Laminate, blister container, and blister package
By using a combination of multi-layer structure and specific materials in the laminated body to adjust the water vapor transmittance and upper yield point stress, the problem of insufficient moldability of fluorine resin laminated body is solved, and high barrier properties and good moldability are achieved. It is suitable for In drug packaging.
Patent Information
- Application Number
- CN202411430993.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2017-03-17
- Filing Date
- 2018-03-12
- Publication Date
- 2024-12-03
AI Technical Summary
In the prior art, the fluorine resin laminate with high barrier properties has a shortage in moldability, and it is difficult to have good moldability while maintaining high barrier properties.
A three-layer or five-layer structure laminated body, including a base layer, an intermediate layer and a fluorine resin layer, is used to adjust the material and thickness of each layer to ensure that the water vapor transmittance is less than 0.5g/m2/24 hours, and Improve the upper yield point stress to above 1,500N/cm2 to enhance moldability.
It realizes the moldability and adaptability of the laminated body while maintaining high barrier properties and low water vapor transmission. It is suitable for blister containers and blister packaging for packaging materials such as medicines.
Smart Images

Figure CN119058208A_ABST
Abstract
Description
[0001] The present invention is a divisional application of Chinese patent application with application number 201880018656.2, application date March 12, 2018, and invention name “Laminate, blister container and blister package”. This application claims the priority of Japanese Patent Application No. 2017-053665 filed in Japan on March 17, 2017. Technical Field
[0002] [Cross-reference of related applications]
[0003] This application claims the benefit of priority based on Japanese Patent Application No. 2017-053665, filed on March 17, 2017, the entirety of which is incorporated herein by reference.
[0004] [Technical field of the invention]
[0005] The present invention relates to a laminate, a blister container and a blister package. Background Art
[0006] Film laminates with high barrier properties are used as packaging materials for foods, pharmaceuticals, etc. In the pharmaceutical field, blister packages (Press Through Package; hereinafter sometimes referred to as "PTP") are used for individual packaging of tablets or capsules.
[0007] In order to suppress the degradation of the contents, the resin film as the forming material of the PTP is required to have a barrier property against water vapor. In addition, since the PTP is usually manufactured by deep drawing, the resin film as the forming material of the PTP is required to have good formability. For example, Patent Documents 1 and 2 describe a laminated body in which a fluorine-based resin film is laminated in order to improve the barrier property against water vapor.
[0008] Prior art literature
[0009] Patent Literature
[0010] Patent Document 1: Japanese Patent Application Publication No. 2014-028508
[0011] Patent Document 2: Japanese Patent Application Publication No. 2012-135980 Summary of the invention
[0012] 1. Technical issues to be resolved
[0013] When a laminate having high barrier properties to water vapor is produced using a fluorine-based resin having high barrier properties, it is required to provide a laminate having excellent moldability in addition to high barrier properties.
[0014] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a laminate having excellent moldability, and a blister container and a blister package using the laminate.
[0015] (II) Technical solution
[0016] That is, the present invention adopts the following configuration.
[0017] [1] A laminate comprising a substrate layer, an intermediate layer and a fluorine-based resin layer in this order, and having a total film thickness of 400 μm or less, wherein the thickness of the fluorine-based resin layer is 20 μm or more and 150 μm or less, and the water vapor permeability of the laminate is 0.5 g / m 2 / Less than 24 hours.
[0018] [2] The laminate according to [1], further comprising a second intermediate layer and a second base layer in this order on the surface of the fluorine-based resin layer opposite to the surface on which the intermediate layer is formed.
[0019] [3] The laminate according to [1] or [2], wherein the fluorine-based resin layer contains polychlorotrifluoroethylene.
[0020] [4] The laminate according to any one of [1] to [3], wherein the upper yield point stress of the laminate is 1,500 N / cm 2 above.
[0021] [5] The laminate according to any one of [1] to [4], wherein the intermediate layer comprises a polyethylene resin and a modified polyethylene resin.
[0022] [6] The laminate according to any one of [1] to [4], wherein the intermediate layer comprises an acid-modified polyolefin resin, an epoxy group-containing resin, and an elastomer resin.
[0023] [7] The laminate according to any one of [2] to [6], wherein the second intermediate layer comprises a polyethylene resin and a modified polyethylene resin.
