Copper-based perovskite Cs5Cu3X8 film prepared by solution method and photoelectric device
The development of copper-based perovskite Cs5Cu3X8 thin films using a one-step spin coating process addresses the limitations of lead-based halides, enabling high-performance ultraviolet detectors and LEDs with improved responsiveness and stability.
Patent Information
- Application Number
- CN202310649689.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-02
- Publication Date
- 2024-12-03
AI Technical Summary
Existing photodetectors and light-emitting diodes face challenges such as complex preparation processes, high costs, difficulty in forming large-area flexible devices, and the toxicity and instability of lead-based halides, limiting their practical application and performance.
A solution method is developed to prepare high-quality copper-based perovskite Cs5Cu3X8 (X=Cl, Br, I) thin films using a one-step spin coating process, which forms pure phase films with a feather-like morphology, suitable for photovoltaic, photoconductive, and light-emitting devices, avoiding lead and other impurities.
The method results in high-performance ultraviolet detectors and LEDs with improved responsiveness, sensitivity, and stability, featuring high PLQE, wide bandgap, and environmental friendliness, suitable for flexible devices.
Smart Images

Figure CN119059551A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical fields of inorganic metal halide materials and image sensing, military surveillance, weather monitoring, information communication, optical display, etc., and specifically to a high-quality copper-based perovskite Cs5Cu3X8 (X=Cl, Br, I) film and a photoelectric device prepared by a solution method. Background Art
[0002] Photodetectors are a type of photoelectric device that can convert photogenerated carriers into electrons and collect them through electrodes to form current. They can be widely used in image sensing, optical measurement, missile guidance, night vision systems, machine vision and other fields, and have great application prospects and scientific research value. At present, commercial ultraviolet photodetectors are mainly vacuum ultraviolet detectors represented by photomultiplier tubes, silicon-based ultraviolet enhanced detectors and wide-bandgap inorganic semiconductor detectors. Although they have mature technical processes, they still have complex preparation processes, high preparation temperatures, difficulty in preparing large-area flexible devices, high costs, high driving voltages, and the need to add expensive filters, which limit the practical application of detectors. In contrast, detectors made of organic materials can be processed by solution, are easy to form films, and can be prepared at low temperature and low cost on a large area. However, the inherent low carrier mobility, poor transmission performance and narrow absorption spectrum of organic materials limit the development of photodetectors.
[0003] Light-emitting diodes (LEDs) are a type of optoelectronic device that can convert electrical energy into light energy by releasing energy through electron-hole recombination. They have been widely used in displays and lighting, and play an indispensable role in human life. Currently, the commercial preparation process of light-emitting diodes (LEDs) is complex and costly, and it is difficult to achieve high-resolution single-pixel imaging and flexible devices.
[0004] As an emerging semiconductor material, perovskite material (ABX3) has the advantages of being a direct bandgap material with adjustable bandgap, high carrier mobility, long carrier diffusion length, high absorption coefficient, absorption band that can cover the ultraviolet to near-infrared band, and relatively balanced electron and hole transport performance. In addition, the raw materials of perovskite are abundant and easy to obtain, low-priced, and can be prepared into optoelectronic devices at low cost and large area through a simple and mild solution preparation process, which has attracted extensive attention from researchers in the field of optoelectronic devices. The use of perovskite, an emerging material, in photodetectors, especially ultraviolet detection and light-emitting diodes (LEDs), is of great significance for the development of high-performance optoelectronic devices and practical applications. At present, although traditional perovskite materials have been proven to be able to prepare photodetectors and LEDs, the toxicity of lead-based halides and the instability of tin-based halides are very unfavorable to their commercialization, especially because the optical bandgap of such materials is wide, and the prepared detectors are not truly blind visible light type. Therefore, it is particularly important to find stable and environmentally friendly lead-free perovskites to prepare photodetectors and LEDs.
[0005] The lead-free copper-based halide Cs5Cu3X8 (X=Cl, Br, I) is a novel wide-bandgap semiconductor material with a bandgap width of about 3.81eV. It only has absorption in the ultraviolet region before 340nm, making it an ideal intrinsic material for preparing ultraviolet detection. At the same time, the material has a very high PLQE and has great research potential in LEDs. Moreover, the material is environmentally friendly and non-toxic, the synthesis method is simple, it can be solution-processed, and it has excellent stability. Therefore, the development of ultraviolet photodetectors and LEDs based on Cs5Cu3X8 (X=Cl, Br, I) perovskite films is of great significance. However, since CsCl, one of the raw materials for synthesizing Cs5Cu3X8 (X=Cl, Br, I) reported so far, has low solubility in conventional non-polar solvents, the preparation methods of Cs5Cu3X8 (X=Cl, Br, I) mainly use high-temperature sintering and grinding methods to prepare X-Ray scintillator thin films. Such methods have complex preparation processes, high preparation temperatures, high preparation costs, and the inevitable presence of monomer impurities such as CsCl in the product, leading to problems such as impure material phases and poor device performance. Therefore, the solution method for preparing Cs5Cu3X8 (X=Cl, Br, I) crystals and thin films is currently a top priority for the application research of this material. Summary of the invention
[0006] The present invention aims at the insufficiency of existing perovskite materials in realizing detection in the ultraviolet region and the toxicity and instability of lead-based perovskite detectors and light-emitting diodes (LEDs), and provides a solution method for preparing high-quality copper-based perovskite Cs5Cu3X8 (X=Cl, Br, I) thin films and photoelectric devices. The preparation method of the present invention is simple, does not contain lead elements, and obtains a precursor solution with uniform components and accurate proportions through a reasonable preparation process, thereby obtaining a high-quality Cs5Cu3X8 (X=Cl, Br, I) pure phase thin film, and can obtain high-performance photovoltaic, photoconductive ultraviolet photoelectric detection electrical appliances and light-emitting diodes (LEDs).
