are long, they will penetrate the load-bearing layer and act on the reinforcement layer. The existing reinforcement layer is difficult to nail into due to its high hardness, which not only affects the loading and reinforcement of the goods, but also causes the reinforcement layer to separate from the load-bearing layer, and damages the composite floor structure. Figure 1 The figure shows a railway freight car composite floor that was damaged by nails being driven into it during actual operation.
[0003] Therefore, it is necessary to develop a new reinforcement layer for railway or vehicle composite floor to overcome the defects of existing reinforcement layers.
[0004] Bamboo is a fast-growing and biodegradable biomass material. "Replacing plastic with bamboo" provides an effective solution to reduce plastic pollution. China has more than 7 million hectares of bamboo forests and is the country with the richest bamboo resources in the world. Bamboo has been used in construction, home decoration and other fields to improve its strength after carbonization. So far, bamboo has not been used as a reinforcement layer for railway freight car composite floors. If successful, it will not only provide a new outlet for bamboo resources, but also solve the defects of existing reinforcement layers. Summary of the invention
[0005] In view of the deficiencies of the prior art, the present invention provides a bamboo charcoal board and application thereof as a reinforcement layer of a composite floor of a railway freight car.
[0006] To this end, the present invention adopts the following technical solution:
[0007] A method for preparing a bamboo charcoal board for a reinforcement layer of a railway freight car composite floor comprises the following steps:
[0008] I. Preparation of blank strips
[0009] The bamboo material is freed of bamboo green and bamboo yellow, and then carbonized and shaped to obtain a rough strip with a length of 1000 mm to 3000 mm, a width of 20 mm to 50 mm, and a thickness of 1 mm to 4 mm;
[0010] II. Hot Press Forming
[0011] The blank strip obtained in step I is coated with glue on both sides, and then placed in a preheated mold in the length direction for assembly and hot pressing to obtain a formed sheet;
[0012] III. Machining
[0013] The formed board obtained in step II is mechanically processed to obtain a bamboo charcoal board of specified shape and size.
[0014] Preferably, the bamboo material is selected from whole bamboo, bamboo segments, bamboo slices or bamboo strips.
[0015] Preferably, in step I, the carbonization includes high-temperature carbonization and low-temperature drying; the process conditions of the high-temperature carbonization are heating at 100°C to 300°C for 1h to 5h under air-tight conditions; the process conditions of the low-temperature drying are drying at ≤40°C to a moisture content of ≤10%.
[0016] More preferably, the high temperature carbonization temperature is 240-260°C.
[0017] Preferably, in step I, the shaping includes one or more operations selected from grinding, slicing, slicing, peeling, leveling, breaking and cutting.
[0018] The striping and slicing refers to splitting the whole bamboo or bamboo segment longitudinally and dividing it into bamboo slices of a specified width. The flattening refers to removing the protruding parts on the surface of the bamboo node. The breaking refers to removing the isolation parts between the internal bamboo nodes. After peeling, flattening and breaking, the green bamboo on the surface of the bamboo and the yellow bamboo inside are removed to obtain bamboo slices of a specified thickness and smooth on both sides. The cutting refers to cutting a long bamboo slice into a specified length.
[0019] There is no restriction on the order of the carbonization and shaping. The bamboo material may be shaped first to obtain bamboo strips of a specified size and then carbonized; or the bamboo material may be carbonized first and then shaped to the specified size.
[0020] Therefore, the step I can be carried out according to the following specific steps:
[0021] I-1. The bamboo segments or whole bamboo are polished, flattened, broken, cut into strips, sliced, and cut to obtain bamboo pieces with both sides smooth and green bamboo and yellow bamboo removed;
[0022] I-2. The bamboo chips obtained in step I-1 are placed in a carbonization furnace, and carbonized at 100 ℃ to 300 ℃, preferably 240 ℃ to 260 ℃, for 1 h to 5 h under air-tight conditions, and then dried at ≤40 ℃ to a moisture content of ≤10%;
[0023] I-3. The carbonized bamboo pieces obtained in step I-2 are flattened and polished, and cut if necessary to obtain roughened strips having a surface roughness of 5.5 μm to 6.5 μm, a length of 1000 mm to 3000 mm, a width of 20 mm to 50 mm, and a thickness of 1 mm to 4 mm.
