Vanadium-based oxide coated C composite material as well as preparation method and application thereof

Through the reaction and carbonization of vanadium-based materials and organic molecular monomers, vanadium-based oxide @C composite materials were prepared, which solved the problem of poor conductivity of vanadium-based oxides and significantly improved their performance in the field of electrochemical energy storage. Especially in terms of rate performance and cycle stability.

CN119059557APending Publication Date: 2024-12-03XIAMEN INST OF RARE EARTH MATERIALS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310626665.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-30
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Vanadium-based oxides have problems such as low conductivity, poor rate performance and cycle stability in secondary batteries and supercapacitors, resulting in rapid deterioration of capacity and unable to meet the actual application needs.

Method used

By mixing vanadium-based material with organic molecular monomers, precursors are prepared, and then polymerization and carbonization are carried out under an oxygen atmosphere or an inert atmosphere, vanadium-based oxide @C composite materials are prepared to improve conductivity and reduce charge and discharge process strain effect.

Benefits of technology

It improves the conductivity and transmission rate of vanadium-based oxides, and improves its performance in electrochemical energy storage, especially in rate performance and cycle stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119059557A_ABST
    Figure CN119059557A_ABST
Patent Text Reader

Abstract

The invention provides a vanadium-based oxide coated C composite material as well as a preparation method and application thereof. The preparation method comprises the following steps: generating a precursor by utilizing a reaction of a vanadium-based material and an organic molecular monomer, then carrying out a polymerization reaction on the precursor in an oxygen atmosphere, and carrying out a high-temperature carbonization reaction in an inert atmosphere or a reducing atmosphere, or directly carrying out the high-temperature carbonization reaction on the precursor in the inert atmosphere or the reducing atmosphere; the vanadium-based oxide coated C composite material is obtained. The vanadium-based oxide coated C composite material is simple in preparation process, the obtained composite material is high in purity and regular in structure, composite materials with different morphological structures and carbon contents can be constructed by regulating and controlling different vanadium-based materials and organic molecular monomers, the problem of poor conductivity of the vanadium-based oxide is solved, and the performance of the vanadium-based oxide coated C composite material in the aspect of energy storage is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of vanadium-based oxide @C composite materials, and in particular relates to a vanadium-based oxide @C composite material and a preparation method and application thereof. Background Art

[0002] Vanadium-based oxides are widely used in electrochemical energy storage fields such as lithium, sodium, potassium, zinc and other secondary batteries and supercapacitors due to their advantages of low cost, sufficient production, multiple valence states, multiple electron transfer and large capacity. Vanadium-based oxides also have rich valence state changes and special layered structures, so they have higher charge storage capacity than other non-precious transition metal oxides. In addition, vanadium-based materials have an open framework and multiple coordination, which can form various vanadium-based materials with different crystal structures.

[0003] However, vanadium-based oxides, like other oxides, also have the disadvantages of low conductivity, poor rate performance and poor charge-discharge cycle stability. During the cycle, severe structural damage, low intrinsic conductivity and dissolution of vanadium ions always lead to rapid deterioration of capacity, which cannot meet practical applications. Summary of the invention

[0004] In view of the problems that vanadium-based oxides have low conductivity, poor rate performance and cycle stability when used as electrode materials for secondary batteries and supercapacitors, the present invention provides a vanadium-based oxide@C composite material and a preparation method and use thereof. The vanadium-based oxide@C composite material can effectively improve the conductivity of vanadium-based oxides, increase the transmission rate of conductive ions, reduce the strain caused by conductive ion intercalation during the charge and discharge process, reduce the negative impact caused by side reactions during the charge and discharge process, and improve its performance in electrochemical energy storage.

[0005] The object of the present invention is achieved through the following technical solutions:

[0006] A method for preparing a vanadium-based oxide@C composite material, the method comprising the following steps:

[0007] (1) mixing a vanadium-based material and an organic molecular monomer, reacting the mixture, and preparing a precursor;

[0008] (2) subjecting the precursor of step (1) to a polymerization reaction under an oxygen atmosphere, and then carbonizing the polymerization product under an inert atmosphere or a reducing atmosphere; or directly carbonizing the precursor under an inert atmosphere or a reducing atmosphere to obtain the vanadium-based oxide@C composite material.

[0009] According to an embodiment of the present invention, the vanadium-based oxide@C composite material is a composite material of vanadium-based oxide and carbon.

[0010] According to an embodiment of the present invention, in step (1), the vanadium-based material is selected from one, two or more of vanadium metal, vanadium-based salt or vanadium-based oxide.