[0007] In order to achieve the above-mentioned invention object, the following technical scheme is adopted:
[0008] A copper-based perovskite Cs5Cu3X8 film prepared by a solution method, the perovskite Cs5Cu3X8 film is composed of feather-shaped grains with a diameter of 30nm to 3μm, wherein the ratio of three elements Cs:Cu:X is 5:3:8, X is Cl, Br or I, and the film is a pure phase perovskite Cs5Cu3X8 film with a thickness of 50nm to 1μm.
[0009] The preferred diameter of the feather-shaped grains is 500 nm to 1 μm.
[0010] The preferred film thickness is 50 nm to 500 nm.
[0011] The method for preparing the copper-based perovskite Cs5Cu3X8 film comprises the following steps:
[0012] The precursor solution is applied to the substrate, and a wet film is obtained by a one-step spin coating method or a one-step spin coating method combined with anti-solvent washing, and the wet film is heated and annealed to obtain the wet film; wherein the precursor solution is a mixture of two or more of cesium chloride, cesium bromide, cesium iodide, cuprous chloride, cuprous bromide and cuprous iodide as raw materials, and is fully dissolved in a solvent. Preferably, the molar ratio of cesium chloride, cesium iodide and cuprous iodide is 2:3:3; the molar ratio of cesium chloride: cuprous chloride: cuprous bromide is 5:1:2; the molar ratio of cesium bromide, cuprous bromide and cuprous chloride is 2:3:3; the molar ratio of cesium bromide: cuprous bromide and cuprous iodide is 5:2:1; the molar ratio of cesium iodide, cuprous iodide and cuprous bromide is 5:2:1; the molar ratio of cesium bromide, cesium iodide and cuprous iodide is 2:3:3. The solvent is a mixed solvent of formamide and dimethyl sulfoxide in a volume ratio of 1-10:1-10, preferably formamide and dimethyl sulfoxide in a volume ratio of 1-3:1-3, and more preferably formamide and dimethyl sulfoxide in a volume ratio of 1:3. The mass fraction of the solute in the solvent is 5%-35%.
[0013] X includes Cl - Br - ,I -The three atomic numbers can be combined or matched in any ratio of X:8-X, for example: Cs5Cu3I (a) Cl (8-a) 、Cs5Cu3Br (a) Cl (8-a) 、Cs5Cu3I (a) Br (8-a) etc., where a can be any value between 0.001 and 7.999.
[0014] The above one-step spin coating method combined with anti-solvent rinsing can further assist crystallization.
[0015] The copper-based perovskite Cs5Cu3X8 film obtained by the method of the present invention is a pure phase of Cs5Cu3X8, without impurities of raw materials and other substances.
[0016] The substrate is a conductive layer or an insulating substrate; wherein the conductive layer is GaN, Ga2O3, PEDOT:PSS, TmPyPB or ITO, and the insulating substrate is quartz or a flexible insulating substrate.
[0017] The wet film preparation process adopts a one-step spin coating method, the spin coating speed is 999 to 9999 rpm, and the spin coating time is 10 to 70 seconds.
[0018] The anti-solvent used in the wet film preparation process is petroleum ether, hexane, heptane, chloropropane, ethyl bromide, nitromethane, dichloroethane, chloroform, n-pentane, carbon tetrachloride, carbon disulfide, benzene, toluene, xylene, benzene bromide, phenol, ethyl ether, isopropyl ether, ethyl acetate, butyl acetate, methyl propionate, propyl propionate, ethanol, methyl ethyl alcohol, n-butanol, tert-butanol, tetrahydrofuran, dioxane or acetone; the volume ratio of the anti-solvent to the precursor solution is 1:1 to 1:10.
[0019] The heating annealing is to anneal the wet film on a hot stage at 60° C. to 180° C. for 2 min to 60 min.
[0020] The above spin coating is preferably performed at room temperature.
[0021] The photoelectric device prepared by using the above film is a photovoltaic ultraviolet photodetector, a photoconductive ultraviolet photodetector or a light emitting diode.
[0022] The photoelectric device prepared by using the above-mentioned film is prepared by the following method:
[0023] At room temperature, cesium chloride, cesium bromide, cesium iodide, cuprous chloride, cuprous bromide and a mixture of two or more cuprous iodide are used as raw materials, and stirred and dissolved in a solvent to obtain a Cs5Cu3X8 (X=Cl, Br, I) precursor solution; the substrate is cleaned; the completely dissolved precursor solution is dropped on the substrate, and a wet film is prepared by one-step spin coating or one-step spin coating combined with an anti-solvent assisted crystallization method; the wet film is placed on a hot stage for heating and annealing to promote crystallization, and a Cs5Cu3X8 (X=Cl, Br, I) perovskite film layer is obtained; the film is coated on an electron transport layer substrate, and a layer of electrode is added on the surface of the perovskite film layer and the electron transport layer to obtain a photovoltaic ultraviolet photodetector;
[0024] Or the film is directly coated onto the patterned interdigitated electrodes to obtain a photoconductive UV photodetector;
[0025] Or a hole transport layer is coated on the surface of the substrate, and then a Cs5Cu3X8 (X = Cl, Br, I) perovskite film is coated on the upper surface of the hole transport layer as a light-emitting layer, and then an electron transport layer is prepared on the light-emitting layer by evaporation or spin coating, and finally a metal electrode is added to the surface of the electron transport layer to obtain a photoelectric device.
