Rapid synthesis method of novel nanocrystalline apatite

Through electron beam radiation method and ultrasonic cleaning technology, the problems of uneven particle size distribution and cumbersome synthesis process of nanocrystalline apatite are solved, and the rapid synthesis of high-purity, defect-free nanocrystalline apatite is achieved, which is suitable for large-scale production And reduce production costs.

CN119059502APending Publication Date: 2024-12-03CHINA UNIV OF GEOSCIENCES (BEIJING) +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310648569.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-06-02
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The prior art has problems such as uneven particle size distribution, complicated synthesis process, long time, use of toxic solvents, and large energy consumption when preparing nanocrystalline apatite, making it difficult to achieve rapid high-purity, defect-free nanocrystalline apatite. synthesis.

Method used

The electron beam radiation method is used to control the electron beam energy, dose and irradiation time through pre-pulverization, grinding and irradiation steps, and the pH value is adjusted by ultrasonic cleaning and deionized water to achieve rapid synthesis of nanocrystalline apatite.

Benefits of technology

It realizes the rapid synthesis of nanocrystalline apatite with simple operation, green and environmental protection, dust-free, controllable particle size, high purity, and no impurities or defects, and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119059502A_ABST
    Figure CN119059502A_ABST
Patent Text Reader

Abstract

The invention provides a rapid synthesis method of novel nanocrystalline apatite, and relates to the field of preparation of radiation-sensitive nanocrystalline mineral materials. According to the method, apatite is placed in a vacuum environment of 10 <-3 > Pa-10 <-7 > Pa and an electron beam irradiation environment of 2.4 * 10 < 5 > ions / (nm < 2 >. S)-1.65 * 10 < 6 > ions / (nm < 2 >. S), local lattice collapse and atom disordering are caused by elastic collision and inelastic collision between electrons and target atoms in apatite crystal lattices, and the apatite is locally crystallized after being completely amorphized, so that the phosphorite is obtained. And obtaining the amorphous matrix wrapping the nanocrystalline apatite under continuous irradiation of electron beams. And putting the powder into a solution with the pH value of 8-10.5 to eliminate the amorphous matrix, thereby obtaining the nanocrystalline apatite with the particle size of 5-10nm. The synthesis speed and the particle size of the nanocrystalline apatite can be regulated and controlled by changing the acceleration voltage and the injection dosage of the electron beam and the irradiation time of the electron beam. The method can simplify the synthesis steps of the nanocrystalline apatite, is green and environment-friendly, and has a wide application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a novel rapid synthesis method of nanocrystalline apatite, and belongs to the field of preparation of radiation-sensitive nanocrystalline mineral materials. Background Art

[0002] Apatite is a typical mineral salt with the chemical formula of Ca 10 (PO4)6(OH)2 is the main component of human and animal bones and teeth, and does not contain any harmful elements to the human body. The 4f and 6h sites in the apatite lattice have a wide range of tolerance for metal cations of different radii. In addition, the OH in the anion channel parallel to the c axis - It is also easily replaced by other halogen atoms. Therefore, it has good stability, physical and chemical activity, biocompatibility and excellent ion exchange performance. However, many problems are exposed in actual applications. Nanocrystalline apatite is widely used in the biomedical field for bone repair and regeneration, environmental protection field for purification of heavy metal ions and organic pollutants in wastewater, nanoelectronics field for the preparation of field effect transistors and photodiodes, energy field for the preparation of high-performance solar cells and fuel cells, and nanocrystalline apatite is also used in cosmetics, food industry, automobile industry, textile industry, building materials and other industries. Therefore, there is an urgent need for nanocrystalline apatite with many conditions such as adjustable shape, uniform composition, concentrated particle size distribution, large specific surface area, fine particles, no agglomeration and excellent biological performance.