[0024] [8] The laminate according to any one of [2] to [6], wherein the second intermediate layer comprises an acid-modified polyolefin resin, an epoxy group-containing resin, and an elastomer resin.
[0025] [9] A blister container comprising the laminate according to any one of [1] to [8].
[0026]
[10] A blister package comprising the laminate according to any one of [1] to [8].
[0027] (III) Beneficial effects
[0028] According to the present invention, it is possible to provide a laminate having excellent moldability, and a blister container and a blister package using the laminate. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 It is a schematic cross-sectional view of a laminated body according to the first embodiment of the present invention.
[0030] Figure 2 It is a schematic cross-sectional view of a laminated body according to a second embodiment of the present invention.
[0031] Description of Reference Numerals
[0032] 1, 2: laminated body, 11: fluorine-based resin layer, 10: intermediate layer, 12: base layer, 13: second intermediate layer, 14: second base layer. DETAILED DESCRIPTION
[0033] Hereinafter, the present invention will be described based on preferred embodiments.
[0034] <Laminated body>
[0035] 《First Implementation Mode》
[0036] Reference Figure 1 , a first embodiment of the laminated body of the present invention is described.
[0037] Figure 1 The laminated body 1 of the present embodiment shown is laminated in this order with a base layer 12, an intermediate layer 10, and a fluorine-based resin layer 11. The intermediate layer 10 functions as an adhesive layer for bonding the fluorine-based resin layer 11 and the base layer 12, and the base layer 12 and the fluorine-based resin layer 11 are laminated via the intermediate layer 10. The thickness of the fluorine-based resin layer 11 is 20 μm or more and 50 μm or less.
[0038] The laminate 1 of this embodiment has a three-layer structure of a base layer 12, an intermediate layer 10, and a fluorine-based resin layer 11. A three-layer laminate can be produced without complicated steps and the uniformity of each layer of the laminate is further improved, which is preferred.
[0039] The water vapor permeability of the laminated body of this embodiment is 0.5 g / m 2 / 24 hours or less, preferably 0.4g / m 2 / 24 hours or less, more preferably 0.3g / m 2 / Less than 24 hours.
[0040] Since the water vapor permeability of the laminate of the present embodiment is within the above-mentioned specific range, it is possible to exert high barrier properties and prevent the deterioration of the contents when manufacturing blister packages for medicines, for example. In the present embodiment, the water vapor permeability can be controlled by adjusting the materials and thickness of each layer of the substrate layer, the fluorine-based resin layer, and the intermediate layer. In the present embodiment, it is particularly preferred to control the water vapor permeability within the above-mentioned specific numerical range by adjusting the materials and thickness of the fluorine-based resin layer, and it is more preferred to control it by adjusting the thickness of the fluorine-based resin layer.
[0041] The upper yield stress of the laminate of the present embodiment measured under the following measurement conditions is preferably 1,500 N / cm 2 More preferably, 2,000 N / cm 2 More than, particularly preferably 2,100 N / cm 2 above.
[0042] By setting the upper yield stress of the laminate to be above the lower limit, the formability during deep drawing is improved. That is, during deep drawing, the drawn portion of the laminate becomes convex, and an extended portion appears compared to the original laminate. If the upper yield stress is above the lower limit, the force required to restore the convex drawn portion to its original shape is reduced, and thus the formability of the laminate is improved. This can improve the adaptability to an automatic packaging line, for example.
[0043] The upper limit of the upper yield point stress is not particularly limited, but can be 5,000 N / cm as an example. 2 the following.
[0044] The upper yield stress can be controlled by adjusting the material and thickness of each layer of the base layer, the fluorine-based resin layer and the intermediate layer. In the present embodiment, it is more preferably controlled by adjusting the thickness of the base layer and the composition of the intermediate layer.
[0045] The upper yield point stress is measured under the following measurement conditions.
[0046] Measuring machine: AUTOGRAPH 100A manufactured by Shimadzu Corporation
[0047] Measurement conditions: JIS K-6732 (tensile speed: 50 mm / min, test temperature: 25°C)
[0048] Test piece shape and dimensions: Based on the dimensions of JIS K-7127 test piece type 5
[0049] Unit: N / cm 2 , Value measured in accordance with JIS K 6732
[0050] Hereinafter, each layer constituting the present invention will be described.