[0026] The preparation method of the photovoltaic ultraviolet photodetector specifically comprises the following steps:
[0027] (1) Cleaning the substrate;
[0028] (2) obtaining an electron transport layer by epitaxial growth;
[0029] (3) at room temperature, cesium chloride, cesium bromide, cesium iodide, cuprous chloride, cuprous bromide and a mixture of two or more cuprous iodide are used as raw materials and fully dissolved in a solvent to obtain a Cs5Cu3X8 precursor solution, wherein X = Cl, Br, I;
[0030] (4) dropping a fully dissolved precursor solution onto the electron transport layer, and forming a wet film by one-step spin coating or one-step spin coating combined with anti-solvent washing; placing the wet film on a hot stage for heating and annealing to obtain a Cs5Cu3X8 perovskite thin film layer, wherein X = Cl, Br, I; and adding a layer of electrode on the surface of the perovskite thin film layer and the electron transport layer to obtain a photovoltaic ultraviolet photodetector.
[0031] The preparation method of the above-mentioned photoconductive ultraviolet photodetector specifically comprises the following steps:
[0032] (1) Cleaning the substrate;
[0033] (2) preparing patterned interdigitated electrodes;
[0034] (3) at room temperature, cesium chloride, cesium bromide, cesium iodide, cuprous chloride, cuprous bromide and a mixture of two or more cuprous iodide are used as raw materials and fully dissolved in a solvent to obtain a Cs5Cu3X8 precursor solution, wherein X = Cl, Br, I;
[0035] (4) dropping a fully dissolved precursor solution onto the interdigital electrodes, and forming a wet film by one-step spin coating or one-step spin coating combined with anti-solvent washing; placing the wet film on a hot stage for heating and annealing, and cooling to obtain a photoconductive ultraviolet photodetector.
[0036] The method for preparing the light emitting diode specifically comprises the following steps:
[0037] (1) Cleaning the substrate;
[0038] (2) coating a hole transport layer on the substrate surface;
[0039] (3) at room temperature, cesium chloride, cesium bromide, cesium iodide, cuprous chloride, cuprous bromide and a mixture of two or more cuprous iodide are used as raw materials and fully dissolved in a solvent to obtain a Cs5Cu3X8 precursor solution, wherein X = Cl, Br, I;
[0040] (4) dropping a fully dissolved precursor solution onto the hole transport layer, and forming a wet film by one-step spin coating or one-step spin coating combined with anti-solvent washing; placing the wet film on a hot stage for heating and annealing to obtain a light-emitting layer; then preparing an electron transport layer on the light-emitting layer by evaporation or spin coating, and finally adding a metal electrode on the surface of the electron transport layer to obtain a light-emitting diode.
[0041] The above-mentioned electrodes are formed by uniformly coating one or more conductive metals with matching energy levels such as Au, Ag, Cu, Cr, In, Al, LiF, etc. on the surface of the perovskite thin film layer and the electron transport layer as anode and cathode respectively through one or more methods such as vacuum coating and magnetron sputtering, with a thickness of 15nm to 900nm.
[0042] The above-mentioned photovoltaic ultraviolet photodetector is preferably covered with a layer of Cs5Cu3X8 (X=Cl, Br, I) polycrystalline film on the epitaxially grown n-GaN and β-Ga2O3, and the Cs5Cu3X8 (X=Cl, Br, I) polycrystalline film forms a pn heterojunction with n-GaN and β-Ga2O3, thereby constituting a photovoltaic ultraviolet photodetector with a self-driving effect.
[0043] The photoconductive ultraviolet photodetector is preferably obtained by directly coating a Cs5Cu3X8 (X=Cl, Br, I) polycrystalline thin film on a patterned interdigitated electrode of an insulating or flexible substrate.
[0044] The light-emitting diode (LED) is preferably prepared by first preparing a hole transport layer on ITO or FTO conductive glass, covering it with a Cs5Cu3X8 (X=Cl, Br, I) polycrystalline thin film as a light-emitting layer, and then preparing an electron transport layer on the film, and finally adding a metal on the surface of the electron transport layer to obtain a light-emitting diode (LED) based on the Cs5Cu3X8 (X=Cl, Br, I) polycrystalline thin film.
[0045] Compared with the prior art, the present invention has the following advantages:
[0046] 1. The film preparation process uses a simple one-step spin coating solution treatment, which does not require complex material synthesis technology and can form a good polycrystalline film. The film has a special tight and continuous feather-like morphology, and the film is a pure phase of Cs5Cu3X8, without raw materials and other material impurities. Its absorption cutoff is before 340nm, there is no absorption of visible light, high PLQY (98%), high fluorescence quantum lifetime (60.2μs), and no self-absorption. It can effectively reduce the dark current of the device, realize the detection of weaker ultraviolet light, and can effectively reduce the probability of non-radiative recombination to prepare high-performance light-emitting diodes (LEDs).