[0011] Exemplarily, the vanadium-based salt is selected from one, two or more of vanadium chloride, vanadium nitrate, vanadium sulfate, vanadium phosphate, vanadium acetate, vanadium acetylacetonate, ammonium metavanadate, ammonium metavanadate, sodium metavanadate, potassium metavanadate, sodium orthovanadate, vanadyl sulfate, vanadium tetrachloride and vanadium trichloride.

[0012] Illustratively, the vanadium-based oxide is selected from one, two or more of vanadium monoxide, vanadium trioxide, vanadium dioxide and vanadium pentoxide.

[0013] According to an embodiment of the present invention, in step (1), the organic molecule monomer is selected from linear or branched C1-C18 alkylamines and their derivatives (such as methylamine, ethylamine, propylamine, pentylamine, hexylamine, heptylamine, octylamine, nonylamine, decylamine, undecylamine, dodecylamine, tridecylamine, tetradecylamine, pentadecylamine, hexadecylamine, heptadecanylamine, octadecylamine, isobutylamine, diisobutylamine, N-ethylbutylamine, diisooctylamine, NN dimethyl n-octylamine, etc.), p-phenylenediamine, o-phenylenediamine, m-phenylenediamine, benzidine, 3,3-diaminobenzidine, p-phenylenediamine, o-phenylenediamine, m-phenylenediamine, benzylamine, triphenylamine, diphenylmethane One, two or more of amine, 1,5-diaminonaphthalene, 1,8-diaminonaphthalene, naphthylamine, diaminodiphenylmethane, 3,3',5,5'-tetramethylbenzidine, N-methyl-1,2-phenylenediamine, aniline, dopamine, pyridine, 1-aminopyridine, 2-aminopyridine, 3-aminopyridine, pyrrole, 1-aminopyrrole, 2-aminopyrrole, 3-aminopyrrole, o-aminophenol, p-aminophenol, m-aminophenol, p-aminobenzoic acid, terephthalic acid, isophthalic acid, 3,5-diaminobenzenesulfonic acid, 2,4-diaminobenzoic acid, p-aminophenylboric acid and p-aminophenylphosphoric acid.

[0014] According to an embodiment of the present invention, in step (1), the mass ratio of the vanadium-based material to the organic molecular monomer is 1:0.1 to 6, such as 1:0.1, 1:0.5, 1:1, 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5, 1:4, 1:4.5, 1:5, 1:5.5 or 1:6.

[0015] According to an embodiment of the present invention, in step (1), the organic molecular monomer and the vanadium-based material may react in the presence of a solvent or in the absence of a solvent.

[0016] Illustratively, the reaction in the absence of a solvent is, for example, that the organic molecular monomer and the vanadium-based material are reacted by dry mixing by grinding, ball milling, blender or crusher; such as the organic molecular monomer and the vanadium-based material are dry mixed by grinding, ball milling, blender or crusher until no obvious particles are present.

[0017] Wherein, the grinding is performed by using a mortar, and the grinding time is 0.1h to 24h.

[0018] Wherein, the rotation speed of the ball mill is 5 to 1500 RPM, and the time of the ball mill is 0.1 h to 24 h.

[0019] Wherein, the rotation speed of the stirrer is 5 to 1500 RPM, and the stirring time is 0.1 h to 24 h.

[0020] Wherein, the rotation speed of the pulverizer is 5 to 20,000 RPM, and the pulverization time is 0.1 h to 24 h.

[0021] Exemplarily, the reaction in the presence of a solvent is, for example, mixing a solvent, an organic molecule monomer and a vanadium-based material, and reacting. There is no particular definition for the mixing method, and it is sufficient to achieve the mixing of the solvent, the organic molecule monomer and the vanadium-based material. For example, the vanadium-based material and the organic molecule monomer can be directly dispersed in the solvent and then stirred and mixed evenly; one, two or more of the vanadium-based material or the organic molecule monomer can be first dissolved in the solvent and then stirred and mixed evenly; the vanadium-based material can be dispersed in the solvent, and the organic molecule monomer can be added and stirred and mixed evenly; or the organic molecule monomer can be dispersed in the solvent, and the vanadium-based material can be added and stirred and mixed evenly; or the vanadium-based material and the organic molecule monomer can be mixed, and then the solvent can be added and stirred and mixed evenly; or the vanadium-based material and the organic molecule monomer can be dispersed in the solvent respectively, and then the above solutions can be mixed, and then stirred and mixed evenly.