[0051] [Base material layer]
[0052] In the present embodiment, the material forming the base material layer 12 is at least one of a polyolefin resin, a polyester resin, or a vinyl resin.
[0053] Examples of the polyolefin resin include polyethylene resin, polypropylene resin, and polymethylpentene resin.
[0054] Examples of the polyester resin include polyethylene terephthalate, polyethylene naphthalate, polyethylene isophthalate, and polybutylene terephthalate.
[0055] Examples of the vinyl resin include polyvinyl acetate resins and polyvinyl chloride resins.
[0056] In the present embodiment, a polyester resin is preferred, and polyethylene terephthalate is more preferred.
[0057] In the present embodiment, by using any one or more of the above-mentioned resins in the base material layer 12 , for example, the moldability during stretch molding is improved.
[0058] In the present embodiment, the thickness of the base layer 12 is not particularly limited, and as an example, the lower limit may be 50 μm or more, 80 μm or more, or 100 μm or more, and the upper limit may be 250 μm or less, 220 μm or less, or 200 μm or less.
[0059] The above-mentioned upper limit values and lower limit values may be combined arbitrarily.
[0060] [Middle layer]
[0061] Middle layer (1)
[0062] In the present embodiment, as the intermediate layer 10, an intermediate layer including a polyethylene-based resin and a modified polyethylene-based resin (hereinafter, sometimes referred to as "intermediate layer (1)") is preferably used.
[0063] Examples of the polyethylene resin include linear low-density polyethylene (LLDPE), low-density polyethylene (LDPE), medium-density polyethylene (MDPE), and high-density polyethylene (HDPE), and linear low-density polyethylene is preferred.
[0064] The modified polyethylene resin is a polyethylene resin modified with an unsaturated carboxylic acid or a derivative thereof, and has an acid functional group such as a carboxyl group or a carboxylic anhydride group in the polyethylene resin. In the present embodiment, a modified polyethylene resin obtained by acid-modifying a polyethylene resin is preferred.
[0065] Examples of the acid modification method include graft modification in which a polyethylene resin and an acid functional group-containing monomer are melt-kneaded in the presence of a radical polymerization initiator such as an organic peroxide or an aliphatic azo compound.
[0066] The polyethylene resin material before modification is not particularly limited as long as it contains ethylene as a raw material monomer, and known polyethylene resins can be used appropriately. Specifically, as polyethylene resins, in addition to the above examples, ethylene-propylene copolymers, ethylene-1-butene copolymers, ethylene-4-methyl-1-pentene copolymers, ethylene-1-hexene copolymers, ethylene-1-octene copolymers and other ethylene-α-olefin copolymers; ethylene-vinyl acetate copolymers, ethylene-(meth)acrylic acid copolymers, ethylene-(meth)acrylate copolymers and other ethylene copolymer resins can be listed.
[0067] The acid functional group-containing monomer is a compound having an ethylenic double bond and a carboxyl group or a carboxylic acid anhydride group in the same molecule, and examples thereof include various unsaturated monocarboxylic acids, dicarboxylic acids, or anhydrides of dicarboxylic acids.
[0068] Examples of the acid-functional monomer having a carboxyl group (carboxyl-containing monomer) include α,β-unsaturated carboxylic acid monomers such as acrylic acid, methacrylic acid, maleic acid, nadic acid, fumaric acid, itaconic acid, crotonic acid, isocrotonic acid, tetrahydrophthalic acid, and endo-bicyclo[2.2.1]hept-5-ene-2,3-dicarboxylic acid (endic acid).
[0069] Examples of the acid functional group-containing monomer having a carboxylic acid anhydride group (carboxylic acid anhydride group-containing monomer) include unsaturated dicarboxylic acid anhydride monomers such as maleic anhydride, nadic anhydride, itaconic anhydride, citraconic anhydride, and nadic anhydride.
[0070] In the components constituting the intermediate layer, these acid functional group-containing monomers may be used alone or in combination of two or more.
[0071] Among them, as the acid functional group-containing monomer, an acid functional group-containing monomer having an acid anhydride group is preferred, a carboxylic acid anhydride group-containing monomer is more preferred, and maleic anhydride is particularly preferred.
[0072] When part of the acid-containing functional group monomer used for acid modification is unreacted, it is preferable to use one from which the unreacted acid-containing functional group monomer is removed in advance in order to prevent a decrease in adhesive force due to the unreacted acid-containing functional group monomer.