[0024] Optionally, step I may also be performed according to the following specific steps:
[0025] IA. Place bamboo segments, whole bamboo or bamboo chips into a carbonization furnace, carbonize at 100°C to 300°C, preferably 240°C to 260°C for 1h to 5h under air-tight conditions, and then dry at ≤40°C to a moisture content of ≤10%;
[0026] IB. The carbonized bamboo obtained in step IA is polished, flattened, broken, cut, sliced, cut to obtain carbonized bamboo strips;
[0027] IC. The carbonized bamboo strips treated in step IB are flattened and polished, and cut if necessary to obtain a roughened strip with a surface roughness of 5.5 μm to 6.5 μm, a length of 1000 mm to 3000 mm, a width of 20 mm to 50 mm, and a thickness of 1 mm to 4 mm.
[0028] As an optional solution, the bamboo material used for carbonization can also be commercially available bamboo strips; even the rough strips can be directly made from commercially available products, and after necessary grinding, flattening and cutting, the rough strips with surface roughness, length, width and thickness that meet the requirements can be obtained.
[0029] Optionally, in step II, before gluing, the blank strip is flattened again if necessary.
[0030] The blank strips will deform during long-term storage and placement. Therefore, according to the actual situation, the deformed blank strips can be flattened again before gluing.
[0031] Preferably, in step II, the glue used for gluing the blank strip is selected from one of environmentally friendly water-resistant urea-formaldehyde resin glue, phenolic resin glue, epoxy resin glue and polyurethane glue, and the solid content is ≥40%.
[0032] Also preferably, in step II, the amount of glue applied to the blank strip is 150 g / m 2 ~300g / m 2 .
[0033] Preferably, in step II, the density of the formed board is 0.8 g / cm 3 ~1.5g / cm 3 Assemble the glue-coated blank strips.
[0034] Preferably, in step II, the mold is preheated to 100°C to 200°C.
[0035] Preferably, in step II, the assembled blank strips are pressed into a specified shape at a hot pressing rate of 1 mm / min to 10 mm / min at a temperature of 100° C. to 200° C. and a pressure of 1 MPa to 8 MPa, and then the heat and pressure are maintained for 4 min to 12 min.
[0036] Also preferably, in step II, after the hot pressing is completed, the sheet is demoulded and cooled naturally.
[0037] As a preferred embodiment, step II of the present invention can be completed according to the following specific operations:
[0038] II-1. The blank strip obtained in step I is flattened again if necessary, and then coated with glue on both sides, with a coating amount of 150g / m 2 ~300g / m 2 The solid content of the glue is ≥40%, and the glue is selected from one of environmentally friendly water-resistant urea-formaldehyde resin glue, phenolic resin glue, epoxy resin glue and polyurethane glue;
[0039] II-2. Preheat the mold to 100℃~200℃, and set the density of the molded board to 0.8g / cm 3 ~1.5g / cm 3 , placing the glue-coated blank strip obtained in step II-1 in the mold along the length direction for assembly;
[0040] II-3. The mold is sent into the press, and the assembled blank strip is pressed into a plate of a specified shape at a hot pressing rate of 1mm / min~10mm / min at a pressure of 1MPa~8MPa and a temperature of 100℃~200℃, and the pressure and temperature are maintained for 4min~12min;
[0041] II-4. Demolding and natural cooling to obtain the bamboo charcoal board.
[0042] Preferably, the machining process in step III includes trimming, cutting, planing, sawing and grinding.
[0043] Preferably, in the step III, the polishing refers to polishing all surfaces except the bottom surface of the bamboo charcoal board to a roughness of 5 μm to 10 μm.
[0044] The second object of the present invention is to provide a bamboo charcoal board for a reinforcement layer of a composite floor of a railway freight car, which is prepared by the above-mentioned preparation method.
[0045] Optionally, the cross section of the bamboo charcoal board is rectangular.
[0046] Optionally, the cross section of the bamboo charcoal board is convex.
[0047] Optionally, the cross section of the bamboo charcoal board is concave-shaped.
[0048] Optionally, the cross section of the bamboo charcoal board is in a mountain shape.
[0049] The present invention has a third object, which is to provide the use of the bamboo charcoal board of the present invention as a reinforcing layer in the preparation of a composite board.