[0022] Preferably, the solvent is one or a mixture of any of an organic solvent and water. For example, the organic solvent may be one, two or more of methanol, ethanol, propanol, toluene, acetone, isopropanol, NMP (N-methylpyrrolidone), DMF (N,N-dimethylformamide), DMSO (dimethyl sulfoxide), THF (tetrahydrofuran), benzene, toluene, xylene, pentane, hexane, octane, cyclohexane, cyclohexanone, toluene-cyclohexanone, chlorobenzene, dichlorobenzene, dichloromethane, chloroform, carbon tetrachloride, ether, propylene oxide, methyl acetate, ethyl acetate, propyl acetate, methyl butyl ketone, methyl isobutyl ketone, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, acetonitrile, phenol, etc.

[0023] Preferably, the ratio of the sum of the masses of the vanadium-based material and the organic molecular monomer to the amount of the solvent is 1g:(1-100)mL, such as 1g:1mL, 1g:5mL, 1g:10mL, 1g:15mL, 1g:20mL, 1g:25mL, 1g:30mL, 1g:35mL, 1g:40mL, 1g:45mL, 1g:50mL, 1g:55mL, 1g:60mL, 1g:65mL, 1g:70mL, 1g:75mL, 1g:80mL, 1g:85mL, 1g:90mL, 1g:95mL or 1g:100mL.

[0024] Preferably, the organic molecular monomer and vanadium-based material before the reaction can be added by dripping with a dropper, dripping with a peristaltic pump, etc. For example, the material can be added by dripping with a peristaltic pump. For another example, the feeding speed is 0.1 to 200 mL / min.

[0025] According to an embodiment of the present invention, in step (1), the reaction is carried out under stirring, and the stirring can be carried out by mechanical stirring, magnetic stirring, ultrasonic stirring, etc. For example, magnetic stirring can be used to mix the materials evenly. For another example, the speed of the magnetic stirring is 5 to 1500 RPM, and the stirring time is 0.1h to 24h.

[0026] According to an embodiment of the present invention, in step (1), the reaction is carried out at room temperature, or under heating conditions, or under high pressure heating conditions (i.e., hydrothermal reaction).

[0027] Exemplarily, the heating is performed by heating in a water bath or an oil bath; the high-pressure heating is performed by performing a hydrothermal reaction in a stirred reactor, a solvent thermal reactor, a hydrothermal reactor, a supercritical reactor or a microwave reactor.

[0028] According to an embodiment of the present invention, in step (1), the reaction time is 0.1 to 72 h; such as 5 h, 10 h, 15 h, 20 h, 25 h, 30 h, 35 h, 40 h, 45 h, 50 h, 55 h, 60 h, 65 h, 70 h or 72 h.

[0029] According to an embodiment of the present invention, in step (1), the reaction temperature is 20-350°C; such as 20°C, 30°C, 40°C, 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, 190°C, 210°C, 220°C, 230°C, 240°C, 250°C, 260°C, 270°C, 280°C, 290°C, 300°C, 310°C, 320°C, 330°C, 340°C or 350°C.

[0030] According to an embodiment of the present invention, if the reaction is carried out at room temperature, the reaction temperature is 20-40°C; if the reaction is carried out under heating conditions, the reaction temperature is 50-250°C; if the reaction is carried out under high pressure heating conditions, the reaction temperature is 100-350°C.

[0031] According to an embodiment of the present invention, in step (1), the reaction mixture is separated by, for example, centrifugation, drying, filtering, etc.

[0032] Preferably, the centrifugation can be performed by a centrifuge; wherein the centrifugation speed is 5 to 20,000 RPM, and the centrifugation time is 1 min to 60 min.

[0033] Preferably, the drying can be performed by at least one of rotary evaporation drying, freeze drying, spray drying, forced air oven drying, vacuum oven drying, and the like.

[0034] Preferably, the filtration is performed by conventional industrial suction filtration.

[0035] Preferably, the present invention does not impose any particular limitation on the method of drying the sample after reaction separation. For example, the material may be dried in an oven.

[0036] According to an embodiment of the present invention, in step (2), the oxygen atmosphere refers to an atmosphere in which oxygen exists, such as a mixed atmosphere of oxygen and an inert atmosphere, or pure oxygen or air.

[0037] According to an embodiment of the present invention, in step (2), the polymerization reaction temperature is 120°C to 400°C, such as 120°C, 130°C, 150°C, 180°C, 200°C, 250°C, 280°C, 300°C, 320°C, 350°C, 380°C or 400°C; the polymerization reaction time is 0.1h to 12h, such as 1h, 2h, 3h, 4h, 5h, 6h, 7h, 8h, 10h or 12h.

[0038] According to an embodiment of the present invention, in step (2), the temperature of the carbonization treatment is 300°C to 1200°C, such as 300°C, 400°C, 450°C, 500°C, 550°C, 600°C, 650°C, 700°C, 750°C, 800°C, 850°C, 900°C, 950°C, 1000°C, 1100°C or 1200°C; the time of the carbonization treatment is 0.1 to 24h, such as 0.1h, 0.3h, 0.5h, 0.7h, 0.9h, 1h, 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h, 11h, 12h, 13h, 14h, 5h, 6h, 7h, 8h, 9h, 10h, 11h or 12h.

