Thin polyurethane composite material for consumer electronics and preparation method thereof

By using a combination of glass fiber cloth and water-based polyurethane materials in consumer electronic decorative materials, the problem of heavy traditional materials is solved, and a high-strength, lightweight and environmentally friendly polyurethane composite material is achieved to meet the lightness and durability requirements of high-end products.

CN119058212AActive Publication Date: 2024-12-03ANHUI ANLI MATERIAL TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411395788.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-08
Publication Date
2024-12-03
Estimated Expiration
2044-10-08

AI Technical Summary

Technical Problem

Traditional consumer electronics decorative materials have thick thickness and average strength and durability, which cannot meet the high requirements of high-end consumer electronics such as thinness, weight loss and durability.

Method used

Using glass fiber cloth as the base cloth layer, and the adhesion promoter emulsion is treated on its surface, combined with aqueous polyurethane material, to form a composite structure consisting of an aqueous polyurethane surface layer, an aqueous polyurethane intermediate layer and an aqueous polyurethane adhesive layer, through silanol molecules The association forms a mesh structure, improves the bonding force between polyurethane and glass fiber cloth, and produces a thin polyurethane composite material.

Benefits of technology

The lightweight and strength improvement of polyurethane synthetic leather has been achieved. The thin polyurethane composite material produced is thin, light in weight, high strength and good durability, which meets the thinning and lightening requirements of high-end consumer electronic products, and uses environmentally friendly water-based materials. , reducing material costs and energy consumption.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a thin polyurethane composite material for consumer electronics and a preparation method thereof, and the thin polyurethane composite material for consumer electronics sequentially comprises a waterborne polyurethane surface layer, a waterborne polyurethane middle layer, a waterborne polyurethane bonding layer and a base cloth layer from outside to inside, the base cloth layer is made of glass fabric, and the side, facing the waterborne polyurethane bonding layer, of the glass fabric is coated with adhesion promoter emulsion. According to the invention, the glass fabric is innovatively applied to the field of polyurethane synthetic leather manufacturing, so that the weight of the polyurethane synthetic leather can be reduced, the strength and toughness of the polyurethane synthetic leather can be improved, and the prepared thin polyurethane composite material has the advantages of thin thickness, light gram weight, high strength, good durability and the like; and the development requirements of thinning, lightening and enhancing consumer electronic decorative materials are met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of polyurethane composite materials, and in particular to a thin polyurethane composite material for consumer electronics and a preparation method thereof. Background Art

[0002] There are many choices for decorative materials for consumer electronic products, such as plastic, metal, glass, ceramic, leather, etc. Each material has its own characteristics, for example: plastic is low-grade; metal affects the signal; glass is easy to break; leather feels good and is high-grade, but has disadvantages such as poor wear resistance and poor durability. In recent years, polyurethane consumer electronic decorative materials that are close to the feel of leather have gradually become popular. This material has a full and delicate feel, high-grade feel, will not break, and is resistant to aging. It solves the problems of poor wear resistance, easy breakage during use, and low service life of leather materials, and is favored by various consumer electronic manufacturers.

[0003] With the development of society, consumers have higher and higher requirements for product quality. Traditional consumer electronic decorative materials are thick and have average strength and durability, which can no longer meet the high requirements of high-end consumer electronic products such as lightness, weight reduction and durability. Therefore, a light, high-strength and durable composite material has become a new demand direction. Summary of the invention

[0004] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a thin polyurethane composite material for consumer electronics and a preparation method thereof. The base fabric layer of the thin polyurethane composite material for consumer electronics adopts glass fiber cloth treated with an adhesion promoter emulsion, which can not only reduce the weight of the polyurethane synthetic leather, but also improve the strength and toughness of the polyurethane synthetic leather. The prepared thin polyurethane composite material has the advantages of thin thickness, light weight, high strength, good durability, etc., and is more in line with the development requirements of thinning, lightening and strengthening of consumer electronic decorative materials.

[0005] To achieve the above object, the present invention adopts the following technical solutions:

[0006] The present invention provides a thin polyurethane composite material for consumer electronics, which comprises, from the outside to the inside, a water-based polyurethane surface layer, a water-based polyurethane middle layer, a water-based polyurethane adhesive layer, and a base fabric layer. The base fabric layer is made of glass fiber cloth, and a layer of adhesion promoter emulsion coating is formed on the side of the glass fiber cloth facing the water-based polyurethane adhesive layer.

[0007] As a further improvement of the above solution of the present invention, the thickness of the glass fiber cloth is 0.08-0.1 mm.

[0008] As a further improvement of the above-mentioned scheme of the present invention, the water-based polyurethane surface layer is made of water-based silicon-based polyurethane slurry, and the water-based silicon-based polyurethane slurry is prepared from the following components in parts by weight: 100 parts of water-based silicon-based polyurethane slurry, 2-5 parts of water-based curing agent, 0.5-2 parts of water-based leveling agent, 0.1-0.5 parts of defoaming agent, 0.5-2 parts of water-based thickener, and 5-20 parts of water-based color paste.