[0003] At present, the methods for preparing nanocrystalline apatite mainly include wet method - hydrothermal method, precipitation method, sol-gel method, microemulsion method, ultrasonic synthesis method, etc. and dry method - solid-state reaction method. The apatite particles prepared by the chemical precipitation method have a wide distribution range of particle sizes, low particle dispersion, and are very easy to generate crystal defects. The particle size of the synthetic apatite is between 33nm and 80nm; the sol-gel method takes a long time to synthesize, and toxic organic solvents are volatilized during the synthesis process; the ion diffusion in the solid-state synthesis method is small, resulting in uneven composition; the mechanical ball milling method has a high sintering temperature, and the grinding process consumes a lot of energy, and the particle size of the synthetic apatite is above 100nm; although the particle size distribution range prepared by the microemulsion method is narrow, it is necessary to remove the oil phase and surfactant on the surface of the particles, and the particle size of the synthetic apatite is about 107nm; the template size in the template method is limited, so it is difficult to achieve large-scale production; the hydrolysis method uses calcium salt and calcium chloride to hydrolyze to synthesize micron-level apatite; the apatite particles prepared by the chemical precipitation method have a wide distribution range of particle sizes, low particle dispersion, and the particle size of the synthetic apatite is between 33nm and 80nm. The above methods have a long implementation period and a complicated synthesis process. In addition, the particle sizes synthesized by hydrothermal and precipitation methods are mostly concentrated in the range of 10nm to 400nm, and the particle size distribution varies greatly. In order to solve the above problems, we invented a new method for rapid synthesis of nanocrystalline apatite, and achieved the synthesis of nanocrystalline apatite with different particle sizes by controlling the energy, dose and irradiation time of the electron beam during the experiment. Summary of the invention

[0004] The purpose of the present invention is to provide a novel rapid synthesis method of nanocrystalline apatite. The method is simple to operate and has a green and environmentally friendly operation process. The block apatite is used as a raw material, and nanocrystalline apatite with different particle sizes is prepared by different energies, electron beam injection doses, and different irradiation times.

[0005] To achieve the above object, the present invention adopts the following technical scheme, a novel method for rapid synthesis of nanocrystalline apatite, comprising the following steps:

[0006] (1) Pre-crushing: Put apatite blocks with a maximum size of 25 cm to 120 cm into a rock crusher for crushing to obtain apatite particles of 10 mm to 30 mm;

[0007] (2) Grinding: Add the pre-crushed apatite particles into a planetary ball mill, select small steel balls with a diameter of 4 mm to 8 mm and large steel balls with a diameter of 10 mm to 16 mm for ball milling, and obtain apatite ultrafine powder with a particle size of 10 μm to 100 μm, wherein the ball mill speed is 100 to 300 revolutions per minute, and the ball milling is performed for 8 h to 12 h;

[0008] (3) Irradiation: Place the ultrafine apatite powder in a heat-conductive non-conductive cavity equipped with a field emission electron gun, connect the water cooling block of an open liquid cooling system, and keep the cavity temperature constant at 20°C to 30°C; at the same time, use a vacuum pump to evacuate the cavity to keep the vacuum degree at 10 -3 Pa~10 -7 Pa; the ultrafine apatite powder is spread in the cavity, and the energy is 200KeV to 700KeV, 2.4x10 5 ions / (nm 2 s)~1.65x10 6 ions / (nm 2 ·s) for 30 min to 1 h to obtain amorphous apatite particles wrapped with nanocrystalline apatite;

[0009] (4) Synthesis: The irradiated apatite powder was placed in 50 mL of deionized water and placed in an ultrasonic cleaning machine. The pH was adjusted to 8 to 10.5 using 1 mol / L dilute nitric acid and 0.5 mol / L sodium hydroxide solution. The ultrasonic cleaning machine was adjusted to a temperature of 20°C to 60°C and a power of 60 kW to 120 kW and vibrated for 30 to 60 minutes before drying to obtain nanocrystalline apatite with a particle size of 5 nm to 10 nm.

[0010] Compared with the prior art, the present invention has the following beneficial effects:

[0011] (1) Compared with other chemical methods, the electron beam radiation synthesis method is simple to operate and does not require the addition of complicated chemical reagents. In addition, the apatite raw material is widely available and suitable for large-scale production, and the synthesis time is greatly shortened.

[0012] (2) By adjusting the electron beam energy, implantation dose, and irradiation time, the size of nanocrystalline apatite can be reduced to 5-10 nm;

[0013] (3) The synthesis process is green, environmentally friendly and dust-free. The prepared nanocrystalline apatite is of high purity, free of impurities or defects. Compared with other preparation methods, the process is relatively simple. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 TEM and FFT of apatite before electron beam irradiation in a specific embodiment.

[0015] Figure 2 In a specific embodiment, 300KeV, 2.4x10 5 ions / (nm 2 ·s) TEM of apatite nanocrystals produced by electron beam irradiation for 30 min (the yellow dashed line indicates the location of the nanocrystals).