[0039] According to the embodiment of the present invention, in step (2), the heating method of the carbonization treatment is not particularly limited, for example, the temperature may be directly raised to the carbonization treatment temperature and kept warm, or it may be paused at an intermediate temperature and then gradually raised to the carbonization treatment temperature, or it may be directly raised from the polymerization reaction temperature to the carbonization treatment temperature. For example, the temperature may be directly raised from 20°C to 500°C; or the temperature may be raised from 20°C to 200°C and kept warm for 2h, and then raised to 500°C.

[0040] According to an embodiment of the present invention, in step (2), the heating rate of the carbonization treatment is 0.05°C to 20°C / min, such as 0.05°C / min, 0.1°C / min, 1°C / min, 2°C / min, 5°C / min, 10°C / min, 15°C / min or 20°C / min.

[0041] According to an embodiment of the present invention, in step (2), the inert atmosphere is one of nitrogen, argon, helium, ammonia, etc., or a mixture of any multiple thereof.

[0042] According to an embodiment of the present invention, in step (2), the reducing atmosphere is pure hydrogen, or a gas mixed with one or more of nitrogen, argon, helium, ammonia, etc.

[0043] The present invention also provides a vanadium-based oxide@C composite material, which is prepared by the above method.

[0044] According to an embodiment of the present invention, the vanadium-based oxide@C composite material includes vanadium-based oxide and carbon, the mass of the vanadium-based oxide accounts for 5% to 95% of the total mass of the composite material, for example, 5%, 10%, 20%, 30%, 40%, 50%, 60%, 70%, 80%, 90% or 95%; the mass of the carbon accounts for 5% to 95% of the total mass of the composite material, for example, 5%, 10%, 20%, 30%, 40%, 50%, 60%, 70%, 80%, 90% or 95%.

[0045] According to an embodiment of the present invention, the morphology of the vanadium-based oxide@C composite material is long strips, sheets, sandwich stacks, core-shell structures or spherical particles.

[0046] According to an embodiment of the present invention, at least one dimension of the vanadium-based oxide@C composite material is 0.1-50 μm, such as at least two dimensions of the vanadium-based oxide@C composite material is 0.1-50 μm, such as three dimensions of the vanadium-based oxide@C composite material is 0.1-50 μm.

[0047] According to an embodiment of the present invention, the specific surface area of ​​the vanadium-based oxide@C composite material is 1 to 300 cm 2 / g.

[0048] The present invention also provides the application of the vanadium-based oxide@C composite material in the field of secondary batteries and supercapacitors. Preferably, the application in lithium-ion secondary batteries, sodium-ion secondary batteries, potassium-ion secondary batteries, zinc-ion secondary batteries, such as zinc-ion secondary batteries.

[0049] Beneficial effects of the present invention:

[0050] The present invention provides a vanadium-based oxide @C composite material and a preparation method and application thereof. The present invention utilizes the reaction of a vanadium-based material and an organic molecular monomer to generate a precursor, and then the precursor is subjected to a polymerization reaction under an oxygen atmosphere, a high-temperature carbonization reaction under an inert atmosphere or a reducing atmosphere, or the precursor is directly subjected to a high-temperature carbonization reaction under an inert atmosphere or a reducing atmosphere to obtain a vanadium-based oxide @C composite material. The vanadium-based oxide @C composite material has a simple preparation process, and the obtained composite material has high purity and a regular structure. Composite materials with different morphological structures and carbon contents can be constructed by regulating different vanadium-based materials and organic molecular monomers, thereby solving the problem of poor electrical conductivity of vanadium-based oxides and improving their performance in energy storage. BRIEF DESCRIPTION OF THE DRAWINGS

[0051] Figure 1 is a SEM image of the vanadium-based oxide@C composite material prepared in Example 1.

[0052] Figure 2 is the XRD pattern of the vanadium-based oxide@C composite material prepared in Example 1.

[0053] Figure 3 This is a rate performance diagram of the vanadium-based oxide@C composite material prepared in Example 1.

[0054] Figure 4 This is a long cycle stability performance diagram of the vanadium-based oxide@C composite material prepared in Example 1.

[0055] Figure 5 This is a SEM image of the vanadium-based oxide@C composite material prepared in Example 2.

[0056] Figure 6 This is a SEM image of the vanadium-based oxide@C composite material prepared in Example 3. DETAILED DESCRIPTION

[0057] The preparation method of the present invention will be described in further detail below in conjunction with specific examples. It should be understood that the following examples are only exemplary illustrations and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.