[0009] As a further improvement of the above scheme of the present invention, the water-based polyurethane intermediate layer is made of water-based polycarbon type polyurethane slurry, and the water-based polycarbon type polyurethane slurry is prepared from the following components in parts by weight: 100 parts of water-based polycarbon type polyurethane slurry, 2-5 parts of water-based curing agent, 0.5-2 parts of water-based leveling agent, 0.1-0.5 parts of defoaming agent, 0.5-2 parts of water-based thickener, and 5-20 parts of water-based color paste.

[0010] As a further improvement of the above scheme of the present invention, the water-based polyurethane adhesive layer is made of a water-based two-component polyether polyurethane slurry, and the water-based two-component polyether polyurethane slurry is prepared from the following components in parts by weight: 100 parts of water-based two-component polyether polyurethane slurry, 5-10 parts of water-based sealing curing agent, 0.5-1 part of water-based leveling agent, 0.1-0.4 part of defoaming agent, 0.5-2 parts of water-based thickener, and 5-10 parts of water-based color paste.

[0011] The present invention provides a method for preparing the aforementioned thin polyurethane composite material for consumer electronics, which comprises the following steps:

[0012] S1. Apply a layer of adhesion promoter emulsion on the surface of the glass fiber cloth and dry it to obtain a base cloth layer;

[0013] S2. Coating a layer of waterborne polyurethane surface slurry on the release paper and drying the waterborne polyurethane surface layer;

[0014] S3. Coating a layer of aqueous polyurethane intermediate layer slurry on the aqueous polyurethane surface layer and drying the aqueous polyurethane intermediate layer;

[0015] S4. Coat a layer of water-based polyurethane adhesive layer slurry on the water-based polyurethane intermediate layer, completely dry the water-based polyurethane adhesive layer, laminate the water-based polyurethane adhesive layer to the base fabric layer, dry and mature the layer, roll it up, mature it in a 60° C. curing room for 12-72 hours, peel off the release paper, and obtain a thin polyurethane composite material for consumer electronics.

[0016] As a further improvement of the above scheme of the present invention, in step S1, the coating amount of the adhesion promoter emulsion is 20-30 g / cm 2 The drying temperature is 100-130°C and the vehicle speed is 6-10m / min.

[0017] As a further improvement of the above scheme of the present invention, in step S2, the coating thickness of the waterborne polyurethane surface slurry is 0.1-0.15 mm, the drying temperature is 90-140° C., and the vehicle speed is 6-10 m / min.

[0018] As a further improvement of the above scheme of the present invention, in step S3, the coating thickness of the aqueous polyurethane intermediate layer slurry is 0.15-0.20 mm, the drying temperature is 90-140° C., and the vehicle speed is 6-10 m / min.

[0019] As a further improvement of the above scheme of the present invention, in step S4, the coating thickness of the waterborne polyurethane adhesive layer slurry is 0.2-0.25 mm, the drying temperature is 80-110° C., the drying and aging temperature is 140-160° C., and the vehicle speed is 6-10 m / min.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] 1. The present invention innovatively uses glass fiber cloth in the field of polyurethane synthetic leather manufacturing. Since glass fiber cloth is an inorganic material and is difficult to react with polyurethane, glass fiber cloth is used as the base cloth layer. At the same time, a layer of adhesion promoter emulsion is treated on the surface of the glass fiber cloth. The silanol molecules generated after hydrolysis are mutually associated and aggregated into a network structure covering the surface of the glass fiber cloth, thereby realizing the organicization of the inorganic glass fiber cloth, thereby realizing the reaction and combination between the glass fiber cloth and the polyurethane, which can not only reduce the weight of the polyurethane synthetic leather, but also improve the strength and toughness of the polyurethane synthetic leather. The obtained thin polyurethane composite material has the advantages of thin thickness, light weight, high strength, good durability, etc., which is more in line with the development requirements of thinning, lightening and strengthening of consumer electronic decorative materials, and provides a new choice for decorative materials for consumer electronic products such as mobile phones and tablets.

[0022] 2. The present invention uses glass fiber cloth with a thickness of 0.08-0.1mm, and the obtained glass fiber polyurethane composite material has a thickness of 0.2-0.22mm and a gram weight of 180-250g / m 2 , the breaking strength is greater than 400N / 3CM, while the thickness of traditional consumer electronic composite materials is more than 0.25mm and the weight is more than 300g / m 2 , the breaking strength can only be guaranteed to be greater than 100N / 3CM. In comparison, the polyurethane composite material prepared by the present invention is thinner and lighter, has higher strength, and is more in line with the development requirements of thinning, lightening and strengthening of consumer electronic decorative materials.

[0023] 3. This invention innovatively uses water-based silicone-based polyurethane material as the surface layer, which has a strong skin-friendly feel, is stain-resistant and wear-resistant, and does not require additional anti-fouling treatment steps, thereby reducing material costs and energy consumption.

[0024] 4. The materials used in the present invention are all water-based environmentally friendly materials, which are more friendly to the ecological environment.

[0025] 5. The thin polyurethane composite material prepared by the present invention is more suitable for the use requirements of various high-end consumer electronic products that are becoming increasingly lighter, thinner and more durable than traditional consumer electronic decorative materials. DETAILED DESCRIPTION

[0026] For ease of understanding of the present invention, the present invention will be described more fully below in conjunction with specific embodiments. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thoroughly understood.