[0047] 2 The optoelectronic device of the present invention uses Cs5Cu3X8 (X = Cl, Br, I) as a semiconductor material. Compared with lead-based and tin-based perovskites, this material is more novel and stable, and has a higher PLQE, a lower defect state density and good carrier transport capacity. The film has a wide intrinsic band gap and no absorption of visible light, and can achieve blind visible light type ultraviolet detection, thereby showing good responsiveness and sensitivity in the ultraviolet region.
[0048] 3. The photovoltaic ultraviolet photodetector of the present invention can increase the carrier transmission speed while maintaining a high photocurrent, thereby improving the device responsiveness. Thanks to the good carrier transmission capability of the film, the device response time is also greatly shortened.
[0049] 4. The photoconductive ultraviolet photodetector of the present invention can improve the device's responsiveness and external quantum efficiency, and can be applied to flexible devices.
[0050] 5. The light-emitting diode (LED) of the present invention benefits from the high-quality, high-PLQE Cs5Cu3X8 (X=Cl, Br, I) thin film, which has high brightness and external quantum efficiency optimization potential, while meeting potential commercialization requirements such as environmental friendliness and good stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0051] Figure 1 This is a schematic diagram of a photovoltaic ultraviolet photodetector device based on Cs5Cu3I2Cl6 thin film according to an embodiment of the present invention;
[0052] Figure 2 This is a schematic diagram of a Cs5Cu3I2Cl6 thin film photoconductive ultraviolet photodetector device according to an embodiment of the present invention;
[0053] Figure 3 This is a schematic diagram of a Cs5Cu3I2Cl6 thin film light emitting diode (LED) device according to an embodiment of the present invention;
[0054] Figure 4 This is the XRD spectrum of the thin film on the gallium nitride substrate prepared in Example 1. It can be seen from the figure that the thin film directly prepared by the low-temperature solution and one-step spin coating method has good crystal orientation, does not exist any impurity peaks, and can perfectly correspond to the Cs5Cu3I2Cl6 standard card, belonging to the orthorhombic phase structure, demonstrating the good crystallinity of the thin film prepared by this method.
[0055] Figure 5 This is the XRD spectrum of the thin film on the quartz substrate prepared in Example 2, and its characteristics are the same as those in Example 1.
[0056] Figure 6 This is the XRD spectrum of the ITO film on the conductive glass prepared in Example 3, and its characteristics are the same as those in Example 1.
[0057] Figure 7 From the XPS spectrum of the Cs5Cu3I2Cl6 film prepared in Example 1-3, it can be seen that the film is mainly composed of four elements: Cs, Cu, I, and Cl, and the semi-quantitative atomic ratio is Cs:Cu:I:Cl=5.2:3.1:1.9:5.8, which is consistent with the stoichiometric ratio of Cs5Cu3I2Cl6.
[0058] Figure 8 This is a planar SEM image of the Cs5Cu3I2Cl6 film on the gallium nitride substrate prepared in Example 1. It can be seen that the film has good coverage and flatness at low magnification, and the film at high magnification is composed of feather-like grains with a diameter of about 1 μm without obvious defects.
[0059] Fig. 9 This is a planar SEM image of the Cs5Cu3I2Cl6 film on a quartz substrate prepared in Example 2. The characteristics are the same as those in Example 1. The film is composed of feather-like grains with a diameter of about 500 nm and has no obvious defects.
[0060] Fig.10 This is a planar SEM image of the Cs5Cu3I2Cl6 film on the ITO conductive glass prepared in Example 3. The characteristics are the same as those in Example 1. The film is composed of feather-like grains with a diameter of about 500 nm and has no obvious defects.
[0061] Fig.11This is a planar AFM image of the Cs5Cu3I2Cl6 film on the gallium nitride substrate prepared in Example 1. It can be seen that the roughness of the film is about 2nm, which is conducive to the interlayer contact of the vertical structure, effectively reducing the dark current, improving the response speed and the extraction of photocurrent.
[0062] Fig.12 This is a planar AFM image of the Cs5Cu3I2Cl6 thin film on the quartz substrate prepared in Example 2.
[0063] Fig.13 This is a planar AFM image of the Cs5Cu3I2Cl6 film on the ITO conductive glass prepared in Example 3.
[0064] Fig.14 This is the optical characterization spectrum of the Cs5Cu3I2Cl6 film prepared in Example 1. Fig.14 It can be seen from A that the absorption spectrum of the film drops significantly at 325nm and the absorption is cut off at around 340nm. Fig.14 The film in B exhibits 462nm blue light emission under ultraviolet excitation, representing the Stokes shift common in low-dimensional perovskites, and the PLE spectrum is basically consistent with the absorption spectrum, demonstrating the good optical properties and potential ultraviolet detection capabilities of the Cs5Cu3I2Cl6 film.
[0065] Fig.15 This is the optical characterization spectrum of the Cs5Cu3I2Cl6 film prepared in Example 2, and its characteristics are the same as those in Example 1.
[0066] Fig.16 This is the optical characterization spectrum of the Cs5Cu3I2Cl6 film prepared in Example 3, and its characteristics are the same as those in Example 1.
[0067] Fig.17 This is the stability XRD of the Cs5Cu3I2Cl6 film prepared in Example 1. It can be seen from the figure that the film is a very stable material in an air environment. After being placed in ambient air for more than 6 months, the film XRD shows no impurity peaks and obvious degradation, proving that the film still has good crystallinity, which is more stable than traditional lead-based and tin-based perovskites.