[0073] In the present embodiment, the modified polyethylene-based resin is preferably maleic anhydride-modified polyethylene.
[0074] In this embodiment, when the total mass of the polyethylene resin and the modified polyethylene resin is set to 100%, the lower limit of the ratio of the polyethylene resin to the total mass of the polyethylene resin and the modified polyethylene resin is preferably 10% or more, and more preferably 20% or more. In addition, the upper limit of the ratio of the polyethylene resin to the total mass of the polyethylene resin and the modified polyethylene resin is preferably 70% or less, and more preferably 60% or less. For example, the mixing ratio of the polyethylene resin to the modified polyethylene resin can be set to [polyethylene resin]: [modified polyethylene resin] = 20:80~60:40.
[0075] In this embodiment, the adhesion between the fluorine-based resin layer and the base layer can be improved by using the intermediate layer (1) using a mixed material of a polyethylene-based resin and a modified polyethylene-based resin, thereby providing a laminate that is less likely to undergo interlayer delamination.
[0076] Middle layer (2)
[0077] In the present embodiment, it is also preferable to use, as the intermediate layer 10 , an intermediate layer (hereinafter referred to as “intermediate layer ( 2 )”) containing an acid-modified polyolefin resin, an epoxy group-containing resin, and an elastomer resin.
[0078] Here, each component contained in the intermediate layer (2) is described.
[0079] ··Acid modified polyolefin resin
[0080] The acid-modified polyolefin resin (hereinafter referred to as "component (A)") is a polyolefin resin modified with an unsaturated carboxylic acid or a derivative thereof, and has an acid functional group such as a carboxyl group or a carboxylic anhydride group in the polyolefin resin.
[0081] The component (A) is obtained by modifying a polyolefin resin with an unsaturated carboxylic acid or a derivative thereof, copolymerizing an acid functional group-containing monomer with an olefin, etc. Among them, the component (A) is preferably a polyolefin resin modified with an acid.
[0082] Examples of the acid modification method include graft modification in which a polyolefin resin and an acid functional group-containing monomer are melt-kneaded in the presence of a radical polymerization initiator such as an organic peroxide or an aliphatic azo compound.
[0083] Examples of the polyolefin resin include polyethylene, polypropylene, poly-1-butene, polyisobutylene, random copolymers of propylene and ethylene or α-olefins, block copolymers of propylene and ethylene or α-olefins, etc. Among them, polypropylene resins such as homopolypropylene (propylene homopolymer; hereinafter, sometimes referred to as "homo PP"), block copolymers of propylene-ethylene (hereinafter, sometimes referred to as "block PP"), and random copolymers of propylene-ethylene (hereinafter, sometimes referred to as "random PP") are preferred, and random PP is particularly preferred.
[0084] Examples of the olefins used in the copolymerization include olefin monomers such as ethylene, propylene, 1-butene, isobutylene, 1-hexene, and α-olefins.
[0085] The acid functional group-containing monomer is a compound having an ethylenic double bond and a carboxyl group or a carboxylic acid anhydride group in the same molecule, and examples thereof include various unsaturated monocarboxylic acids, dicarboxylic acids, or anhydrides of dicarboxylic acids.
[0086] Examples of the acid-functional monomer having a carboxyl group (carboxyl-containing monomer) include α,β-unsaturated carboxylic acid monomers such as acrylic acid, methacrylic acid, maleic acid, nadic acid, fumaric acid, itaconic acid, crotonic acid, isocrotonic acid, tetrahydrophthalic acid, and endo-bicyclo[2.2.1]hept-5-ene-2,3-dicarboxylic acid (nadic acid).
[0087] Examples of the acid functional group-containing monomer having a carboxylic acid anhydride group (carboxylic acid anhydride group-containing monomer) include unsaturated dicarboxylic acid anhydride monomers such as maleic anhydride, nadic anhydride, itaconic anhydride, citraconic anhydride, and nadic anhydride.
[0088] In the component (A), these acid functional group-containing monomers may be used alone or in combination of two or more.
[0089] Among them, since the reactivity with the component (B) described later is high, as the acid functional group-containing monomer, an acid functional group-containing monomer having an acid anhydride group is preferred, a carboxylic acid anhydride group-containing monomer is more preferred, and maleic anhydride is particularly preferred.