[0027] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.

[0028] The specific information of the raw materials used in the following examples and comparative examples is as follows:

[0029] Fiberglass cloth: electronic fiberglass cloth produced by Taishan Fiberglass Co., Ltd.;

[0030] Adhesion promoter emulsion: Dow Corning Z-6011;

[0031] Water-based polycarbonate polyurethane slurry: Stahl WF-73-575;

[0032] Water-based silicone-based polyurethane slurry: SLOCK 1089R7;

[0033] Water-based two-component polyether polyurethane slurry: Anke Chemical 3355;

[0034] Water-based thickener: Wanhua Chemical U-506;

[0035] Defoamer: Stahl 2459;

[0036] Water-based curing agent: SF-150, produced by Zhejiang Shunfa Chemical Additives Co., Ltd.;

[0037] Water-based leveling agent: Stahl LA-91-120;

[0038] Water-based color paste: water-based color paste produced by Zhejiang Deep Blue New Materials Co., Ltd.;

[0039] Water-based sealing curing agent: Stahl XR-22-903.

[0040] The above raw materials are only for illustrating the sources and components of the reagents used in the experiments of the present invention so as to fully disclose the information, and do not mean that the present invention cannot be realized by using other similar reagents or reagents provided by other suppliers.

[0041] Example 1

[0042] This embodiment provides a thin polyurethane composite material for consumer electronics, which is prepared by the following steps:

[0043] S1. A layer of adhesion promoter emulsion is applied by roller coating on the surface of glass fiber cloth with a thickness of 0.08 mm. The coating amount of adhesion promoter emulsion is 20 g / m2 by wet weight. 2 , and then dried in an oven, the drying conditions are: temperature 100 ° C, speed 10m / min, to obtain a semi-finished base fabric;

[0044] S2. A layer of water-based silicone-based polyurethane slurry having a thickness of 0.1 mm was coated on the release paper and dried in an oven under the following conditions: a temperature of 90°C and a speed of 10 m / min to obtain a water-based polyurethane surface layer;

[0045] The water-based silicone-based polyurethane slurry is prepared from the following raw materials in parts by weight: 100 parts of water-based silicone-based polyurethane 1089R7, 2 parts of water-based curing agent SF-150, 0.5 parts of water-based leveling agent LA-91-120, 0.1 parts of defoamer 2459, 0.6 parts of water-based thickener U-506, and 20 parts of water-based color paste;

[0046] S3. A layer of waterborne polycarbonate polyurethane slurry having a thickness of 0.15 mm was coated on the waterborne polyurethane surface layer, and the waterborne polyurethane intermediate layer was obtained after drying in an oven. The drying conditions were: temperature 90 ° C, speed 10 m / min;

[0047] The water-based polycarbonate polyurethane slurry is prepared from the following raw materials in parts by weight: 100 parts of water-based polycarbonate polyurethane WF-73-575, 2 parts of water-based curing agent SF-150, 0.5 parts of water-based leveling agent LA-91-120, 0.1 parts of defoaming agent 2459, 0.6 parts of water-based thickener U-506, and 20 parts of water-based color paste;

[0048] S4. Coat a layer of 0.2 mm thick water-based two-component polyether polyurethane slurry on the surface of the water-based polyurethane intermediate layer, dry it completely in an oven at 110°C, and then laminate it with the semi-finished base fabric obtained in step S1, and continue to put it into the oven for drying and aging. The drying and aging conditions are: temperature 140°C, speed 10m / min; then roll it directly without peeling off the release paper, and then put it in a 60°C aging room for 12 hours. After the aging is completed, peel off the release paper to obtain a finished thin polyurethane composite material for consumer electronics;

[0049] Among them, the water-based two-component polyether polyurethane slurry is prepared from the following raw materials in parts by weight: 100 parts of water-based two-component polyether polyurethane 3355, 5 parts of water-based closed curing agent XR-22-903, 0.5 parts of water-based leveling agent LA-91-120, 0.1 parts of defoaming agent 2459, 0.6 parts of water-based thickener U-506, and 10 parts of water-based color paste.

[0050] The thin polyurethane composite material for consumer electronics prepared in this embodiment has a thickness of 0.2 mm (reference standard: GB / T8949-2008) and a gram weight of 180-190 g / m 2 (Reference standard: ASTM D751); Peel ≥40N / 3CM (Reference standard: GB / T8949-2008); Breaking strength ≥400N / 3CM (Reference standard: GB / T 8949-2008); Wear resistance: wet wool felt*1Kg*5000 times without breaking; 70℃*95%RH constant temperature and humidity test for 5 weeks without fogging; No powdering (Reference standard: QB / T 4671-2014).

[0051] Example 2

[0052] This embodiment provides a thin polyurethane composite material for consumer electronics, which is prepared by the following steps:

[0053] S1. A layer of adhesion promoter emulsion is applied by roller coating on the surface of glass fiber cloth with a thickness of 0.083 mm. The coating amount of adhesion promoter emulsion is 22 g / m2 by wet weight. 2 Then, it is dried in an oven at a temperature of 110°C and a speed of 9 m / min to obtain a semi-finished base fabric.