[0068] Fig.18 The current-voltage characteristic curve of the photovoltaic ultraviolet photodetector based on the Cs5Cu3I2Cl6 thin film prepared in Example 1 under different light intensity irradiation conditions; it can be seen from the figure that in the dark state, the Cs5Cu3I2Cl6 thin film detector has a current as low as 1.1×10 -12 The dark current of the device is 1.1 pA (1.1 pA), and as the light intensity increases, the photocurrent and electric field of the device also increase.
[0069] Fig.19 The current variation curve of the photovoltaic ultraviolet photodetector based on Cs5Cu3I2Cl6 thin film prepared in Example 1 under different light intensities over time; it can be seen from the figure that the device can maintain good repeatability and good switching characteristics under different incident light intensities, and is as low as 0.13μW / cm 2 The incident light below still has an obvious switching response, which is attributed to the lower dark current and noise current of the prepared thin film device.
[0070] Fig. 20 The responsiveness (R) of the photovoltaic ultraviolet photodetector based on the Cs5Cu3I2Cl6 thin film prepared in Example 1 under different light intensities can reach up to 117 mA / W.
[0071] Fig.21 The normalized detection (D*) of the photovoltaic ultraviolet photodetector based on Cs5Cu3I2Cl6 thin film prepared in Example 1 under different light intensities can reach up to 1.9×10 13 Jones.
[0072] Fig. 22 This is the response speed curve of the photovoltaic ultraviolet photodetector based on Cs5Cu3I2Cl6 thin film prepared in Example 1 under 250Hz modulated light; it can be seen that the rising edge response speed of the device is 750μs, and the falling edge response speed is 770μs, showing an ultra-fast response speed.
[0073] Fig.23 Comparing the current-time curves of the photovoltaic ultraviolet photodetector based on the Cs5Cu3I2Cl6 thin film prepared in Example 1 after being placed at a high temperature of 85 degrees Celsius for two months, it can be seen that the photocurrent of the device has almost no attenuation and has good thermal stability.
[0074] Fig.24 The current-time curve of the photovoltaic ultraviolet photodetector based on Cs5Cu3I2Cl6 thin film prepared in Example 1 running continuously in air for 400 hours without packaging shows that the device has good air stability and continuous operation stability.
[0075] Fig.25 The IV curves of the photoconductive ultraviolet photodetector based on Cs5Cu3I2Cl6 thin film prepared in Example 2 under different light intensities show that the device has a very obvious switching ratio under different light intensities.
[0076] Fig.26The light intensity dependence time-current curve of the photoconductive ultraviolet photodetector based on Cs5Cu3I2Cl6 thin film prepared in Example 2 under 5V bias voltage shows that the device has good switching characteristics and light intensity dependence.
[0077] Fig. 27 This is the current-external quantum efficiency curve of the light emitting diode (LED) based on the Cs5Cu3I2Cl6 thin film prepared in Example 3. It can be seen that the LED can achieve an electroluminescent performance of EQE greater than 0.01%.
[0078] Fig.28 The voltage-current curve and voltage-brightness curve of the light-emitting diode (LED) based on the Cs5Cu3I2Cl6 thin film prepared in Example 3 show that the light-emitting device can operate at a large current and the brightness can be greater than 40 candelas per square centimeter.
[0079] Fig.29 This is a dissolution experiment of the three drugs in Comparative Example 1 in pure formamide, pure DMSO and a mixed solvent of the two. Finally, the mixed solvent of formamide and DMSO was able to fully dissolve the monomers to obtain the Cs5Cu3I2Cl6 precursor solution, laying the foundation for the subsequent film and device preparation. DETAILED DESCRIPTION
[0080] The following is a detailed description of an embodiment of the present invention. This embodiment is implemented based on the technical solution of the present invention, and a detailed implementation method and a specific operation process are given in conjunction with the accompanying drawings. However, the protection scope of the present invention is not limited to the following embodiments.
[0081] Example 1
[0082] See also Figure 1 The photovoltaic ultraviolet photodetector of this embodiment is a Cs5Cu3I2Cl6 polycrystalline film formed by a one-step spin coating method on an epitaxially grown n-GaN substrate, and the film forms a pn junction with n-GaN, thereby forming a photovoltaic structure device capable of self-driving. Among them, the Cs5Cu3I2Cl6 polycrystalline film serves as a light absorption layer and a carrier transmission channel, contributing to the photocurrent.
[0083] The preparation method of the ultraviolet photodetector of this embodiment is as follows:
[0084] Step 1. Clean the sapphire (Al2O3) substrate to remove surface impurities;
[0085] Step 2. Obtain an approximately 4.5 μm thick n-GaN film as an electron transport layer by epitaxial growth;
[0086] Step 3. Add 23.3 mg CsCl, 24.0 mg CsI and 13.7 mg CuCl (3:2:3) into 375 μL (dimethyl sulfoxide) DMSO and 125 μL formamide (FM) mixed solvent (DMSO:FM=3:1), heat to 40°C, stir for 3 hours to fully dissolve, and obtain Cs5Cu3I2Cl6 precursor solution;
[0087] Step 4. Filter the dissolved Cs5Cu3I2Cl6 precursor solution using a 0.22 μm filter to filter out unnecessary impurities;
[0088] Step 5. Fix the cleaned n-GaN substrate on a coating machine, use a pipette to absorb a certain amount of precursor solution, and use a one-step spin coating method to prepare a thin film on the n-GaN, where the rotation speed is 4500 rpm and the spin coating is 30 seconds; the film thickness is 120nm to 160nm.