[0050] Therefore, the present invention also provides a composite board material, comprising a reinforcing layer and a bearing layer which are tightly combined together, wherein the reinforcing layer is the bamboo charcoal board described in the present invention, and the bearing layer is made of foamed polyurethane reinforced with wood particles.
[0051] The bearing layer made of foamed polyurethane reinforced with wood particles has been described in detail in the Chinese invention patent application with publication number CN113910732A (publication date January 11, 2022), and is hereby introduced into this application.
[0052] The reinforcing layer of the composite board of the present invention can be a bamboo charcoal board with a rectangular cross section as described in the present invention.
[0053] Optionally, the reinforcement layer may be two or more bamboo charcoal boards having a convex, concave or mountain-shaped cross section as described in the present invention.
[0054] Preferably, the reinforcing layer may be two or more bamboo charcoal boards with convex, concave or mountain-shaped cross sections as described in the present invention, and the bamboo charcoal boards are arranged to be evenly spaced from each other.
[0055] For example, when the reinforcing layer can be 2, 3, 4 or 5 bamboo charcoal boards with convex, concave or mountain-shaped cross sections as described in the present invention, the bamboo charcoal boards are arranged to be evenly spaced from each other.
[0056] When the reinforcing layer is the bamboo charcoal board with a convex, concave or mountain-shaped cross section as described in the present invention, the protrusions on the bamboo charcoal board play the role of reinforcing ribs.
[0057] The present invention also provides a method for preparing the composite plate, comprising the following steps:
[0058] 1) Enhancement layer preparation
[0059] The bamboo charcoal board of the present invention is cut into required sizes, and the surface of the bamboo charcoal board contacting the bearing layer is polished or sandblasted, preferably polished;
[0060] 2) Forming of composite panels
[0061] First, spray an appropriate amount of release agent evenly in the mold cavity; then place the reinforcement layer obtained in step 1) at the bottom of the mold cavity, with the polished or sandblasted surface facing upward, and apply polyurethane adhesive on the surface; then introduce the foamed material obtained by mixing wood particles and foamed polyurethane into the mold cavity; finally, after the mold is closed, heat it to 40℃-80℃ and keep it warm for 40-120min, demold it after the foamed material is cured and formed, and mature it at 40-60℃ for 6-24h to obtain the product.
[0062] Preferably, the polyurethane adhesive can be selected from commercially available products, such as the polyurethane adhesive produced by Nanjing Jufa New Materials Company, brand Urebond 2055, or the adhesive produced by Foshan Zhebao Technology Co., Ltd., brand ZB010.
[0063] Preferably, the polyurethane adhesive is applied with a thickness of 0.3 to 1.5 mm.
[0064] The above-mentioned wood particles can be modified, and the specific treatment method has been described in detail in the Chinese invention patent application with publication number CN113910732A (publication date January 11, 2022), which is introduced into this application.
[0065] The raw materials of the foamed polyurethane have also been described in detail in the Chinese invention patent application with publication number CN113910732A (publication date January 11, 2022), which is introduced into this application.
[0066] The present invention also provides application of the composite board as a railway freight car floor.
[0067] The beneficial technical effects of the present invention include:
[0068] (1) Compared with the existing composite board materials that use long fiber reinforced polymer as the reinforcement layer material (such as "glass reinforced plastic"), the present invention uses a lightweight bamboo charcoal board as the reinforcement layer, which reduces the overall mass / density of the composite board and ensures that the composite board is suitable for various types of vehicles so that the vehicle's own weight does not exceed the standard.
[0069] (2) Bamboo charcoal board is a renewable raw material, which can solve the problem of difficult recycling of composite boards in the later stage. In addition, my country has abundant bamboo resources and does not need to rely on imports, which provides a new outlet for bamboo resources.
[0070] (3) Compared with the existing preparation method of long fiber reinforced polymer sheet, the preparation process of the bamboo charcoal sheet of the present invention mainly involves hot pressing and mechanical processing, which is more environmentally friendly. The side of the bamboo charcoal board in contact with the bearing layer does not need sandblasting, and simple grinding can provide the required roughness.
[0071] (4) Bamboo is cheap and the processing technology of bamboo charcoal board is simple, which reduces the manufacturing cost of composite board.