[0090] When part of the acid-containing functional group monomer used for acid modification is unreacted, in order to prevent the reduction of adhesive force caused by the unreacted acid-containing functional group monomer, it is preferred to use a substance from which the unreacted acid-containing functional group monomer has been removed in advance as the (A) component. Here, "unreacted" means not used for acid modification.
[0091] Among them, as the component (A), maleic anhydride-modified polypropylene is preferred from the viewpoint of being able to exhibit high adhesiveness to the fluorine-based resin layer.
[0092] ··Resins containing epoxy groups
[0093] In the present embodiment, the epoxy group-containing resin (hereinafter, referred to as "component (B)") is preferably a component having an epoxy group and a vinyl group. The epoxy group-containing resin preferably has a 1,2-vinyl structure, and more preferably is an epoxidized polybutadiene obtained by partially epoxidizing butadiene. Particularly preferably is a substance obtained by partially epoxidizing 1,2-polybutadiene.
[0094] Examples of the epoxy group-containing resin that can be used in the present embodiment include liquid polybutadiene JP-100 and JP-200 from NIPPON SODA CO., LTD. and ADK CIZER BF-1000 from ADEKA CORPORATION.
[0095] The number average molecular weight of the epoxy group-containing resin is preferably 500 or more and 4,000 or less.
[0096] By setting the number average molecular weight of the epoxy group-containing resin to be equal to or less than the above upper limit, a decrease in tackiness due to being in a solid state at room temperature can be suppressed, and a decrease in adhesiveness can be prevented.
[0097] The number average molecular weight in the present embodiment is a value in terms of polystyrene measured by GPC (gel permeation chromatography).
[0098] As the epoxy group-containing resin, epoxidized polybutadiene is particularly preferably used.
[0099] ··Elastomer resin
[0100] The elastomer resin (hereinafter referred to as "component (C)") may be any component having properties as an elastomer, and examples thereof include styrene elastomers, acrylic elastomers, urethane elastomers, olefin elastomers, and ester elastomers.
[0101] Among them, olefin elastomers are preferred, for example, block copolymers having a hard segment and a soft segment, the hard segment being composed of polystyrene, etc., and the soft segment being composed of polyethylene, polybutadiene, polyisoprene, etc. Olefin polymers that can be used for olefin elastomers include copolymers of aromatic olefins and aliphatic olefins such as styrene-butadiene copolymers, styrene-isoprene copolymers, and styrene-ethylene copolymers.
[0102] In the present embodiment, it is preferred that 1 to 50 parts by mass of component (C) be contained relative to 50 to 99 parts by mass of component (A). It is more preferred that 15 to 35 parts by mass of component (B) be contained relative to 65 to 85 parts by mass of component (C).
[0103] In the present embodiment, the thickness of the intermediate layer 10 is 5 μm or more and 50 μm or less, and preferably 10 μm or more and 30 μm or less.
[0104] In this embodiment, by setting the thickness of the intermediate layer 10 to be greater than the lower limit, adhesion can be improved and interlayer delamination can be prevented. In addition, by setting the thickness of the intermediate layer to be less than the upper limit, degradation of moldability due to thick film can be prevented.
[0105] [Fluorine resin layer]
[0106] As the fluorine resin material for the fluorine resin layer 11, polytetrafluoroethylene (PTFE), tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (PFA), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), tetrafluoroethylene-hexafluoropropylene-perfluoroalkyl vinyl ether (EPA), tetrafluoroethylene-ethylene copolymer (ETFE), polyvinylidene fluoride (PVDF), polychlorotrifluoroethylene (PCTFE), chlorotrifluoroethylene-ethylene copolymer (ECTFE) and a mixture of one or more of these materials can be used, preferably polychlorotrifluoroethylene (PCTFE).
[0107] In the present embodiment, the thickness of the fluorine-based resin layer 11 is 20 μm to 150 μm, preferably 25 μm to 100 μm, and more preferably 30 μm to 50 μm.
[0108] In this embodiment, by setting the thickness of the fluorine-based resin layer 11 to be greater than the above lower limit, the water vapor permeability of the laminate can be reduced. For example, when used in blister packaging for medicines, high moisture resistance can be achieved to prevent degradation of the contents due to water vapor.
[0109] In the present embodiment, by setting the thickness of the fluorine-based resin layer 11 to be equal to or less than the above upper limit, the production cost can be reduced.