[0016] Figure 3In a specific embodiment, 300KeV, 4.9x10 5 ions / (nm 2 ·s) TEM of apatite nanocrystals produced by electron beam irradiation for 30 min (the yellow dashed line indicates the location of the nanocrystals).

[0017] Figure 4 In a specific embodiment, 300KeV, 9.8x10 5 ions / (nm 2 ·s), and TEM of apatite nanocrystals was produced by electron beam irradiation for 30 min (the yellow dashed line indicates the position of the nanocrystals).

[0018] Figure 5 In a specific embodiment, 300KeV, 1.65x10 6 ions / (nm 2 ·s) TEM of apatite nanocrystals produced by electron beam irradiation for 30 min (the yellow dashed line indicates the location of the nanocrystals). DETAILED DESCRIPTION

[0019] In order to better illustrate the present invention, typical but non-limiting embodiments of the present invention are as follows:

[0020] Example 1

[0021] (1) using a jaw crusher with a rotor size of Φ1000 mm x 700 mm at 600 kW for pre-crushing to obtain apatite particles with an average particle size of 28.9 mm;

[0022] (2) 100 g of apatite particles were added to a planetary ball mill, 40 large steel balls with a diameter of 10 mm and 280 small steel balls with a diameter of 6 mm were added, and after ball milling for 12 h, ultrafine apatite powder with an average particle size of 27 μm was obtained;

[0023] (3) Place 10 g of apatite nanopowder in a vacuum chamber at 10 -6 Pa, in a constant temperature alumina chamber equipped with a field emission electron gun, 300KeV, 2.4x10 5 ions / (nm 2 ·s) electron beam is injected into apatite nanopowder, and after 30 minutes, an amorphous apatite matrix wrapped with nanocrystalline apatite is obtained;

[0024] (4) The irradiated apatite powder was placed in 50 mL of deionized water and placed in an ultrasonic cleaning machine. The pH was adjusted to 8 using 1 mol / L dilute nitric acid and 0.5 mol / L sodium hydroxide solution. The ultrasonic cleaning machine was adjusted to a temperature of 40° C. and a power of 60 kW. The powder was vibrated for 40 minutes and then dried to obtain nanocrystalline apatite with an average particle size of 4.98 nm.

[0025] Example 2

[0026] (1) using a jaw crusher with a rotor size of Φ1000 mm x 700 mm at 700 kW for pre-crushing to obtain apatite particles with an average particle size of 24.1 mm;

[0027] (2) 100 g of apatite particles were added to a planetary ball mill, 40 large steel balls with a diameter of 10 mm and 280 small steel balls with a diameter of 6 mm were added, and after ball milling for 12 h, an apatite ultrafine powder with an average particle size of 26.4 μm was obtained;

[0028] (3) Place 10 g of apatite nanopowder in a vacuum chamber at 10 -6 Pa, in a constant temperature alumina chamber equipped with a field emission electron gun, 300KeV, 4.9x10 5 ions / (nm 2 ·s) electron beam was injected into apatite nanopowder, and after 30 minutes, nanocrystalline apatite with an average particle size of 29nm was obtained;

[0029] (4) The irradiated apatite powder was placed in 50 mL of deionized water and placed in an ultrasonic cleaning machine. The pH was adjusted to 8 using 1 mol / L dilute nitric acid and 0.5 mol / L sodium hydroxide solution. The ultrasonic cleaning machine was adjusted to a temperature of 40° C. and a power of 60 kW. The powder was vibrated for 40 minutes and then dried to obtain nanocrystalline apatite with an average particle size of 3.72 nm.

[0030] Example 3

[0031] (1) using a jaw crusher with a rotor size of Φ1000 mm x 700 mm at 800 kW for pre-crushing to obtain apatite particles with an average particle size of 18.4 mm;

[0032] (2) 100 g of apatite particles were added to a planetary ball mill, 40 large steel balls with a diameter of 10 mm and 280 small steel balls with a diameter of 6 mm were added, and after ball milling for 12 h, an apatite ultrafine powder with an average particle size of 27.5 μm was obtained;

[0033] (3) Place 10 g of apatite nanopowder in a vacuum chamber at 10 -6 Pa, in a constant temperature alumina chamber equipped with a field emission electron gun, 300KeV, 9.8x10 5 ions / (nm 2 ·s) electron beam was injected into apatite nanopowder, and after 30 minutes, nanocrystalline apatite with an average particle size of 17nm was obtained;

[0034] (4) The irradiated apatite powder was placed in 50 mL of deionized water and placed in an ultrasonic cleaning machine. The pH was adjusted to 8 using 1 mol / L dilute nitric acid and 0.5 mol / L sodium hydroxide solution. The ultrasonic cleaning machine was adjusted to a temperature of 40° C. and a power of 60 kW. The powder was vibrated for 40 minutes and then dried to obtain nanocrystalline apatite with an average particle size of 4.4 nm.