[0072] (5) As a reinforcing layer, the bamboo charcoal board is easy to be nailed with long nails and is not easy to separate from the bearing layer, so the structure of the composite board will not be destroyed.
[0073] (6) The composite board of the present invention is easy to punch holes, so it can be conveniently and quickly fixed to a railway freight car by bolting; it is also easy to replace and remove, thereby improving the efficiency of vehicle maintenance. BRIEF DESCRIPTION OF THE DRAWINGS
[0074] The present invention is further described below in conjunction with the accompanying drawings.
[0075] Figure 1 The photo shows a railway freight car composite floor whose reinforcement layer is "glass reinforced plastic" and is damaged by nail penetration during actual use. The enlarged part of the picture shows that the reinforcement layer around the nail is separated from the bearing layer (the nail head has been ground flat), and the reinforcement layer is delaminated at the place indicated by the arrow, and the composite floor is broken.
[0076] Figure 2 The schematic diagram of the size structure of the rectangular cross section of the bamboo charcoal board of Examples 2 and 5 is shown.
[0077] Figure 3 The schematic diagram of the size structure of the convex cross section of the bamboo charcoal board of Examples 3 and 6 is shown.
[0078] Figure 4 The schematic diagram of the size structure of the concave cross section of the bamboo charcoal board of Examples 4 and 7 is shown.
[0079] Figure 5 The schematic diagram of the size structure of the mountain-shaped cross section of the bamboo charcoal board of Examples 5 and 8 is shown.
[0080] Figure 2-Figure 5 The unit is mm (millimeter).
[0081] Figure 6 Schematic cross-sectional views of the composite panels of Examples 9 and 13 are shown.
[0082] Figure 7 Schematic cross-sectional views of the composite panels of Examples 10 and 14 are shown.
[0083] Figure 8Schematic cross-sectional views of the composite panels of Examples 11 and 15 are shown.
[0084] Fig. 9 Schematic cross-sectional views of the composite panels of Examples 12 and 16 are shown.
[0085] Figure 6 to Figure 9 The meanings of the reference symbols are as follows:
[0086] 1: bearing layer, 2: bamboo charcoal board.
[0087] Fig.10 The photograph shows the composite board prepared in Example 9.
[0088] Fig.11 The photos show Fig.10 The process of nailing the composite sheet shown in FIG. 1 ; wherein:
[0089] A: shows the composite board and three nails ready to be driven in; B: the nails are driven in from the bearing layer of the composite board; C: the nails pass through the reinforcing layer of the composite board. DETAILED DESCRIPTION
[0090] The present invention is described below with reference to specific examples. It will be appreciated by those skilled in the art that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention in any way.
[0091] The experimental methods in the following examples are conventional methods unless otherwise specified. The raw materials, reagents and materials used in the following examples are commercially available products unless otherwise specified. The purchase of some reagents and materials is as follows:
[0092] Phenolic resin glue: Beijing Taier Chemical Co., Ltd., 965 phenolic resin glue;
[0093] Polyurethane adhesive: Nanjing Jufa New Materials Co., Ltd., Urebond2055.
[0094] Embodiment 1~4: A bamboo charcoal board
[0095] Ⅰ. Preparation of blank strips: Cut bamboo strips (commercially available) with a width of 20mm to 30mm and a thickness of 1mm to 2mm and without yellow and green bamboo strips into a uniform length of 3000mm, put them into a 250℃ high-temperature carbonization furnace for carbonization for 2.5h, take them out and flatten them, cool them naturally, and place them at room temperature for 2 to 3 days until the moisture content is ≤10%, and finally use a 150-200 mesh grinding wheel / sandpaper to grind the surface to a roughness (Ra) of (6±0.5)μm to obtain blank strips.