[0089] Step 6. The prepared film was transferred to a hot plate at 100 °C for 5 min for further annealing to evaporate the remaining solvent and enhance the crystallinity of the film;
[0090] Step 8. Cool the annealed film to room temperature, and then evaporate a layer of Au and In on the film and n-GaN as an anode and a cathode, respectively, to obtain an ultraviolet photodetector based on the Cs5Cu3I2Cl6 film;
[0091] Example 2
[0092] See also Figure 2 The photoconductive ultraviolet photodetector of this embodiment is a Cs5Cu3I2Cl6 polycrystalline film formed on the patterned interdigitated electrode by a one-step spin coating method. The film forms an ohmic contact with the electrode and realizes the ultraviolet light detection function under an external bias. Among them, the Cs5Cu3I2Cl6 polycrystalline film serves as a light absorption layer and a carrier transmission channel, contributing to the photocurrent.
[0093] The preparation method of the ultraviolet photodetector of this embodiment is as follows:
[0094] Step 1. Clean the insulating substrate to remove surface impurities;
[0095] Step 2. Prepare gold interdigital electrodes by magnetron sputtering process, wherein the electrode finger length is 2 mm, the finger width is 20 μm, the channel spacing is 20 μm, and the number of interdigital pairs is 50;
[0096] Step 3. Add 23.3 mg CsCl, 24.0 mg CsI and 13.7 mg CuCl (3:2:3) into 375 μL (dimethyl sulfoxide) DMSO and 125 μL formamide (FM) mixed solvent (DMSO:FM=3:1), heat to 40°C, stir for 3 hours to fully dissolve, and obtain Cs5Cu3I2Cl6 precursor solution;
[0097] Step 4. Filter the dissolved Cs5Cu3I2Cl6 precursor solution using a 0.22 μm filter to filter out unnecessary impurities;
[0098] Step 5. Fix the cleaned patterned interdigital electrode substrate on a coating machine, use a pipette to absorb a certain amount of precursor solution, and use a one-step spin coating method to prepare a thin film on the interdigital electrode, where the rotation speed is 2500 rpm and the spin coating is 30 seconds; the film thickness is 160nm to 200nm.
[0099] Step 6. The prepared film was transferred to a hot plate at 100 °C for 5 min for further annealing to evaporate the remaining solvent and enhance the crystallinity of the film;
[0100] Step 7. Cooling the annealed film to room temperature, thereby obtaining a photoconductive ultraviolet photodetector based on the Cs5Cu3I2Cl6 film;
[0101] Example 3
[0102] The light emitting diode (LED) of this embodiment is a Cs5Cu3I2Cl6 polycrystalline thin film formed by a one-step spin coating method on a PEDOT:PSS hole transport layer spin-coated on an ITO substrate, and then a layer of electron transport layer TmPyPB is evaporated on the thin film, and finally a layer of LiF / Al electrode is evaporated on TmPyPB. Among them, the Cs5Cu3I2Cl6 polycrystalline thin film serves as the light emitting layer, and holes-electrons will recombine and emit light in the thin film layer.
[0103] Step 1. Clean the ITO conductive glass to remove surface impurities;
[0104] Step 2. Use a 0.22 μm filter to filter the PEDOT:PSS diluted with water in a ratio of 1:1, fix the cleaned ITO conductive glass on a gel coater, use a pipette to absorb a certain amount of PEDOT:PSS solution, and apply it to the ITO by a one-step spin coating method, wherein the rotation speed condition is 4000 rpm and the spin coating is 50 seconds;
[0105] Step 3. Place the spin-coated PEDOT:PSS wet film on a hot plate at 150°C for annealing and crystallization;
[0106] Step 4. Add 23.3 mg CsCl, 24.0 mg CsI and 13.7 mg CuCl (3:2:3) to 375 μL (dimethyl sulfoxide) DMSO and 125 μL formamide (FM) mixed solvent (DMSO:FM = 3:1), heat at 40°C, and stir for 3 hours to fully dissolve;
[0107] Step 5. Filter the dissolved Cs5Cu3I2Cl6 precursor solution using a 0.22 μm filter to filter out unnecessary impurities;
[0108] Step 6. Fix the annealed PEDOT:PSS / ITO substrate on a coating machine, use a pipette to absorb a certain amount of precursor solution, and use a one-step spin coating method to prepare a thin film on the upper layer of PEDOT:PSS, where the rotation speed is 8000 rpm and the spin coating is 50 seconds; the film thickness is 80nm to 120nm.
[0109] Step 7: The prepared film is transferred to a hot plate at 100°C for 5 minutes for further annealing to volatilize the remaining solvent and enhance the crystallinity of the film;
[0110] Step 8. Place the annealed film in a vacuum coating machine to evaporate the TmPyPB electron transport layer and the LiF / Al electrode, and finally obtain a light-emitting diode (LED) device with a structure of ITO / PEDOT:PSS / Cs5Cu3I2Cl6 / TmPyPB / LiF / Al;
[0111] Example 4
[0112] The method for preparing the photovoltaic type ultraviolet photodetector, the photoconductive type ultraviolet photodetector and the light emitting diode (LED) device is consistent with the above embodiments. The component ratio of the Cs5Cu3X8 (X=Cl, Br, I) precursor solution in step 3 is regulated, specifically by adjusting the drug ratio when preparing the precursor solution:
[0113] 47.0 mg CsI, 6.8 mg CuI and 7.1 mg CuCl (5:1:2) or 12.1 mg CsCl, 28.2 mg CsI, 20.6 mg CuI (2:3:3) were added to 445 μl (dimethyl sulfoxide) DMSO and 55 μl formamide (FM) mixed solvent (DMSO:FM=8:1), heated to 40°C, and stirred for 3 hours for full dissolution to obtain a Cs5Cu3I6Cl2 precursor solution; the device preparation method was the same as the steps in Examples 1-3 to obtain three devices based on Cs5Cu3I6Cl2 thin films.