[0054] S2. A layer of water-based silicone-based polyurethane slurry having a thickness of 0.11 mm was coated on the release paper and dried in an oven under the following conditions: a temperature of 100 ° C and a speed of 9 m / min to obtain a water-based polyurethane surface layer;

[0055] The water-based silicone-based polyurethane slurry is prepared from the following raw materials in parts by weight: 100 parts of water-based silicone-based polyurethane 1089R7, 2.5 parts of water-based curing agent SF-150, 0.8 parts of water-based leveling agent LA-91-120, 0.2 parts of defoamer 2459, 0.5 parts of water-based thickener U-506, and 16 parts of water-based color paste;

[0056] S3. A layer of waterborne polycarbonate polyurethane slurry having a thickness of 0.16 mm was coated on the waterborne polyurethane surface layer, and the waterborne polyurethane intermediate layer was obtained after drying in an oven. The drying conditions were: temperature 100 ° C, speed 9 m / min;

[0057] The water-based polycarbonate polyurethane slurry is prepared from the following raw materials in parts by weight: 100 parts of water-based polycarbonate polyurethane WF-73-575, 2.5 parts of water-based curing agent SF-150, 0.8 parts of water-based leveling agent LA-91-120, 0.2 parts of defoamer 2459, 0.5 parts of water-based thickener U-506, and 16 parts of water-based color paste;

[0058] S4. Coat a layer of 0.21 mm thick water-based two-component polyether polyurethane slurry on the surface of the water-based polyurethane intermediate layer, dry it completely in an oven at 105°C, and then laminate it with the semi-finished base fabric obtained in step S1, and continue to put it into the oven for drying and aging. The drying and aging conditions are: temperature 145°C, vehicle speed 9m / min; then roll it directly without peeling off the release paper, and then put it in a 60°C aging room for 24 hours. After the aging is completed, peel off the release paper to obtain a finished thin polyurethane composite material for consumer electronics;

[0059] Among them, the water-based two-component polyether polyurethane slurry is prepared from the following raw materials in parts by weight: 100 parts of water-based two-component polyether polyurethane 3355, 6 parts of water-based closed curing agent XR-22-903, 0.6 parts of water-based leveling agent LA-91-120, 0.15 parts of defoamer 2459, 0.5 parts of water-based thickener U-506, and 9 parts of water-based color paste.

[0060] The thin polyurethane composite material for consumer electronics prepared in this embodiment has a thickness of 0.21 mm (reference standard: GB / T8949-2008); a gram weight of 190-200 g / m 2 (Reference standard: ASTM D751); Peel ≥45N / 3CM (Reference standard: GB / T8949-2008); Breaking strength ≥450N / 3CM (Reference standard: GB / T 8949-2008); Wear resistance: wet wool felt*1Kg*5500 times without breaking; 70℃*95%RH constant temperature and humidity test for 6 weeks without fogging; No powdering (Reference standard: QB / T 4671-2014).

[0061] Example 3

[0062] This embodiment provides a thin polyurethane composite material for consumer electronics, which is prepared by the following steps:

[0063] S1. A layer of adhesion promoter emulsion is applied by roller coating on the surface of glass fiber cloth with a thickness of 0.085 mm. The coating amount of adhesion promoter emulsion is 24 g / m2 by wet weight. 2 Then, it is dried in an oven at a temperature of 115°C and a speed of 8m / min to obtain a semi-finished base fabric.

[0064] S2. A layer of water-based silicone-based polyurethane slurry having a thickness of 0.12 mm was coated on the release paper and dried in an oven under the following drying conditions: a temperature of 110 ° C and a speed of 8 m / min to obtain a water-based polyurethane surface layer;

[0065] The water-based silicone-based polyurethane slurry is prepared from the following raw materials in parts by weight: 100 parts of water-based silicone-based polyurethane 1089R7, 3 parts of water-based curing agent SF-150, 1.2 parts of water-based leveling agent LA-91-120, 0.3 parts of defoamer 2459, 0.8 parts of water-based thickener U-506, and 14 parts of water-based color paste;

[0066] S3. A layer of waterborne polycarbonate polyurethane slurry having a thickness of 0.17 mm was coated on the waterborne polyurethane surface layer, and the waterborne polyurethane intermediate layer was obtained after drying in an oven. The drying conditions were: temperature 110 ° C, speed 8 m / min;

[0067] The water-based polycarbonate polyurethane slurry is prepared from the following raw materials in parts by weight: 100 parts of water-based polycarbonate polyurethane WF-73-575, 3 parts of water-based curing agent SF-150, 1.2 parts of water-based leveling agent LA-91-120, 0.3 parts of defoamer 2459, 0.8 parts of water-based thickener U-506, and 14 parts of water-based color paste;

[0068] S4. Coating a layer of 0.22 mm thick water-based two-component polyether polyurethane slurry on the surface of the water-based polyurethane intermediate layer, completely drying in an oven at 100° C., and then laminating the semi-finished base fabric obtained in step S1, and continuing to put it into the oven for drying and aging. The drying and aging conditions are: temperature 150° C., speed 8 m / min; then rolling it directly without peeling off the release paper, and then putting it in a 60° C. aging room for 36 hours. After the aging is completed, the release paper is peeled off to obtain a finished thin polyurethane composite material for consumer electronics;

[0069] Among them, the water-based two-component polyether polyurethane slurry is prepared from the following raw materials in parts by weight: 100 parts of water-based two-component polyether polyurethane 3355, 7 parts of water-based closed curing agent XR-22-903, 0.7 parts of water-based leveling agent LA-91-120, 0.2 parts of defoaming agent 2459, 0.8 parts of water-based thickener U-506, and 8 parts of water-based color paste.