[0096] Ⅱ. Hot pressing: Coat both sides of the blank strip prepared in Ⅰ with phenolic resin glue, with a coating amount of 250g / m2 Then, the density of the formed board is 0.9g / cm 3 (Example 1), 1.0 g / cm 3 (Example 2), 1.2 g / cm 3 (Example 3) and 1.4 g / cm 3 (Example 4) Place the blank into a mold preheated to 160°C for embryo assembly, so that the length direction of the blank strip is consistent with the mold, and then send it into a press to press it into a flat plate or a special-shaped plate at 5mm / min. The hot pressing temperature is 160°C, the heat preservation and pressure holding time is 5min~7min, and the holding pressure is 3MPa (Example 1), 4MPa (Example 2), 5.5MPa (Example 3) and 7.5MPa (Example 4) respectively, to obtain a hot-pressed plate; the final density of the plate prepared in Example 1 is 0.86g / cm 3 The final density of the board prepared in Example 2 is 0.98 g / cm 3 The final density of the board prepared in Example 3 is 1.19 g / cm 3 The final density of the board prepared in Example 4 is 1.38 g / cm 3 ;
[0097] III. Machining
[0098] The hot-pressed plate obtained in step II is machined, and the roughness of the remaining surfaces except the bottom surface is 8 μm to 10 μm, thereby finally obtaining the bamboo charcoal boards of Examples 1 to 4.
[0099] The cross-sectional dimensions and structures of the bamboo charcoal boards of Examples 1 to 4 are as follows: Figure 2-Figure 5 As shown. Among them:
[0100] Example 1 The cross section of the bamboo charcoal board is rectangular, and the cross section size structure diagram is shown in Figure 2 .
[0101] The cross section of the bamboo charcoal board of Example 2 is a convex shape, and the cross section size structure diagram is shown in Figure 3 .
[0102] The cross section of the bamboo charcoal board of Example 3 is a concave shape, and the schematic diagram of the cross section size structure is shown in Figure 4 .
[0103] Example 4 The cross section of the bamboo charcoal board is in the shape of a mountain. The cross section size structure diagram is shown in Figure 5 .
[0104] Embodiment 5~8: A bamboo charcoal board
[0105] Ⅰ. Preparation of blank strips: Cut bamboo strips (commercially available) with a width of 20mm to 30mm and a thickness of 1mm to 2mm and without yellow / green bamboo into a uniform length of 3000mm, put them into a 210℃ high-temperature carbonization furnace for carbonization for 3.5h, take them out and flatten them, cool them, and place them at room temperature for 2 to 3 days until their moisture content is ≤10%. Finally, use a 150-mesh to 200-mesh grinding wheel / sandpaper to grind the surface to a roughness (Ra) of (6±0.5)μm to obtain blank strips.
[0106] Ⅱ. Hot pressing: Apply polyurethane glue on both sides of the blank strip prepared in Ⅰ, with a coating amount of 200g / m 2 Then, the density of the formed board is 0.9g / cm 3 (Example 5), 1.0 g / cm 3 (Example 6), 1.2 g / cm 3 (Example 7) and 1.4 g / cm 3 (Example 8) Place the blank into a mold preheated to 130°C for embryo assembly, so that the length direction of the blank is consistent with the mold, and send it into a press to press it into a flat plate or a special-shaped plate at 5mm / min. The hot pressing temperature is 130°C, the heat preservation and pressure holding time is 10min~12min, and the holding pressure is 3MPa (Example 5), 4MPa (Example 6), 5.5MPa (Example 7) and 7.5MPa (Example 8) respectively, to obtain a hot-pressed plate; the final density of the plate prepared in Example 5 is 0.85g / cm 3 The final density of the board prepared in Example 6 is 0.96 g / cm 3 The final density of the board prepared in Example 7 is 1.14 g / cm 3 The final density of the board prepared in Example 8 is 1.37 g / cm 3 ;
[0107] III. Machining
[0108] The hot-pressed plate obtained in step II is machined, and the roughness of the remaining surfaces except the bottom surface is 8 μm to 10 μm, and finally the bamboo charcoal boards of Examples 5 to 8 are obtained.
[0109] The cross-sectional dimensions and structures of the bamboo charcoal boards of Examples 5 to 8 are as follows: Figure 2-Figure 5 As shown. Among them:
[0110] The cross section of the bamboo charcoal board of Example 5 is rectangular, and the cross section size structure diagram is shown in Figure 2 .
[0111] The cross section of the bamboo charcoal board of Example 6 is a convex shape, and the cross section size structure diagram is shown in Figure 3 .
[0112] The cross section of the bamboo charcoal board of Example 7 is a concave shape, and the cross section size structure diagram is shown in Figure 4 .