[0110] Second Implementation Method
[0111] Reference Figure 2 , a second embodiment of the laminated body of the present invention is described.
[0112] Figure 2 The laminated body 2 of the present embodiment shown is composed of a base material layer 12 , an intermediate layer 10 , a fluorine-based resin layer 11 , a second intermediate layer 13 , and a second base material layer 14 laminated in this order.
[0113] The laminated body 2 having a five-layer structure is preferred because of its high laminated body strength. In addition, the laminated body 2 having a five-layer structure is preferred because it is less likely to curl.
[0114] The materials constituting the base layer, the intermediate layer, and the fluorine-based resin layer in this embodiment are the same as those described in the first embodiment.
[0115] The description of the material constituting the second base layer 14 is the same as that of the base layer 12. The material of the second base layer 14 and the base layer 12 may be the same or different, but preferably the same material.
[0116] The description of the material constituting the second intermediate layer 13 is the same as that of the intermediate layer 10. The material of the second intermediate layer 13 and the intermediate layer 10 may be the same or different, but preferably the same material.
[0117] The water vapor permeability of the laminate 2 of the present embodiment is 0.5 g / m 2 / 24 hours or less, preferably 0.4g / m 2 / 24 hours or less, more preferably 0.3g / m 2 / Less than 24 hours.
[0118] Since the water vapor permeability of the laminate of the present embodiment is within the above-mentioned specific range, when, for example, a blister package for medicine is produced, the laminate can exhibit high barrier properties and prevent the deterioration of the contents.
[0119] Similar to the first embodiment, in this embodiment, the water vapor permeability of the laminate 2 can be controlled by adjusting the material and thickness of each layer of the substrate layer 12, the intermediate layer 10, the fluorine-based resin layer 11, the second intermediate layer 13, and the second substrate layer 14. In this embodiment, it is particularly preferred to control the water vapor permeability within the above-mentioned specific numerical range by adjusting the material and thickness of the fluorine-based resin layer 11, and it is more preferred to control it by adjusting the thickness of the fluorine-based resin layer 11.
[0120] The upper yield stress of the laminate of the present embodiment measured under the above-mentioned measurement conditions is preferably 1,500 N / cm 2 More preferably, 2,000 N / cm 2 More than, particularly preferably 2,200 N / cm 2 above.
[0121] By setting the upper yield stress of the laminate to be equal to or greater than the lower limit, the deep drawing property of the laminate is improved, and thus, for example, the laminate can be more compatible with an automatic packaging line.
[0122] The upper yield point stress can be controlled by adjusting the material and thickness of each layer of the substrate layer, the fluororesin layer and the intermediate layer. In the present embodiment, it is more preferably controlled by adjusting the thickness of the substrate layer 12 and the second substrate layer 14, and the composition of the intermediate layer 10 and the second intermediate layer 13.
[0123] In the present embodiment, the material constituting the base material layer 12 and the material constituting the second base material layer 14 may be the same or different, but are preferably made of the same resin material.
[0124] The thickness of the second base layer 14 is preferably 0.5 to 1.1 times, more preferably 0.9 to 1.1 times, and particularly preferably 0.95 to 1.05 times that of the base layer 12 .
[0125] In the present embodiment, the material constituting the intermediate layer 10 and the material constituting the second intermediate layer 13 may be the same or different, but are preferably made of the same resin material.
[0126] The thickness of the second intermediate layer 13 is more preferably 0.9 to 1.1 times, and particularly preferably 0.95 to 1.05 times, that of the intermediate layer 10 .
[0127] The upper limit of the total film thickness of the laminate of the present invention is 400 μm or less, preferably 300 μm or less. In addition, the lower limit of the total film thickness is preferably 80 μm or more, more preferably 200 μm or more. By setting it to this film thickness, it is easy to protect the contents and easy to store and use after molding.
[0128] <Blister container, blister pack>
[0129] The blister container and the blister package according to the embodiment of the present invention are manufactured by deep drawing the laminated body according to the first or second embodiment of the present invention.
[0130] When the laminated body 1 according to the first embodiment of the present invention is used, the fluorine-based resin layer 11 may be placed on the inside or outside, but is preferably molded on the outside.
[0131] The blister package according to the embodiment of the present invention is used for individual packaging of tablets or capsules, for example.