[0070] The thin polyurethane composite material for consumer electronics prepared in this embodiment has a thickness of 0.22 mm (reference standard: GB / T8949-2008) and a gram weight of 200-210 g / m 2(Reference standard: ASTM D751); Peel ≥50N / 3CM (Reference standard: GB / T8949-2008); Breaking strength ≥480N / 3CM (Reference standard: GB / T 8949-2008); Wear resistance: wet wool felt*1Kg*6000 times without breaking; 70℃*95%RH constant temperature and humidity test for 7 weeks without fogging; No powdering (Reference standard: QB / T 4671-2014).

[0071] Example 4

[0072] This embodiment provides a thin polyurethane composite material for consumer electronics, which is prepared by the following steps:

[0073] S1. A layer of adhesion promoter emulsion is applied by roller coating on the surface of glass fiber cloth with a thickness of 0.09 mm. The coating amount of adhesion promoter emulsion is 26 g / m2 by wet weight. 2 Then, it is dried in an oven at a temperature of 120°C and a speed of 7 m / min to obtain a semi-finished base fabric;

[0074] S2. A layer of water-based silicone-based polyurethane slurry having a thickness of 0.13 mm was coated on the release paper and dried in an oven under the following conditions: a temperature of 120°C and a speed of 7 m / min to obtain a water-based polyurethane surface layer;

[0075] The water-based silicone-based polyurethane slurry is prepared from the following raw materials in parts by weight: 100 parts of water-based silicone-based polyurethane 1089R7, 3.5 parts of water-based curing agent SF-150, 1.5 parts of water-based leveling agent LA-91-120, 0.4 parts of defoamer 2459, 1 part of water-based thickener U-506, and 12 parts of water-based color paste;

[0076] S3. A layer of waterborne polycarbonate polyurethane slurry having a thickness of 0.18 mm was coated on the waterborne polyurethane surface layer, and the waterborne polyurethane intermediate layer was obtained after drying in an oven. The drying conditions were: temperature 120 ° C, speed 7 m / min;

[0077] The water-based polycarbonate polyurethane slurry is prepared from the following raw materials in parts by weight: 100 parts of water-based polycarbonate polyurethane WF-73-575, 3.5 parts of water-based curing agent SF-150, 1.5 parts of water-based leveling agent LA-91-120, 0.4 parts of defoamer 2459, 1 part of water-based thickener U-506, and 12 parts of water-based color paste;

[0078] S4. Coat a layer of 0.23 mm thick water-based two-component polyether polyurethane slurry on the surface of the water-based polyurethane intermediate layer, dry it completely in an oven at 95°C, and then laminate it with the semi-finished base fabric obtained in step S1, and continue to put it into the oven for drying and aging. The drying and aging conditions are: temperature 153°C, speed 8m / min; then roll it directly without peeling off the release paper, and then put it in a 60°C aging room for 48 hours. After the aging is completed, peel off the release paper to obtain a finished thin polyurethane composite material for consumer electronics;

[0079] Among them, the water-based two-component polyether polyurethane slurry is prepared from the following raw materials in parts by weight: 100 parts of water-based two-component polyether polyurethane 3355, 8 parts of water-based closed curing agent XR-22-903, 0.8 parts of water-based leveling agent LA-91-120, 0.25 parts of defoaming agent 2459, 1 part of water-based thickener U-506, and 7 parts of water-based color paste.

[0080] The thin polyurethane composite material for consumer electronics prepared in this embodiment has a thickness of 0.235 mm (reference standard: GB / T 8949-2008); a gram weight of 210-220 g / m 2 (Reference standard: ASTM D751); Peel ≥55N / 3CM (Reference standard: GB / T 8949-2008); Breaking strength ≥500N / 3CM (Reference standard: GB / T 8949-2008); Wear resistance: wet wool felt*1Kg*4000 times without breaking; 70℃*95%RH constant temperature and humidity test for 8 weeks without fogging; No powdering (Reference standard: QB / T 4671-2014).

[0081] Example 5

[0082] This embodiment provides a thin polyurethane composite material for consumer electronics, which is prepared by the following steps:

[0083] S1. A layer of adhesion promoter emulsion is applied by roller coating on the surface of glass fiber cloth with a thickness of 0.095 mm. The coating amount of adhesion promoter emulsion is 28 g / m2 by wet weight. 2 Then, it is dried in an oven at a temperature of 125°C and a speed of 6.5 m / min to obtain a semi-finished base fabric.