[0114] Example 5
[0115] 41.9 mg CsCl, 4.9 mg CuCl and 14.2 mg CuBr (5:1:2) or 21.1 mg CsBr, 25.1 mg CsCl, 14.7 mg CuCl (2:3:3) were added to 70 μl (dimethyl sulfoxide) DMSO and 430 μl formamide (FM) mixed solvent (DMSO:FM=1:6), heated to 40°C, and stirred for 3 hours for full dissolution to obtain a Cs5Cu3Br2Cl6 precursor solution; the device preparation method was the same as the steps in Examples 1-3 to obtain three devices based on Cs5Cu3Br2Cl6 thin films.
[0116] Example 6
[0117] 46.2 mg CsBr, 6.2 mg CuBr and 8.6 mg CuCl (5:1:2) or 14.6 mg CsCl, 27.7 mg CsBr, 18.7 mg CuBr (2:3:3) were added to 125 μl (dimethyl sulfoxide) DMSO and 375 μl formamide (FM) mixed solvent (DMSO:FM=1:3), heated to 40°C, and stirred for 3 hours for full dissolution to obtain a Cs5Cu3Br6Cl2 precursor solution; the device preparation method was the same as the steps in Examples 1-3 to obtain three devices based on Cs5Cu3Br6Cl2 thin films.
[0118] Example 7
[0119] 40.9 mg CsBr, 5.5 mg CuBr and 14.6 mg CuI (5:1:2) or 19.9 mg CsI, 24.5 mg CsBr, 16.5 mg CuBr (2:3:3) were added to 430 μl (dimethyl sulfoxide) DMSO and 70 μl formamide (FM) mixed solvent (DMSO:FM=6:1), heated to 40°C, and stirred for 3 hours for full dissolution to obtain Cs5Cu3I2Br6 precursor solution; the device preparation method was the same as the steps in Examples 1-3 to obtain three devices based on Cs5Cu3I2Br6 thin films.
[0120] Example 8
[0121] 41.4 mg CsI, 6.0 mg CuI and 13.5 mg CuBr (5:1:2) or 14.6 mg CsBr, 26.8 mg CsI, 19.6 mg CuI (2:3:3) were added to 250 μL of dimethyl sulfoxide (DMSO) and 250 μL of formamide (FM) mixed solvent (DMSO:FM=1:1), heated to 40°C, and stirred for 3 hours for full dissolution to obtain a Cs5Cu3I6Br2 precursor solution; the device preparation method was the same as the steps in Examples 1-3 to obtain three devices based on Cs5Cu3I6Br2 thin films.
[0122] Based on the precursor solutions of Cs5Cu3X8 (X=Cl, Br, I) in different proportions in Examples 1-8, the detection limits of photovoltaic ultraviolet photodetectors obtained by the same film and device preparation processes can all be higher than 10 10 The light-to-dark current ratio (Ratio) of photoconductive ultraviolet photodetectors can be greater than 100, and the external quantum efficiency (EQE) of light-emitting diodes (LEDs) can reach an average of 0.01%.
[0123] Comparative Example 1
[0124] This example compares the solubility of the monomer in the Cs5Cu3X8 (X = Cl, Br, I) precursor solution with that in the formamide solvent and other organic solvents, proving for the first time that formamide can be mixed with other organic solvents to achieve the preparation of different precursor solutions. Taking the Cs5Cu3I2Cl6 precursor solution as an example, the comparison solvents are organic solvents such as DMSO, DMF, acetonitrile, and ethanol:
[0125] Solution 1: Add 23.3 mg CsCl, 24.0 mg CsI and 13.7 mg CuCl (3:2:3) into 500 μL formamide, 500 μL DMSO, 500 μL DMF, 500 μL acetonitrile, 500 μL ethylene glycol and 500 μL water respectively, and stir at room temperature for 1 hour. CsCl is insoluble in DMSO, DMF, acetonitrile and ethylene glycol, but is soluble in formamide.
[0126] Solution 2: Add 23.3 mg CsCl, 24.0 mg CsI and 13.7 mg CuCl (3:2:3) into 500 μL pure formamide and 500 μL pure DMSO respectively. CuCl cannot be completely dissolved in pure formamide and CsCl cannot be dissolved in pure DMSO, so Cs5Cu3I2Cl6 thin film and device cannot be obtained.
[0127] Solution 3: Add 23.3mg CsCl, 24.0mg CsI and 13.7mg CuCl (3:2:3) into 500μl mixed solvent of formamide and DMSO at a volume ratio of 1:3. All three chemicals can be quickly dissolved to obtain a colorless and transparent Cs5Cu3I2Cl6 precursor solution. (See Fig.29 , Table 1)
[0128] Table 1 shows the dissolution states of the three drugs in comparative example 1 in common organic solvents.