[0058] Unless otherwise specified, the experimental methods used in the following examples are all conventional methods; the reagents, materials, etc. used in the following examples, unless otherwise specified, can be obtained from commercial channels.

[0059] Example 1

[0060] A vanadium-based oxide@C composite material comprises the following steps:

[0061] Step 1: Use 60 mL of water to disperse 1.0 g of V2O5 powder, add 1 mL of aniline to the V2O5 solution, and then use a magnetic stirrer to stir for 1 hour, and then put it into a hydrothermal reactor, hydrotherm at 180°C for 24 hours, filter, wash with excess water, and then dry in a forced air drying oven at 60°C for 24 hours to obtain a precursor;

[0062] Step 2: Keep the precursor at 700° C. in a nitrogen atmosphere for 12 hours to obtain a vanadium-based oxide@C composite material. The vanadium-based oxide@C composite material includes vanadium-based oxide and carbon, wherein the mass of the vanadium-based oxide accounts for 85% of the total mass of the composite material; and the mass of the carbon accounts for 15% of the total mass of the composite material.

[0063] Figure 1 : is a SEM image of the vanadium-based oxide@C composite material prepared in Example 1. It can be seen from the SEM image that the vanadium-based oxide@C composite material prepared in Example 1 is stacked in a regular strip shape of 10 μm.

[0064] Figure 2 This is the XRD test curve of the vanadium-based oxide@C composite material prepared in Example 1. From XRD, it can be seen that the structure of the material is V2O3 without other impurities.

[0065] Test Example 1

[0066] Take the vanadium-based oxide @C composite material prepared in Example 1, weigh each raw material according to the weight ratio of vanadium-based oxide @C composite material: Ketjen black (KT-black): PTFE = 8:1:1, add NMP solvent to prepare a negative electrode slurry, and then evenly coat it on a titanium foil, and then cut it into pole pieces with a diameter of 10 mm after vacuum drying at 90°C; use 2M Zn(CF3SO3)2 as the electrolyte, glass fiber as the diaphragm, and zinc foil as the negative electrode to assemble a CR2032 zinc ion battery for testing.

[0067] Figure 3 is the rate performance diagram of the vanadium-based oxide@C composite material prepared in Example 1. Figure 3 It can be concluded that the vanadium-based oxide @C composite material has excellent rate performance when used as the positive electrode of zinc ion battery, with a reversible discharge capacity of about 305 mAh / g at a current density of 0.3 A / g; and a reversible discharge capacity of more than 212 mAh / g at a high current density of 5.0 A / g. This shows that the vanadium-based oxide @C composite material prepared by the present invention has excellent specific capacity and rate performance.

[0068] Figure 4 is a long cycle stability performance diagram of the vanadium-based oxide@C composite material prepared in Example 1. Figure 4 It can be concluded that the vanadium-based oxide @C composite material has excellent cycle stability when used as the positive electrode of zinc ion battery. At a current density of 3A / g, 92% of the initial capacity is retained after 1000 cycles. This shows that the vanadium-based oxide @C composite material prepared by the present invention has excellent long-cycle stability.

[0069] Example 2

[0070] A vanadium-based oxide@C composite material comprises the following steps:

[0071] Step 1: Use 60 mL of water to disperse 1.0 g of V2O5 powder, add 1 mL of aniline to the V2O5 solution, then stir it with a magnetic stirrer for 24 hours, filter it, wash it with excess water, and then dry it in a forced air drying oven at 60 ° C for 24 hours to obtain a precursor;

[0072] Step 2: Keep the precursor at 700° C. in a nitrogen atmosphere for 12 hours to obtain a vanadium-based oxide@C composite material. The vanadium-based oxide@C composite material includes vanadium-based oxide and carbon, wherein the mass of the vanadium-based oxide accounts for 88% of the total mass of the composite material; and the mass of the carbon accounts for 12% of the total mass of the composite material.

[0073] Figure 5This is a SEM image of the vanadium-based oxide @C prepared in Example 2. From the SEM image, it can be seen that the vanadium-based oxide @C composite material prepared in Example 2 has a block and strip structure with a size of 5 to 10 microns as a whole, and small particles are attached to the surface.

[0074] Using it as an electrode and testing it according to the test method of Test Example 1, at a current density of 0.3A / g, it has a reversible discharge capacity of about 350mAh / g; at a high current density of 5.0A / g, it has a reversible discharge capacity of more than 260mAh / g; at a current density of 3A / g, it retains 90% of the initial capacity after 1000 cycles.