[0084] S2. A layer of water-based silicone-based polyurethane slurry having a thickness of 0.14 mm was coated on the release paper and dried in an oven under the following conditions: a temperature of 130 ° C and a speed of 6.5 m / min to obtain a water-based polyurethane surface layer;

[0085] The water-based silicone-based polyurethane slurry is prepared from the following raw materials in parts by weight: 100 parts of water-based silicone-based polyurethane 1089R7, 4 parts of water-based curing agent SF-150, 1.8 parts of water-based leveling agent LA-91-120, 0.45 parts of defoamer 2459, 1.2 parts of water-based thickener U-506, and 10 parts of water-based color paste;

[0086] S3. A layer of waterborne polycarbonate polyurethane slurry having a thickness of 0.19 mm was coated on the waterborne polyurethane surface layer, and the waterborne polyurethane intermediate layer was obtained after drying in an oven. The drying conditions were: temperature 130 ° C, speed 6.5 m / min;

[0087] The water-based polycarbonate polyurethane slurry is prepared from the following raw materials in parts by weight: 100 parts of water-based polycarbonate polyurethane WF-73-575, 4 parts of water-based curing agent SF-150, 1.8 parts of water-based leveling agent LA-91-120, 0.5 parts of defoamer 2459, 1.2 parts of water-based thickener U-506, and 10 parts of water-based color paste;

[0088] S4. Coating a layer of 0.24 mm thick water-based two-component polyether polyurethane slurry on the surface of the water-based polyurethane intermediate layer, completely drying in a 90°C oven, laminating the semi-finished base fabric obtained in step S1, and continuing to put it into the oven for drying and aging. The drying and aging conditions are: temperature 157°C, vehicle speed 6.5m / min; then rolling it directly without peeling off the release paper, and then putting it in a 60°C aging chamber for aging for 60 hours. After the aging is completed, the release paper is peeled off to obtain a finished thin polyurethane composite material for consumer electronics;

[0089] Among them, the water-based two-component polyether polyurethane slurry is prepared from the following raw materials in parts by weight: 100 parts of water-based two-component polyether polyurethane 3355, 9 parts of water-based closed curing agent XR-22-903, 0.9 parts of water-based leveling agent LA-91-120, 0.3 parts of defoaming agent 2459, 1.2 parts of water-based thickener U-506, and 6 parts of water-based color paste.

[0090] The thin polyurethane composite material for consumer electronics prepared in this embodiment has a thickness of 0.245 mm (reference standard: GB / T 8949-2008); a gram weight of 210-225 g / m 2 (Reference standard: ASTM D751); Peel ≥ 60N / 3CM (Reference standard: GB / T8949-2008); Breaking strength ≥ 530N / 3CM (Reference standard: GB / T 8949-2008); Wear resistance: wet wool felt*1Kg*7000 times without breaking; 70℃*95%RH constant temperature and humidity test for 9 weeks without fogging; No powdering (Reference standard: QB / T 4671-2014).

[0091] Example 6

[0092] This embodiment provides a thin polyurethane composite material for consumer electronics, which is prepared by the following steps:

[0093] S1. A layer of adhesion promoter emulsion is applied by roller coating on the surface of glass fiber cloth with a thickness of 0.1 mm. The coating amount of adhesion promoter emulsion is 30 g / m2 by wet weight. 2 Then, it is dried in an oven at a temperature of 130°C and a speed of 6 m / min to obtain a semi-finished base fabric;

[0094] S2. A layer of water-based silicone-based polyurethane slurry having a thickness of 0.15 mm was coated on the release paper and dried in an oven under the following conditions: a temperature of 140°C and a speed of 6 m / min to obtain a water-based polyurethane surface layer;

[0095] The water-based silicone-based polyurethane slurry is prepared from the following raw materials in parts by weight: 100 parts of water-based silicone-based polyurethane 1089R7, 5 parts of water-based curing agent SF-150, 2 parts of water-based leveling agent LA-91-120, 0.5 parts of defoamer 2459, 2 parts of water-based thickener U-506, and 5 parts of water-based color paste;

[0096] S3. A layer of waterborne polycarbonate polyurethane slurry having a thickness of 0.2 mm was coated on the waterborne polyurethane surface layer, and the waterborne polyurethane intermediate layer was obtained after drying in an oven. The drying conditions were: temperature 140 ° C, speed 6 m / min;

[0097] The water-based polycarbonate polyurethane slurry is prepared from the following raw materials in parts by weight: 100 parts of water-based polycarbonate polyurethane WF-73-575, 5 parts of water-based curing agent SF-150, 2 parts of water-based leveling agent LA-91-120, 0.5 parts of defoamer 2459, 2 parts of water-based thickener U-506, and 5 parts of water-based color paste;

[0098] S4. Coat a layer of 0.25 mm thick water-based two-component polyether polyurethane slurry on the surface of the water-based polyurethane intermediate layer, dry it completely in an oven at 80°C, and then laminate it with the semi-finished base fabric obtained in step S1, and continue to put it into the oven for drying and aging. The drying and aging conditions are: temperature 160°C, vehicle speed 6m / min; then roll it directly without peeling off the release paper, and then put it in a 60°C aging room for 72 hours. After the aging is completed, peel off the release paper to obtain a finished thin polyurethane composite material for consumer electronics;

[0099] Among them, the water-based two-component polyether polyurethane slurry is prepared from the following raw materials in parts by weight: 100 parts of water-based two-component polyether polyurethane 3355, 10 parts of water-based closed curing agent XR-22-903, 1 part of water-based leveling agent LA-91-120, 0.4 parts of defoamer 2459, 2 parts of water-based thickener U-506, and 5 parts of water-based color paste.

