Method for preparing water treatment agent through resource utilization of aluminum mud, water treatment agent and application of water treatment agent
Through the reaction of bauxite, aluminum mud and hydrochloric acid and the addition of calcium aluminate, a polymer aluminum chloride water treatment agent containing iron was prepared, which solved the problem of resource utilization of aluminum profile aluminum mud and achieved efficient and low-cost water The production of treatment agents has solved many problems in the prior art.
Patent Information
- Application Number
- CN202411545707.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-01
- Publication Date
- 2024-12-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In the prior art, when producing water treatment agents, aluminum profile aluminum mud has problems such as low content of polymer aluminum chloride, poor filtration performance, high heating energy consumption, complex process flow, high impurity content, heavy metal exceeding standards and high production costs, which is difficult to Realize the utilization of high-purity and low-hybrid resources of aluminum profile aluminum clay.
By mixing bauxite, aluminum mud and hydrochloric acid, a primary liquid of aluminum chloride is generated, and calcium aluminate is added to prepare an iron-containing polymer aluminum chloride water treatment agent. The process is simplified by the room temperature self-reaction heating process. Reduce energy consumption, improve filtration performance and water treatment effect, and reduce impurity content and production costs.
It has achieved the preparation of high-purity and low-mulsion polymer aluminum chloride water treatment agent, with excellent performance, low sulfur and phosphorus impurities, good water treatment effect, low cost, simple and reliable process, industrial production has been achieved, and has broad industrial application prospects .
Smart Images

Figure SMS_1 
Figure SMS_12 
Figure SMS_28
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of resource utilization of aluminum mud, and in particular to a method for preparing a water treatment agent by resource utilization of aluminum mud, the water treatment agent and application thereof. Background Art
[0002] Aluminum profile processing plants produce a large amount of aluminum-containing sludge, referred to as aluminum sludge, when performing surface treatments such as pickling and alkali washing on aluminum surfaces to remove oil stains and oxide films on the aluminum surfaces. The main components of aluminum sludge are ultrafine particles of γ-Al(OH)3 and amorphous Al(OH)3. It has a large specific surface area, high surface activity, and is difficult to dehydrate. After dehydration by a plate and frame filter press, the moisture content is still as high as 70~80%. Therefore, it is very difficult to recycle aluminum sludge.
[0003] At present, there are various problems that need to be solved in the production of water treatment agents using aluminum profiles and aluminum mud, such as: low content of polyaluminum chloride in water treatment agents, multiple filtration of materials during production, poor filtration performance, high heating energy consumption, complex process flow, high content of impurities such as sulfur and phosphorus, excessive heavy metal content, high production costs, and poor performance of water treatment agents.
[0004] Therefore, it is hoped to provide a new preparation method to prepare a high-purity, low-impurity, low-heavy metal content polyaluminium chloride liquid product using aluminium profile aluminium mud as raw material, so as to achieve resource recycling of aluminium profile aluminium mud. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides a method for preparing a water treatment agent by resource utilization of aluminum mud, a water treatment agent and its application. The preparation method of the present invention has a simple and reliable process flow, can be completed by self-reaction heating at room temperature, does not require additional heating, has mild conditions and low energy consumption, and the prepared water treatment agent is an iron-containing polyaluminum chloride water treatment agent with low sulfur and phosphorus impurity content, excellent performance, good water treatment effect, and uses aluminum profile aluminum mud as raw material, realizing the resource utilization of aluminum profile aluminum mud, with low cost, outstanding economic and environmental benefits, and has now achieved industrial production, with broad prospects for industrial application.
[0006] In a first aspect, the present invention provides a method for preparing a water treatment agent by utilizing aluminum mud resources, the method comprising the following steps: (1) mixing bauxite, aluminum mud and hydrochloric acid to obtain a reaction solution, and reacting the reaction solution to obtain a primary aluminum chloride solution; (2) Adding calcium aluminate to the aluminum chloride primary liquid for reaction to obtain the water treatment agent.