[0075] Example 3

[0076] A vanadium-based oxide@C composite material comprises the following steps:

[0077] Step 1: Use 60 mL of water to disperse 1.0 g of V2O5 powder, add 2.0 g of m-phenylenediamine to the V2O5 solution, and then use a magnetic stirrer to stir for 1 hour, and then put it into a hydrothermal reactor, hydrotherm at 100 ° C for 24 hours, filter, wash with excess water, and then use a forced air drying oven at 60 ° C for 24 hours to obtain a precursor;

[0078] Step 2: Keep the precursor at 700°C in a nitrogen atmosphere for 12 hours to obtain a vanadium-based oxide@C composite material. The vanadium-based oxide@C composite material includes vanadium-based oxide and carbon, wherein the mass of the vanadium-based oxide accounts for 70% of the total mass of the composite material; and the mass of the carbon accounts for 30% of the total mass of the composite material.

[0079] Figure 6 : is a SEM image of the vanadium-based oxide@C composite material prepared in Example 3. It can be seen from the SEM image that the vanadium-based oxide@C composite material prepared in Example 3 is agglomerated particles with a size of about 500 nm.

[0080] Using it as an electrode and testing it according to the test method of Test Example 1, at a current density of 0.3A / g, it has a reversible discharge capacity of about 342mAh / g; at a high current density of 5.0A / g, it has a reversible discharge capacity of more than 243mAh / g; at a current density of 3A / g, it retains 82% of the initial capacity after 1000 cycles.

[0081] Example 4

[0082] A vanadium-based oxide@C composite material comprises the following steps:

[0083] Step 1: Use 60 mL of water to disperse 1.0 g of V2O5 powder, add 1.0 g of m-phenylenediamine to the V2O5 solution, and then use a magnetic stirrer to stir for 1 hour, and then put it into a hydrothermal reactor, hydrotherm at 100 ° C for 24 hours, filter, wash with excess water, and then use a forced air drying oven at 60 ° C for 24 hours to obtain a precursor;

[0084] Step 2: Keep the precursor at 700° C. in a nitrogen atmosphere for 12 hours to obtain a vanadium-based oxide@C composite material. The vanadium-based oxide@C composite material includes vanadium-based oxide and carbon, wherein the mass of the vanadium-based oxide accounts for 83% of the total mass of the composite material; and the mass of the carbon accounts for 17% of the total mass of the composite material.

[0085] Using it as an electrode and testing it according to the test method of Test Example 1, at a current density of 0.3A / g, it has a reversible discharge capacity of about 366mAh / g; at a high current density of 5.0A / g, it has a reversible discharge capacity of more than 287mAh / g; at a current density of 3A / g, it retains 90% of the initial capacity after 1000 cycles.

[0086] Example 5

[0087] A vanadium-based oxide@C composite material comprises the following steps:

[0088] Step 1: Use 60 mL of water to disperse 1.0 g of V2O5 powder, add 0.5 g of m-phenylenediamine to the V2O5 solution, and then use a magnetic stirrer to stir for 1 hour, and then put it into a hydrothermal reactor, hydrotherm at 100 ° C for 24 hours, filter, wash with excess water, and then use a forced air drying oven at 60 ° C for 24 hours to obtain a precursor;

[0089] Step 2: Keep the precursor at 700° C. in a nitrogen atmosphere for 12 hours to obtain a vanadium-based oxide@C composite material. The vanadium-based oxide@C composite material includes vanadium-based oxide and carbon, wherein the mass of the vanadium-based oxide accounts for 92% of the total mass of the composite material; and the mass of the carbon accounts for 8% of the total mass of the composite material.

[0090] Using it as an electrode and testing it according to the test method of Test Example 1, at a current density of 0.3A / g, it has a reversible discharge capacity of about 402mAh / g; at a high current density of 5.0A / g, it has a reversible discharge capacity of more than 298mAh / g; at a current density of 3A / g, it retains 84% ​​of the initial capacity after 1000 cycles.

[0091] Example 6

[0092] A vanadium-based oxide@C composite material comprises the following steps:

[0093] Step 1: 1.0 g p-phenylenediamine and 1.0 g V2O5 were mixed in a planetary ball mill for 24 h to obtain a precursor;

[0094] Step 2: Keep the precursor at 200°C for 3 hours in an oxygen atmosphere, and then keep it at 800°C for 2 hours in a nitrogen atmosphere to obtain a vanadium-based oxide@C composite material. The vanadium-based oxide@C composite material includes vanadium-based oxide and carbon, the mass of the vanadium-based oxide accounts for 83% of the total mass of the composite material; the mass of the carbon accounts for 17% of the total mass of the composite material.