[0100] The thin polyurethane composite material for consumer electronics prepared in this embodiment has a thickness of 0.25 mm (reference standard: GB / T8949-2008); a gram weight of 225-250 g / m 2 (Reference standard: ASTM D751), peeling ≥70N / 3CM (Reference standard: GB / T8949-2008); breaking strength ≥580N / 3CM (Reference standard: GB / T 8949-2008); wear resistance: wet wool felt*1Kg*8000 times without breaking; 70℃*95%RH constant temperature and humidity test for 10 weeks without fogging; no powdering (Reference standard: QB / T 4671-2014).

[0101] Comparative Example

[0102] This embodiment provides a thin polyurethane composite material for consumer electronics, which is prepared by the following steps:

[0103] S1. The glass fiber cloth having a thickness of 0.1 mm was baked in an oven under the following conditions: a temperature of 130°C and a speed of 6 m / min to obtain a semi-finished base fabric;

[0104] S2. A layer of water-based silicone-based polyurethane slurry having a thickness of 0.15 mm was coated on the release paper and dried in an oven under the following conditions: a temperature of 140°C and a speed of 6 m / min to obtain a water-based polyurethane surface layer;

[0105] The water-based silicone-based polyurethane slurry is prepared from the following raw materials in parts by weight: 100 parts of water-based silicone-based polyurethane 1089R7, 5 parts of water-based curing agent SF-150, 2 parts of water-based leveling agent LA-91-120, 0.5 parts of defoamer 2459, 2 parts of water-based thickener U-506, and 5 parts of water-based color paste;

[0106] S3. A layer of waterborne polycarbonate polyurethane slurry having a thickness of 0.2 mm was coated on the waterborne polyurethane surface layer, and the waterborne polyurethane intermediate layer was obtained after drying in an oven. The drying conditions were: temperature 140 ° C, speed 6 m / min;

[0107] The water-based polycarbonate polyurethane slurry is prepared from the following raw materials in parts by weight: 100 parts of water-based polycarbonate polyurethane WF-73-575, 5 parts of water-based curing agent SF-150, 2 parts of water-based leveling agent LA-91-120, 0.5 parts of defoamer 2459, 2 parts of water-based thickener U-506, and 5 parts of water-based color paste;

[0108] S4. Coat a layer of 0.25 mm thick water-based two-component polyether polyurethane slurry on the surface of the water-based polyurethane intermediate layer, dry it completely in an oven at 80°C, and then laminate it with the semi-finished base fabric obtained in step S1, and continue to put it into the oven for drying and aging. The drying and aging conditions are: temperature 160°C, vehicle speed 6m / min; then roll it directly without peeling off the release paper, and then put it in a 60°C aging room for 72 hours. After the aging is completed, peel off the release paper to obtain a finished thin polyurethane composite material for consumer electronics;

[0109] Among them, the water-based two-component polyether polyurethane slurry is prepared from the following raw materials in parts by weight: 100 parts of water-based two-component polyether polyurethane 3355, 10 parts of water-based closed curing agent XR-22-903, 1 part of water-based leveling agent LA-91-120, 0.4 parts of defoamer 2459, 2 parts of water-based thickener U-506, and 5 parts of water-based color paste.

[0110] The thin polyurethane composite material for consumer electronics prepared in this embodiment has a thickness of 0.25 mm (reference standard: GB / T8949-2008); a gram weight of 205-230 g / m 2 (Reference standard: ASTM D751), peeling ≥15N / 3CM (Reference standard: GB / T8949-2008); breaking strength ≥420N / 3CM (Reference standard: GB / T 8949-2008); wear resistance: wet wool felt*1Kg*2000 times without breaking; 70℃*95%RH constant temperature and humidity test for 3 weeks without fogging; no powdering (Reference standard: QB / T 4671-2014).

[0111] From the above test of Examples 1-6, increasing the thickness of the polyurethane coating, increasing the drying and aging time, increasing the amount of curing agent, and extending the aging time can improve the wear resistance, peeling, breaking strength and aging resistance of the product; from the comparative example, without applying the adhesion promoter emulsion, the polyurethane and the glass fiber cloth are not firmly combined, which has a significant impact on the peeling, wear resistance, breaking strength and aging resistance of the finished product. From the test data, the thickness of the product of Examples 1-6 can be 0.2-0.25mm, and the gram weight is 180-250g / m 2 The peeling strength is at least 40N / 3CM, the breaking strength is more than 400N / 3CM, the wet wool felt can be tested for more than 6000 times under a load of 1Kg without breaking, and the hydrolysis resistance can be tested at 70℃*95%RH constant temperature and humidity for at least 5 weeks without fogging or powdering. Overall, the product of the present invention is light, thin and durable, and its performance is far superior to ordinary consumer electronic decorative materials.