[0132] Since the water vapor permeability of the laminate of the present invention is low, deterioration of the contents such as tablets and capsules can be prevented.
[0133] The laminated body according to the first embodiment of the present invention is preferably produced by simultaneously melt-extruding a resin as a raw material for the base layer, a resin as a raw material for the intermediate layer, and a resin as a raw material for the fluorine-based resin layer.
[0134] In addition, the laminate of the second embodiment is preferably manufactured by simultaneously melt-extruding a resin serving as the raw material for the substrate layer, a resin serving as the raw material for the intermediate layer, a resin serving as the raw material for the fluorine-based resin layer, a resin serving as the raw material for the second intermediate layer, and a resin serving as the raw material for the second substrate layer.
[0135] Example
[0136] Hereinafter, the present invention will be described in further detail using examples, but the present invention is not limited to these examples.
[0137] <Three-layer laminate>
[0138] 《Examples 1 to 5, Comparative Examples 1 to 2》
[0139] A laminate having a three-layer structure with a substrate layer, an intermediate layer, and a fluorine-based resin layer in sequence was manufactured. The resins as raw materials for each layer shown in Table 1 were heated and melted, and multilayer film was formed using an extruder capable of co-extrusion multilayer molding to obtain a laminate having a three-layer structure with a substrate layer, an intermediate layer, and a fluorine-based resin layer in sequence.
[0140] The water vapor transmission rate of each obtained laminate was measured by the following method.
[0141] [Water vapor transmission rate measurement]
[0142] The laminate obtained according to the above-mentioned <Three-layer laminate> was measured using a water vapor transmission rate tester (manufactured by Systech Instruments Ltd and Illinois Instruments, Inc., product name "L80-5000") in accordance with JIS K7129:2008 (method A) at a test chamber temperature (cell temperature) of 40°C and a relative humidity difference of 90% RH. The water vapor transmission rate is measured in grams of water vapor permeating per square meter of area in 24 hours [g / m 2 / 24h] indicates.
[0143] [Table 1]
[0144]
[0145] In Table 1, each symbol represents the following material. The value in [ ] is the thickness of each layer.
[0146] ·PET: polyethylene terephthalate resin. NOVAPEX I4 manufactured by Mitsubishi Chemical Corporation was used.
[0147] ·PCTFE: polychlorotrifluoroethylene resin. DF0050-C1 manufactured by DAIKIN INDUSTRIES, LTD. was used.
[0148] ECTFE: Chlorotrifluoroethylene-ethylene copolymer.
[0149] · Intermediate layers 1 to 3: Intermediate layers 1 to 3 shown in the following Table 2. The ratio of each material in Table 2 is a mass ratio (%).
[0150] [Table 2]
[0151]
[0152] ·evaluate
[0153] The following tests were performed on each of the laminated bodies of Examples 1 to 5 and Comparative Examples 1 and 2.
[0154] [Upper yield point stress]
[0155] The upper yield point stress is measured under the following measurement conditions.
[0156] Measuring machine: AUTOGRAPH 100A manufactured by Shimadzu Corporation
[0157] Measurement conditions: JIS K-6732 (tensile speed: 50 mm / min, test temperature: 25°C)
[0158] Test piece shape and dimensions: Based on the dimensions of JIS K-7127 test piece type 5
[0159] Unit: N / cm 2 , Value measured in accordance with JIS K 6732
[0160] [Moldability]
[0161] The presence or absence of molding defects during the molding of the blister package was visually observed, and the moldability of the laminate was evaluated according to the following criteria.
[0162] ◎: The thickness of the drawn portion is uneven, and the shape after drawing is maintained very well.
[0163] ○: The thickness of the drawn portion is uneven, and the shape after drawing is generally well maintained.
[0164] △: The drawn portion has a slight uneven thickness or the shape cannot be maintained after drawing.
[0165] ×: The thickness of the drawn portion is uneven, or the shape of the drawn portion cannot be maintained after drawing.
[0166] [Contents protection]
[0167] Blister packages were prepared using the laminates of Examples 1 to 5 and Comparative Examples 1 to 2, and the contents (deliquescent test agents) were placed in the packages, and the degradation of the contents was visually evaluated according to the following criteria. At this time, the blister packages were prepared with the fluorine-based resin layer of the laminate facing the outside.
[0168] ◎; No deterioration of the contents was observed.
[0169] ○: Almost no deterioration of the contents was observed.