[0095] Using it as an electrode and testing it according to the test method of Test Example 1, at a current density of 0.3A / g, it has a reversible discharge capacity of about 280mAh / g; at a high current density of 5.0A / g, it has a reversible discharge capacity of more than 198mAh / g; at a current density of 3A / g, it retains 88% of the initial capacity after 1000 cycles.

[0096] Example 7

[0097] A vanadium-based oxide@C composite material comprises the following steps:

[0098] Step 1: Use 60 mL of ethanol to disperse 1.0 g of V2O5 powder, add 2.0 g of 1,5-diaminonaphthalene to the V2O5 solution, and then use a magnetic stirrer to stir for 24 hours, then put it into a hydrothermal reactor, hydrotherm at 150°C for 12 hours, filter, wash with excess water, and then dry in a forced air drying oven at 80°C for 24 hours to obtain a precursor;

[0099] Step 2: Keep the precursor at 200°C for 3 hours in an oxygen atmosphere, and then keep it at 500°C for 24 hours in a nitrogen atmosphere to obtain a vanadium-based oxide@C composite material. The vanadium-based oxide@C composite material includes vanadium-based oxide and carbon, the mass of the vanadium-based oxide accounts for 77% of the total mass of the composite material; the mass of the carbon accounts for 23% of the total mass of the composite material.

[0100] Using it as an electrode and testing it according to the test method of Test Example 1, at a current density of 0.3A / g, it has a reversible discharge capacity of about 265mAh / g; at a high current density of 5.0A / g, it has a reversible discharge capacity of more than 167mAh / g; at a current density of 3A / g, it retains 90% of the initial capacity after 1000 cycles.

[0101] Example 8

[0102] A vanadium-based oxide@C composite material comprises the following steps:

[0103] Step 1: Weigh 1.0 g of p-aminobenzenesulfonic acid and 1.0 g of ammonium metavanadate, mix the two, add 60 mL of aqueous solution, and then stir at 80° C. using a magnetic stirrer for 24 h, filter, wash with excess water, and then dry in a forced air drying oven at 80° C. for 24 h to obtain a precursor;

[0104] Step 2: Keep the precursor at 500° C. for 24 hours in a nitrogen / hydrogen mixed atmosphere to obtain a vanadium-based oxide@C composite material. The vanadium-based oxide@C composite material includes vanadium-based oxide and carbon, wherein the mass of the vanadium-based oxide accounts for 74% of the total mass of the composite material; and the mass of the carbon accounts for 26% of the total mass of the composite material.

[0105] Using it as an electrode and testing it according to the test method of Test Example 1, it has a reversible discharge capacity of about 420 mAh / g at a current density of 0.3 A / g; at a high current density of 5.0 A / g, it has a reversible discharge capacity of more than 312 mAh / g; at a current density of 3 A / g, it retains 86% of the initial capacity after 1000 cycles.

[0106] Example 9

[0107] A vanadium-based oxide@C composite material comprises the following steps:

[0108] Step 1: Weigh 1.0g of p-aminobenzoic acid and 1.0g of VCl3, mix the two, add 60mL of ethanol solution, put them into a hydrothermal reactor, hydrothermal at 180°C for 12h, filter, wash with excess water, and dry in a forced air drying oven at 80°C for 24h to obtain a precursor;

[0109] Step 2: Keep the precursor at 500° C. for 24 hours in a nitrogen / hydrogen mixed atmosphere to obtain a vanadium-based oxide@C composite material. The vanadium-based oxide@C composite material includes vanadium-based oxide and carbon, wherein the mass of the vanadium-based oxide accounts for 78% of the total mass of the composite material; and the mass of the carbon accounts for 22% of the total mass of the composite material.

[0110] Using it as an electrode and testing it according to the test method of Test Example 1, at a current density of 0.3A / g, it has a reversible discharge capacity of about 334mAh / g; at a high current density of 5.0A / g, it has a reversible discharge capacity of more than 231mAh / g; at a current density of 3A / g, it retains 83% of the initial capacity after 1000 cycles.

[0111] The above is an explanation of the embodiments of the present invention. However, the present invention is not limited to the above embodiments. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a vanadium-based oxide@C composite material, the method comprising the following steps: (1) mixing a vanadium-based material and an organic molecular monomer, reacting the mixture, and preparing a precursor; (2) subjecting the precursor of step (1) to a polymerization reaction under an oxygen atmosphere, and then carbonizing the polymerization product under an inert atmosphere or a reducing atmosphere; or directly carbonizing the precursor under an inert atmosphere or a reducing atmosphere to obtain the vanadium-based oxide@C composite material.