[0112] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0113] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A thin polyurethane composite material for consumer electronics, which comprises, from outside to inside, a waterborne polyurethane surface layer, a waterborne polyurethane intermediate layer, a waterborne polyurethane adhesive layer, and a base fabric layer, characterized in that: The base fabric layer is made of glass fiber cloth, and the side of the glass fiber cloth facing the waterborne polyurethane adhesive layer is coated with an adhesion promoter emulsion.

2. The thin polyurethane composite material for consumer electronics according to claim 1, characterized in that: The thickness of the glass fiber cloth is 0.08-0.1 mm.

3. The thin polyurethane composite material for consumer electronics according to claim 1, characterized in that: The waterborne polyurethane surface layer is made of waterborne silicon-based polyurethane slurry, and the waterborne silicon-based polyurethane slurry is prepared from the following components in parts by weight: 100 parts of waterborne silicon-based polyurethane slurry, 2-5 parts of waterborne curing agent, 0.5-2 parts of waterborne leveling agent, 0.1-0.5 parts of defoaming agent, 0.5-2 parts of waterborne thickener, and 5-20 parts of waterborne color paste.

4. The thin polyurethane composite material for consumer electronics according to claim 1, characterized in that: The waterborne polyurethane intermediate layer is made of waterborne polycarbon type polyurethane slurry, and the waterborne polycarbon type polyurethane slurry is prepared from the following components in parts by weight: 100 parts of waterborne polycarbon type polyurethane slurry, 2-5 parts of waterborne curing agent, 0.5-2 parts of waterborne leveling agent, 0.1-0.5 parts of defoaming agent, 0.5-2 parts of waterborne thickener, and 5-20 parts of waterborne color paste.

5. The thin polyurethane composite material for consumer electronics according to claim 1, characterized in that: The waterborne polyurethane adhesive layer is made of a waterborne two-component polyether polyurethane slurry, and the waterborne two-component polyether polyurethane slurry is prepared from the following components in parts by weight: 100 parts of waterborne two-component polyether polyurethane slurry, 5-10 parts of waterborne sealing curing agent, 0.5-1 part of waterborne leveling agent, 0.1-0.4 part of defoaming agent, 0.5-2 parts of waterborne thickener, and 5-10 parts of waterborne color paste.

6. A method for preparing a thin polyurethane composite material for consumer electronics as claimed in any one of claims 1 to 5, characterized in that: It includes the following steps: S1. Apply a layer of adhesion promoter emulsion on the surface of the glass fiber cloth and dry it to obtain a base cloth layer; S2. Coating a layer of waterborne polyurethane surface slurry on the release paper and drying the waterborne polyurethane surface layer; S3. Coating a layer of aqueous polyurethane intermediate layer slurry on the aqueous polyurethane surface layer and drying the aqueous polyurethane intermediate layer; S4. Coat a layer of water-based polyurethane adhesive layer slurry on the water-based polyurethane intermediate layer, completely dry the water-based polyurethane adhesive layer, laminate the water-based polyurethane adhesive layer to the base fabric layer, dry and mature the layer, roll it up, mature it in a 60° C. curing room for 12-72 hours, peel off the release paper, and obtain a thin polyurethane composite material for consumer electronics.

7. The method for preparing a thin polyurethane composite material for consumer electronics according to claim 6, characterized in that: In step S1, the coating amount of the adhesion promoter emulsion is 20-30 g / cm 2 The drying temperature is 100-130°C and the vehicle speed is 6-10m / min.

8. The method for preparing a thin polyurethane composite material for consumer electronics according to claim 6, characterized in that: In step S2, the coating thickness of the waterborne polyurethane surface slurry is 0.1-0.15 mm, the drying temperature is 90-140° C., and the vehicle speed is 6-10 m / min.

9. The method for preparing a thin polyurethane composite material for consumer electronics according to claim 6, characterized in that: In step S3, the coating thickness of the waterborne polyurethane intermediate layer slurry is 0.15-0.20 mm, the drying temperature is 90-140° C., and the vehicle speed is 6-10 m / min.

10. The method for preparing a thin polyurethane composite material for consumer electronics according to claim 6, characterized in that: In step S4, the coating thickness of the waterborne polyurethane adhesive layer slurry is 0.2-0.25 mm, the drying temperature is 80-110° C., the drying and aging temperature is 140-160° C., and the vehicle speed is 6-10 m / min.

Citation Information

Patent Citations

  • Polyurethane synthetic leather for regenerated fiber waterborne electronic products and preparation method of polyurethane synthetic leather

    CN113684693A

  • Base cloth for airbag, airbag composed of the same, and manufacturing method of the same

    JP2011168131A

  • Waterproof, weather-resistant and substantially non-stretching textile a method for producing it, and a component made from it

    US4619854A

  • Automobile interior PU leather suitable for glue spraying and coating and preparation method therefor

    WO2021136231A1