[0129]
[0130] It can be seen from Table 1 that most solvents cannot prepare Cs5Cu3I2Cl6 precursor solutions with uniform composition.
[0131] The above shows and describes the basic principles, main features and advantages of the present invention. The present invention is not limited by the above embodiments. The above embodiments and descriptions are only preferred examples of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A copper-based perovskite Cs5Cu3X8 film prepared by a solution method, characterized in that The perovskite Cs5Cu3X8 film is composed of feather-shaped grains with a diameter of 30nm to 3μm, in which the ratio of the three elements Cs:Cu:X is 5:3:
8. X is Cl, Br or I, and the film is a pure phase perovskite Cs5Cu3X8 film with a thickness of 50nm to 1μm.
2. A method for preparing the copper-based perovskite Cs5Cu3X8 thin film according to claim 1, characterized in that The following steps are involved: The precursor solution is applied to the substrate, a one-step spin coating method is used, or a one-step spin coating method is used in combination with anti-solvent washing to obtain a wet film, and the wet film is heated and annealed to obtain the obtained product; wherein the precursor solution is obtained by using a mixture of two or more of cesium chloride, cesium bromide, cesium iodide, cuprous chloride, cuprous bromide and cuprous iodide as raw materials and fully dissolving them in a solvent; and the solvent is a mixed solvent of formamide and dimethyl sulfoxide in a volume ratio of 1 to 10:1 to 10.
3. The method for preparing the thin film according to claim 2, characterized in that The substrate is a conductive layer or an insulating substrate; wherein the conductive layer is GaN, Ga2O3, PEDOT:PSS, TmPyPB or ITO, and the insulating substrate is quartz or a flexible insulating substrate.
4. The method for preparing the thin film according to claim 2, characterized in that The spin coating method adopts a rotation speed of 999 to 9999 rpm and a spin coating time of 10 to 70 seconds.
5. The method for preparing the thin film according to claim 2, characterized in that The anti-solvent used in the wet film preparation process is petroleum ether, hexane, heptane, chloropropane, ethyl bromide, nitromethane, dichloroethane, chloroform, n-pentane, carbon tetrachloride, carbon disulfide, benzene, toluene, xylene, benzene bromide, phenol, ethyl ether, isopropyl ether, ethyl acetate, butyl acetate, methyl propionate, propyl propionate, ethanol, methyl ethyl alcohol, n-butanol, tert-butanol, tetrahydrofuran, dioxane or acetone; the volume ratio of the anti-solvent to the precursor solution is 1:1 to 1:
10.
6. The method for preparing a thin film according to claim 2, characterized in that The heating annealing is to anneal the wet film on a hot stage at 60° C. to 180° C. for 2 min to 60 min.
7. A photoelectric device prepared using the thin film according to claim 1, characterized in that The photoelectric device is a photovoltaic ultraviolet photodetector, a photoconductive ultraviolet photodetector or a light emitting diode.
8. A method for preparing the photovoltaic ultraviolet photodetector according to claim 7, characterized in that The method comprises the following steps: (1) Cleaning the substrate; (2) obtaining an electron transport layer by epitaxial growth; (3) at room temperature, cesium chloride, cesium bromide, cesium iodide, cuprous chloride, cuprous bromide and a mixture of two or more cuprous iodide are used as raw materials and fully dissolved in a solvent to obtain a Cs5Cu3X8 precursor solution, wherein X = Cl, Br, I; (4) dropping a fully dissolved precursor solution onto the electron transport layer, and forming a wet film by one-step spin coating or one-step spin coating combined with anti-solvent washing; placing the wet film on a hot stage for heating and annealing to obtain a Cs5Cu3X8 perovskite thin film layer, wherein X = Cl, Br, I; (5) A layer of electrode is added on the surface of the perovskite thin film layer and the electron transport layer to obtain a photovoltaic ultraviolet photodetector.
9. A method for preparing the photoconductive ultraviolet photodetector according to claim 7, characterized in that The method comprises the following steps: (1) Cleaning the substrate; (2) preparing patterned interdigitated electrodes; (3) at room temperature, cesium chloride, cesium bromide, cesium iodide, cuprous chloride, cuprous bromide and a mixture of two or more cuprous iodide are used as raw materials and fully dissolved in a solvent to obtain a Cs5Cu3X8 precursor solution, wherein X = Cl, Br, I; (4) dropping a fully dissolved precursor solution onto the interdigital electrodes, and forming a wet film by one-step spin coating or one-step spin coating combined with anti-solvent washing; placing the wet film on a hot stage for heating and annealing, and cooling to obtain a photoconductive ultraviolet photodetector.
10. A method for preparing a light emitting diode according to claim 7, characterized in that The method comprises the following steps: (1) Cleaning the substrate; (2) coating a hole transport layer on the substrate surface; (3) at room temperature, cesium chloride, cesium bromide, cesium iodide, cuprous chloride, cuprous bromide and a mixture of two or more cuprous iodide are used as raw materials and fully dissolved in a solvent to obtain a Cs5Cu3X8 precursor solution, wherein X = Cl, Br, I; (4) dropping a fully dissolved precursor solution onto the hole transport layer, and forming a wet film by one-step spin coating or one-step spin coating combined with anti-solvent washing; placing the wet film on a hot stage for heating and annealing to obtain a light-emitting layer; then preparing an electron transport layer on the light-emitting layer by evaporation or spin coating, and finally adding a metal electrode on the surface of the electron transport layer to obtain a light-emitting diode.