[0170] △: Deterioration of the contents was slightly observed.
[0171] ×: Remarkable deterioration of the contents was observed.
[0172] [determination]
[0173] Each evaluation item is comprehensively judged and determined, and a three-stage evaluation is performed (◎, ○, ×).
[0174] [Table 3]
[0175]
[0176] As shown in the above results, the laminates of Examples 1 to 5, to which the fluorine-based resin layer of the present invention is applied, have a specific thickness and a water vapor permeability of the laminate in a specific range, have high upper yield stress, good moldability, and good protection of the contents. In contrast, the laminate of Comparative Example 1, in which the thickness of the fluorine-based resin layer is outside the range of the present invention, has poor moldability, and the laminate of Comparative Example 2, in which the water vapor permeability value is outside the range of the present invention, has poor protection of the contents.
[0177] <Five-layer laminate>
[0178] 《Examples 6 to 10, Comparative Examples 3 to 4》
[0179] A laminate having a five-layer structure of a substrate layer, an intermediate layer, a fluorine-based resin layer, a second intermediate layer, and a second substrate layer in sequence was manufactured. The resins as raw materials for each layer shown in Table 4 were heated and melted, and multilayer film-forming was performed using an extruder capable of co-extrusion multilayer molding to obtain a laminate having a five-layer structure of a substrate layer, an intermediate layer, a fluorine-based resin layer, a second intermediate layer, and a second substrate layer in sequence.
[0180] [Table 4]
[0181]
[0182] In Table 4, each symbol represents the following material. The value in [ ] is the thickness of each layer.
[0183] ·PET: polyethylene terephthalate resin. NOVAPEX I4 manufactured by Mitsubishi Chemical Corporation was used.
[0184] ·PCTFE: polychlorotrifluoroethylene resin. DF0050-C1 manufactured by DAIKIN INDUSTRIES, LTD. was used.
[0185] · Intermediate layers 1 to 3: Intermediate layers 1 to 3 shown in Table 2 above.
[0186] [Water vapor transmission rate]
[0187] The measurement was performed by the same method as above.
[0188] ·evaluate
[0189] The upper yield stress, content protection and moldability of each of the laminates of Examples 6 to 10 and Comparative Examples 3 to 4 were evaluated by the same method as above. The results are shown in Table 5.
[0190] [Table 5]
[0191]
[0192] As shown in the above results, the laminates of Examples 6 to 10, in which the fluorine-based resin layer has a specific thickness and the water vapor permeability of the laminate is within a specific range, have high upper yield stress and good formability and protection of the contents. In contrast, the laminate of Comparative Example 3, in which the thickness of the fluorine-based resin layer is outside the range of the present invention and the water vapor permeability is also outside the range of the present invention, has poor formability. In addition, the laminate of Comparative Example 4 has poor protection of the contents because the thickness of the fluorine-based resin layer is thin.
Claims
1. A laminated body comprising a substrate layer, an intermediate layer, a fluorine-based resin layer, a second intermediate layer and a second substrate layer in this order, and having a total film thickness of 400 μm or less, characterized in that: The thickness of the substrate layer is not less than 100 μm and not more than 200 μm, and the thickness of the second substrate layer is 0.5 to 1.1 times of the thickness of the substrate layer. The thickness of the intermediate layer is not less than 10 μm and not more than 30 μm, and the thickness of the second intermediate layer is 0.9 to 1.1 times of the thickness of the intermediate layer. The thickness of the fluorine-based resin layer is not less than 20 μm and not more than 150 μm. The water vapor permeability of the laminate is 0.5 g / m 2 / 24 hours or less, The upper yield stress of the laminate is 1,500 N / cm 2 above, The substrate layer and the second substrate layer each contain only polyethylene terephthalate, The intermediate layer and the second intermediate layer each contain only a linear low-density polyethylene and a maleic anhydride-modified polyethylene, and the content of the linear low-density polyethylene is 10% by mass or more and 70% by mass or less relative to 100% by mass of the total of the linear low-density polyethylene and the maleic anhydride-modified polyethylene, The fluorine-based resin layer contains polychlorotrifluoroethylene. 2 . A blister container comprising the laminate according to claim 1 . 3 . A blister package comprising the laminate according to claim 1 .
Citation Information
Patent Citations
High moisture barrier films
CN1222408C