[0035] Example 4

[0036] (1) using a jaw crusher with a rotor size of Φ1000 mm x 700 mm at 900 kW for pre-crushing to obtain apatite particles with an average particle size of 15.5 mm;

[0037] (2) 100 g of apatite particles were added to a planetary ball mill, 40 large steel balls with a diameter of 10 mm and 280 small steel balls with a diameter of 6 mm were added, and after ball milling for 12 h, an apatite ultrafine powder with an average particle size of 23.1 μm was obtained;

[0038] (3) Place 10 g of apatite nanopowder in a vacuum chamber at 10 -6 Pa, in a constant temperature alumina chamber equipped with a field emission electron gun, 300KeV, 1.65x10 6 ions / (nm 2 ·s) electron beam was injected into apatite nanopowder, and after 30 minutes, nanocrystalline apatite with an average particle size of 9nm was obtained;

[0039] (4) The irradiated apatite powder was placed in 50 mL of deionized water and placed in an ultrasonic cleaning machine. The pH was adjusted to 8 using 1 mol / L dilute nitric acid and 0.5 mol / L sodium hydroxide solution. The ultrasonic cleaning machine was adjusted to a temperature of 40° C. and a power of 60 kW. The powder was vibrated for 40 minutes and then dried to obtain nanocrystalline apatite with an average particle size of 4.15 nm.

Claims

1. A novel method for rapid synthesis of nanocrystalline apatite, characterized in that Place apatite at 10 -3 Pa~10 -7 Pa vacuum and 2.4x10 5 ions / (nm 2 s)~1.65x10 6 ions / (nm 2 ·s) electron beam irradiation environment, to obtain nanocrystalline apatite with a particle size of 5nm to 10nm, the preparation method is as follows: (1) placing apatite blocks with a maximum size of 25 cm to 120 cm in a rock crusher for pre-crushing to obtain apatite particles with a particle size of 10 mm to 30 mm; (2) placing the pre-crushed apatite particles into a planetary ball mill for ball milling to obtain apatite ultrafine powder with a particle size of 10 μm to 30 μm; (3) Spreading the ultrafine apatite powder into a cavity in a vacuum environment and connecting it to an open liquid cooling system to keep the cavity temperature at 20°C to 30°C; (4) The electron gun emits a high-energy electron beam and injects it into the ultrafine apatite powder. After 30 minutes to 1 hour, an amorphous apatite matrix wrapped with nanocrystalline apatite can be obtained; (5) The powder is placed in a beaker filled with deionized water, the pH value and temperature are adjusted, and the powder is placed in an ultrasonic cleaning machine for vibration for 30 to 60 minutes and then dried to obtain nanocrystalline apatite with a particle size of 5 to 10 nm.

2. The preparation method according to claim 1, characterized in that: The apatite may be but is not limited to Ca 10 (PO4)6F2、Ba 10 (VO4)6Cl2、Pb 10 (AsO4)6(OH)2Apatite structure type inorganic compound.

3. The preparation method according to claim 1, characterized in that: The vacuum degree in the cavity is 10 -3 Pa~10 -7 Pa.

4. The preparation method according to claim 1, characterized in that: The electron gun is a field emission electron gun, the energy of the high-energy electron beam is 200KeV~700KeV, and the injection dose is 2.4x10 5 ions / (nm 2 s)~1.65x10 6 ions / (nm 2 ·s).

5. The preparation method according to claim 1, characterized in that: The cavity bottom material in contact with the apatite powder is but not limited to high temperature alloys such as nickel / cobalt / iron-based alloys, ceramic materials such as silicon carbide, and metal elements with good thermal and electrical conductivity such as copper.

6. The preparation method according to claim 1, characterized in that: The method can controllably prepare the particle size of nanocrystalline apatite by changing the electron beam energy, the injection dose and the irradiation time.

7. The preparation method according to claim 1, characterized in that: The pH value of the apatite suspension in the beaker is adjusted to 8-10.5, the temperature in the ultrasonic cleaning machine is adjusted to 20-60° C., and the power is adjusted to 60KW-120KW.