[0113] The cross section of the bamboo charcoal board of Example 8 is in the shape of a mountain. The schematic diagram of the cross section size is shown in Figure 5 .
[0114] Embodiments 9 to 16 A composite board for railway freight car floor
[0115] The composite board material of Examples 9 to 16 includes a bearing layer and a reinforcing layer arranged on one side of the bearing layer, and the bearing layer and the reinforcing layer are tightly compounded together; the width is 308 mm, the length is 2968±3 mm or 2948±3 mm, and the thickness is 70 mm.
[0116] The bearing layer is made of polyurethane foam material reinforced with wood particles. Based on the total weight of the bearing layer, the wood particles account for 70%. The length of the wood particles is 5-20 mm and the width is 2-5 mm. The wood particles are modified. The raw material composition of the bearing layer is:
[0117]
[0118] The reinforcing layers are made of the bamboo charcoal boards of Examples 1 to 8 respectively.
[0119] The composite plates of Examples 9 to 16 were prepared by the following method:
[0120] (1) Modification of wood particles
[0121] 38% water, 20% water-soluble phenolic resin, 20% polyethylene glycol (number average molecular weight 500), 10% acetic anhydride and 12% preservative ACQ are mixed in a mass ratio to prepare a modification liquid. At normal temperature and pressure, wood particles are completely immersed in the modification liquid for 12 hours. After being taken out and filtered, the modified wood particles are dried at 100°C for 12 hours to obtain modified wood particles.
[0122] (2) Preparation of foaming material
[0123] According to the above weight parts, the polyurethane foaming raw material and the modified wood particles obtained in step I are uniformly mixed to obtain.
[0124] (3) Enhancement layer preparation
[0125] The bamboo charcoal boards of Examples 1 to 8 are cut into required sizes, and the surfaces of the bamboo charcoal boards contacting the bearing layer are polished.
[0126] (4) Forming of composite panels
[0127] ① Spray an appropriate amount of release agent evenly in the mold cavity; ② Place the reinforcement layer obtained in step (3) at the bottom of the mold cavity as shown in Table 1, with the unpolished and rough side facing downward; when the number of bamboo charcoal boards is greater than 1, the bamboo charcoal boards are evenly spaced; the polished side of the bamboo charcoal board is evenly coated with a polyurethane adhesive of grade Urebond 2055 (Nanjing Jufa New Materials Co., Ltd.) or a polyurethane adhesive of grade ZB010 (Foshan Zhebao Technology Co., Ltd.) with a thickness of about 1.0 mm; ③ Introduce the foamed material obtained in step (2) into the mold cavity; (3) Close the mold, heat to 65°C, pressurize to a pressure of 0.8MPa to 1.2MPa, keep the temperature and pressure for 60 minutes, demould after the foamed material is solidified, and mature for 16 hours at 45°C to obtain the composite board for railway freight car floor.
[0128] Table 1 Configuration of the reinforcement layer of the composite board of Examples 9 to 16
[0129]
[0130]
[0131] Comparative Example 1 Wood particle reinforced board for railway freight car floor
[0132] The board of this comparative example is a wood particle reinforced board, without a reinforcement layer, 308 mm wide, 2968±3 mm or 2948±3 mm long, and 70 mm thick. The composition of the wood particle reinforced board is the same as the load-bearing layer of Example 9, and is prepared by the following method:
[0133] (1) Modification of wood particles
[0134] Same as step (1) of Example 9.
[0135] (2) Preparation of foaming material
[0136] Same as step (2) of Example 9.
[0137] (3) Sheet forming
[0138] ① spraying an appropriate amount of release agent evenly in the mold cavity; ② introducing the foamed material obtained in step (2) into the mold cavity; (3) closing the mold, heating to 65° C., pressurizing to 0.8-1.2 MPa, maintaining the temperature and pressure for 60 minutes, demolding after the foamed material is solidified, and aging at 45° C. for 16 hours to obtain the sheet material for railway freight car floor.
[0139] Test Example 1 Performance measurement of the composite boards of Examples 9 to 16 and the board of Comparative Example 1
[0140] The density and overall bending load of the composite panels prepared in Examples 9 to 1 and the panels prepared in Comparative Example 1 were measured using the test methods specified in the Interim Technical Specifications for Composite Floors of Railway Flat Cars (TJ / CL 577-2022). The results are shown in Table 2.