[0007] The preparation method provided by the present invention has a simple and reliable process flow, can be completed by self-reaction heating at room temperature, does not require additional heating, has mild conditions, low energy consumption, and uses aluminum profile aluminum mud as raw materials, thus realizing resource utilization of aluminum profile aluminum mud, with low cost and outstanding economic and environmental benefits. Currently, industrial production has been realized, and the industrial application prospects are broad. The prepared water treatment agent is an iron-containing polyaluminum chloride water treatment agent with low sulfur and phosphorus impurity content and excellent performance. Specifically: The present invention uses bauxite as a raw material. On the one hand, it can generate heat by self-reaction during the preparation process, and the temperature of the reaction liquid can be raised to 65-75°C without additional heating. The normal temperature and pressure conditions are mild and the energy consumption is low, which meets the situation that heating cannot be performed in the actual production process. On the other hand, bauxite contains iron, so that the prepared water treatment agent is an iron-containing polyaluminum chloride water treatment agent, which can improve the filterability of the product and optimize the water treatment capacity of the product, and meet people's demand for iron-containing polyaluminum chloride water treatment agent products. Using aluminum profile aluminum mud as a raw material solves the problem of resource utilization of aluminum profile aluminum mud, with low cost and outstanding economic and environmental benefits. At the same time, the introduction of calcium aluminate can finally convert sulfate in aluminum mud into calcium sulfate, realizing the efficient removal of impurities phosphorus and sulfur in the solution, so that the prepared water treatment agent has excellent performance and low sulfur and phosphorus impurity content.
[0008] As a preferred technical solution of the present invention, the bauxite and aluminum mud are added to the hydrochloric acid in sequence and mixed to obtain the reaction solution.
[0009] In the preparation process of the present invention, the order of adding bauxite and aluminum mud must be controlled so that the temperature of the self-reaction exothermic system rises faster. If aluminum mud is added first, the acidity of the system decreases, the temperature rises slowly, and incomplete reaction occurs.
[0010] As a preferred technical solution of the present invention, the basicity of the aluminum chloride primary solution is -15% to 10%, for example, -15%, -10%, -5%, 0%, 5% and 10%.
[0011] As a preferred technical solution of the present invention, the acid content of the aluminum chloride primary solution is 0-1.5%, such as 0%, 0.5%, 1%, 1.5%, etc. The acid content of the aluminum chloride primary solution is determined by a conventional acid-base titration method.
[0012] The present invention adjusts the feed ratio of bauxite, aluminum mud and hydrochloric acid so that the basicity and acid content of the primary aluminum chloride solution are within the range, so as to facilitate subsequent reactions. When the basicity and acid content are not within the range, they can be adjusted by adding an appropriate amount of hydrochloric acid or aluminum mud or bauxite.
[0013] As a preferred technical solution of the present invention, the aluminum mud is selected from aluminum mud produced by aluminum profile processing, wherein the soluble alumina content is 10-25%, for example, 10%, 15%, 20%, 25%, etc., and the attached water content is 50-80%, for example, 50%, 60%, 70%, 80%, etc.
[0014] The aluminum mud provided by the present invention is selected from the aluminum mud produced by aluminum profile processing. The aluminum mud has a high aluminum oxide content and does not need to add other materials (such as aluminum powder, etc.). The use of aluminum mud solves the problem of resource utilization of aluminum profile aluminum mud and has low cost. The prepared water treatment agent can be used for sewage treatment, with outstanding economic and environmental benefits and broad application prospects.
[0015] As a preferred technical solution of the present invention, the mass ratio of the aluminum mud to the hydrochloric acid is 1:(0.9~1.3), for example, 1:0.9, 1:1.0, 1:1.1, 1:1.2, 1:1.3, etc.
[0016] As a preferred technical solution of the present invention, the hydrochloric acid can be industrial hydrochloric acid, and the mass concentration of the hydrochloric acid is 24-33%, for example, 24%, 26%, 28%, 30%, 33%, etc.
[0017] As a preferred technical solution of the present invention, the mass ratio of the bauxite to the aluminum mud is 1:(5-16), for example, 1:5, 1:8, 1:10, 1:12, 1:14, 1:16, etc.
[0018] The invention adjusts the ratio of bauxite, aluminum mud and hydrochloric acid within this range so that the basicity and acid content of the primary aluminum chloride solution are within a suitable range, so as to facilitate subsequent reactions.
[0019] As a preferred technical solution of the present invention, the mass ratio of the hydrochloric acid to the calcium aluminate is 3 to 7:1, for example, 3:1, 4:1, 5:1, 6:1, 7:1, etc.