2. The preparation method according to claim 1, wherein In step (1), the vanadium-based material is selected from one, two or more of vanadium metal, vanadium-based salt or vanadium-based oxide. Preferably, the vanadium-based salt is selected from one, two or more of vanadium chloride, vanadium nitrate, vanadium sulfate, vanadium phosphate, vanadium acetate, vanadium acetylacetonate, ammonium metavanadate, ammonium metavanadate, sodium metavanadate, potassium metavanadate, sodium orthovanadate, vanadyl sulfate, vanadium tetrachloride and vanadium trichloride. Preferably, the vanadium-based oxide is selected from one, two or more of vanadium monoxide, vanadium trioxide, vanadium dioxide and vanadium pentoxide.

3. The preparation method according to claim 1 or 2, wherein In step (1), the organic molecule monomer is selected from linear or branched C1-C18 alkylamines and their derivatives (such as methylamine, ethylamine, propylamine, pentylamine, hexylamine, heptylamine, octylamine, nonylamine, decylamine, undecylamine, dodecylamine, tridecylamine, tetradecylamine, pentadecylamine, hexadecylamine, heptadecanylamine, octadecylamine, isobutylamine, diisobutylamine, N-ethylbutylamine, diisooctylamine, NN dimethyl n-octylamine, etc.), p-phenylenediamine, o-phenylenediamine, m-phenylenediamine, benzidine, 3,3-diaminobenzidine, p-phenylenediamine, o-phenylenediamine, m-phenylenediamine, benzylamine, triphenylamine, diphenylamine, 1,5- One, two or more of diaminonaphthalene, 1,8-diaminonaphthalene, naphthylamine, diaminodiphenylmethane, 3,3',5,5'-tetramethylbenzidine, N-methyl-1,2-phenylenediamine, aniline, dopamine, pyridine, 1-aminopyridine, 2-aminopyridine, 3-aminopyridine, pyrrole, 1-aminopyrrole, 2-aminopyrrole, 3-aminopyrrole, o-aminophenol, p-aminophenol, m-aminophenol, p-aminobenzoic acid, terephthalic acid, isophthalic acid, 3,5-diaminobenzenesulfonic acid, 2,4-diaminobenzoic acid, p-aminophenylboric acid and p-aminophenylphosphoric acid.

4. The preparation method according to any one of claims 1 to 3, wherein: In step (1), the mass ratio of the vanadium-based material to the organic molecular monomer is 1:0.1-6.

5. The preparation method according to any one of claims 1 to 4, wherein: In step (1), the organic molecular monomer and the vanadium-based material may react in the presence of a solvent or in the absence of a solvent. Preferably, the reaction in the absence of solvent is, for example, that the organic molecular monomer and the vanadium-based material are reacted by dry mixing by grinding, ball milling, blender or crusher; such as the organic molecular monomer and the vanadium-based material are dry mixed by grinding, ball milling, blender or crusher until no obvious particles are present. Preferably, the reaction in the presence of a solvent is, for example, mixing the solvent, the organic molecule monomer and the vanadium-based material and reacting them. Preferably, the ratio of the sum of the masses of the vanadium-based material and the organic molecular monomer to the solvent is 1 g: (1-100) mL.

6. The preparation method according to any one of claims 1 to 5, wherein: In step (1), the reaction is carried out at room temperature, under heating conditions, or under high pressure heating conditions; And / or, in step (1), the reaction time is 0.1 to 72 hours; And / or, in step (1), the reaction temperature is 20 to 350°C.

7. The preparation method according to any one of claims 1 to 6, wherein: In step (2), the polymerization reaction temperature is 120° C. to 400° C.; the polymerization reaction time is 0.1 h to 12 h; And / or, in step (2), the temperature of the carbonization treatment is 300° C. to 1200° C.; the time of the carbonization treatment is 0.1 to 24 hours.

8. A vanadium-based oxide@C composite material, wherein the vanadium-based oxide@C composite material is prepared by the above method.

9. The vanadium-based oxide@C composite material according to claim 8, wherein: The vanadium-based oxide@C composite material comprises vanadium-based oxide and carbon, wherein the mass of the vanadium-based oxide accounts for 5-95% of the total mass of the composite material; and the mass of the carbon accounts for 5-95% of the total mass of the composite material. And / or, the vanadium-based oxide@C composite material has a morphology of long strips, flakes, sandwich stacking, core-shell structure or spherical particles. And / or, at least one dimension of the vanadium-based oxide@C composite material is 0.1-50 μm.

10. Application of the vanadium-based oxide@C composite material according to claim 8 or 9 in the field of secondary batteries and supercapacitors. Preferably, the invention is used in lithium ion secondary batteries, sodium ion secondary batteries, potassium ion secondary batteries, zinc ion secondary batteries, such as zinc ion secondary batteries.