[0141] Table 2 Performance test results of the plates of various embodiments and comparative examples
[0142]
[0143]
[0144] Test Example 2
[0145] Fig.10 The photograph shows the composite sheet prepared in Example 9, which was subjected to a nail penetration test. Fig.11 The photos show the nailing process. The nails are driven into the load-bearing layer of the composite board made of wood particle reinforced polyurethane material (A and B) and out of the reinforcing layer (bamboo charcoal board) (C). Fig.11 It can be clearly seen that the bamboo charcoal board did not split or separate after the iron nail penetrated.
Claims
1. A method for preparing a bamboo charcoal board for a reinforcement layer of a railway freight car composite floor, comprising the following steps: I. Preparation of blank strips The bamboo material is freed of bamboo green and bamboo yellow, and then carbonized and shaped to obtain a rough strip with a length of 1000 mm to 3000 mm, a width of 20 mm to 50 mm, and a thickness of 1 mm to 4 mm; II. Hot Press Forming The blank strip obtained in step I is coated with glue on both sides, and then placed in a preheated mold in the length direction for assembly and hot pressing to obtain a formed sheet; III. Machining The formed board obtained in step II is mechanically processed to obtain a bamboo charcoal board of a specified shape and size; Preferably, the bamboo material is selected from whole bamboo, bamboo segments, bamboo slices or bamboo strips.
2. The preparation method according to claim 1, characterized in that: In the step I, the carbonization includes high-temperature carbonization and low-temperature drying; the process conditions of the high-temperature carbonization are heating at 100°C to 300°C for 1h to 5h under air-tight conditions; the process conditions of the low-temperature drying are drying at ≤40°C to a moisture content of ≤10%; Preferably, the high temperature carbonization temperature is 240-260°C; Also preferably, in the step I, the shaping comprises one or more operations selected from the group consisting of grinding, slicing, slicing, peeling, flattening, breaking and cutting; Preferably, step I is performed according to the following specific steps: I-1. The bamboo segments or whole bamboo are polished, flattened, broken, cut into strips, sliced, and cut to obtain bamboo pieces with both sides smooth and green bamboo and yellow bamboo removed; I-2. The bamboo chips obtained in step I-1 are placed in a carbonization furnace, and carbonized at 100 ℃ to 300 ℃, preferably 240 ℃ to 260 ℃, for 1 h to 5 h under air-tight conditions, and then dried at ≤40 ℃ to a moisture content of ≤10%; I-3. The carbonized bamboo pieces obtained in step I-2 are flattened and polished, and cut if necessary to obtain a roughened strip having a surface roughness of 5.5 μm to 6.5 μm, a length of 1000 mm to 3000 mm, a width of 20 mm to 50 mm, and a thickness of 1 mm to 4 mm; Or, the step I is carried out according to the following specific steps: IA. Place bamboo segments, whole bamboo or bamboo chips into a carbonization furnace, carbonize at 100°C to 300°C, preferably 240°C to 260°C for 1h to 5h under air-tight conditions, and then dry at ≤40°C to a moisture content of ≤10%; IB. The carbonized bamboo obtained in step IA is polished, flattened, broken, cut, sliced, cut to obtain carbonized bamboo strips; IC. The carbonized bamboo strips treated in step IB are flattened and polished, and cut if necessary to obtain a roughened strip with a surface roughness of 5.5 μm to 6.5 μm, a length of 1000 mm to 3000 mm, a width of 20 mm to 50 mm, and a thickness of 1 mm to 4 mm.
3. The preparation method according to claim 1, characterized in that: In the step II, before gluing, the blank strip is flattened again if necessary; Preferably, in step II, the glue used for coating the blank strip is selected from one of environmentally friendly water-resistant urea-formaldehyde resin glue, phenolic resin glue, epoxy resin glue and polyurethane glue, and the solid content is ≥40%; Also preferably, in step II, the amount of glue applied to the blank strip is 150 g / m 2 ~300g / m 2 ; Preferably, in step II, the density of the formed board is 0.8 g / cm 3 ~1.5g / cm 3 Assembling the glue-coated blank strips; Preferably, in step II, the mold is preheated to 100° C. to 200° C.; Preferably, in step II, the assembled blank strips are pressed into a specified shape at a hot pressing rate of 1 mm / min to 10 mm / min under the conditions of 100° C. to 200° C. and a pressure of 1 MPa to 8 MPa, and then the heat and pressure are maintained for 4 min to 12 min; Also preferably, in step II, after the hot pressing is completed, the sheet is demoulded and cooled naturally.
4. The preparation method according to claim 1 or 3, characterized in that: The step II is completed according to the following specific operations: II-1. The blank strip obtained in step I is flattened again if necessary, and then coated with glue on both sides, with a coating amount of 150g / m 2 ~300g / m 2 The solid content of the glue is ≥40%, and the glue is selected from one of environmentally friendly water-resistant urea-formaldehyde resin glue, phenolic resin glue, epoxy resin glue and polyurethane glue; II-2. Preheat the mold to 100℃~200℃, and set the density of the molded board to 0.8g / cm 3 ~1.5g / cm 3 , placing the glue-coated blank strip obtained in step II-1 in the mold along the length direction for assembly; II-3. The mold is sent into the press, and the assembled blank strip is pressed into a plate of a specified shape at a hot pressing rate of 1mm / min~10mm / min at a pressure of 1MPa~8MPa and a temperature of 100℃~200℃, and the pressure and temperature are maintained for 4min~12min; II-4. Demolding and natural cooling to obtain the bamboo charcoal board.
5. The preparation method according to claim 1, characterized in that: The machining process in step III includes trimming, cutting, planing and grinding; Preferably, in the step III, the polishing refers to polishing all surfaces except the bottom surface of the bamboo charcoal board to a roughness of 5 μm to 10 μm.
6. A bamboo charcoal board for a reinforcement layer of a railway freight car composite floor prepared by the preparation method according to any one of claims 1 to 5; Optionally, the cross section of the bamboo charcoal board is rectangular; Optionally, the cross section of the bamboo charcoal board is a convex shape; Optionally, the cross section of the bamboo charcoal board is a concave shape; Optionally, the cross section of the bamboo charcoal board is in a mountain shape.
7. Use of the bamboo charcoal board according to claim 6 as a reinforcing layer in the preparation of a composite board.
8. A composite board, comprising a reinforcing layer and a bearing layer which are tightly combined together, wherein the reinforcing layer is the bamboo charcoal board according to claim 6, and the bearing layer is made of foamed polyurethane reinforced with wood particles; Optionally, the reinforcement layer may be a bamboo charcoal board having a rectangular cross section; Optionally, the reinforcement layer may be two or more bamboo charcoal boards with convex, concave or mountain-shaped cross sections; Preferably, when the reinforcement layer is two or more bamboo charcoal boards with convex, concave or mountain-shaped cross sections, the bamboo charcoal boards are arranged to be evenly spaced from each other.
9. The method for preparing the composite sheet material according to claim 8, comprising the following steps: 1) Enhancement layer preparation The bamboo charcoal board of claim 6 is cut into required sizes, and the surface of the bamboo charcoal board contacting the bearing layer is polished or sandblasted, preferably polished; 2) Forming of composite panels First, spray an appropriate amount of mold release agent evenly in the mold cavity; then place the reinforcement layer obtained in step 1) at the bottom of the mold cavity, with the polished or sandblasted surface facing upward, and apply polyurethane adhesive on the surface; then introduce the foamed material obtained by mixing wood particles and foamed polyurethane into the mold cavity; finally, heat the mold to 40°C-80°C after closing the mold, keep the temperature for 40-120 minutes, demould after the foamed material is solidified, and mature it at 40-60°C for 6-24 hours to obtain the product; Preferably, the polyurethane adhesive is applied with a thickness of 0.3 to 1.5 mm.
10. Use of the composite board material according to claim 8 or the composite board material prepared by the preparation method according to claim 9 as a railway freight car floor.
Citation Information
Patent Citations
Composite board for railway flatcar as well as preparation method and application of composite board
CN113910732A
Molded composite board of regenerated polymer as basic material and bamboo strip as reinforcing material
CN1486841A
Truck floor manufacturing process and product thereof
WO2024016427A1