[0020] As a preferred technical solution of the present invention, the reaction time of step (1) is 3 to 4 hours, for example, 3 hours, 3.5 hours, 4 hours, etc.
[0021] The reaction in step (1) of the present invention does not require additional heating, and the prepared aluminum chloride primary liquid does not need to be filtered, and calcium aluminate powder can be directly added. After the reaction is completed, the water treatment agent prepared has good filtering performance.
[0022] As a preferred technical solution of the present invention, the reaction time of step (2) is 1 to 1.5 h, for example, 1 h, 1.2 h, 1.4 h, 1.5 h, etc.
[0023] After the reaction in step (2) of the present invention is completed, water can be added according to the concentration of the desired product and the amount of water added can be adjusted according to the actual situation. After filtering, the water treatment agent can be obtained. At the same time, the filter residue obtained by filtering can be used as a raw material for making bricks, pottery or building materials.
[0024] In a second aspect, the present invention provides a water treatment agent, which is prepared by the method described in the first aspect.
[0025] The water treatment agent provided by the invention is an iron-containing polyaluminium chloride water treatment agent, which has excellent performance, low sulfur and phosphorus impurity content, low cost and good water treatment effect.
[0026] As a preferred technical solution of the present invention, the aluminum oxide content in the water treatment agent is 8-12%, the basicity is 50-75%, and the insoluble matter content is less than 0.3%.
[0027] In a third aspect, the present invention provides use of the water treatment agent described in the second aspect in sewage treatment.
[0028] The technical solution provided by the embodiment of the present invention has the following advantages compared with the prior art: The preparation method of the present invention has a simple and reliable process flow, can be completed by self-reaction heating at room temperature, does not require additional heating, has mild conditions and low energy consumption, and the prepared water treatment agent is an iron-containing polyaluminum chloride water treatment agent with low sulfur and phosphorus impurity content, excellent performance and good water treatment effect. In addition, aluminum profile aluminum mud is used as raw material, thus realizing resource utilization of aluminum profile aluminum mud, with low cost and outstanding economic and environmental benefits. Industrial production has been achieved at present, and the industrial application prospect is broad. DETAILED DESCRIPTION
[0029] In order to more clearly understand the above-mentioned objectives, features and advantages of the present invention, the scheme of the present invention will be further described below. It should be noted that the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.
[0030] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein; it is obvious that the embodiments in the specification are only part of the embodiments of the present invention, rather than all of the embodiments.
[0031] Example 1 This embodiment provides a water treatment agent and a preparation method thereof, the preparation method comprising the following steps: Aluminum mud is the aluminum mud filter cake from the aluminum profile processing plant, in which the soluble aluminum oxide content is 12.14%, the attached water content is 78%, and the mass concentration of hydrochloric acid is 26.3%; The materials are added in a mass ratio of 13:1:13:2 among hydrochloric acid, bauxite, aluminum mud and calcium aluminate. First, hydrochloric acid is added to the reactor, then bauxite is added, and then aluminum mud is added. The reaction is carried out for 3 hours to obtain a primary aluminum chloride liquid. The basicity of the primary liquid is adjusted to -15~10%, and the acid content is 0~1.5%. Calcium aluminate powder is added to the primary liquid, and the reaction is carried out for 1.5 hours. The water treatment agent product is obtained after filtering through a plate and frame filter press.
[0032] Example 2 This embodiment provides a water treatment agent and a preparation method thereof, the preparation method comprising the following steps: Aluminum mud is the aluminum mud filter cake from the aluminum profile processing plant, in which the soluble aluminum oxide content is 12.14%, the attached water content is 78%, and the mass concentration of hydrochloric acid is 26.3%; The materials are added in a mass ratio of 13:1:13:3 among hydrochloric acid, bauxite, aluminum mud and calcium aluminate. First, hydrochloric acid is added to the reactor, then bauxite is added first, and then aluminum mud is added. After reacting for 3 hours, aluminum chloride primary liquid is obtained. The basicity of the primary liquid is adjusted to -15~10%, and the acid content is 0~1.5%. Calcium aluminate powder is added to the primary liquid, reacted for 1.5 hours, and filtered through a plate and frame filter press to obtain the water treatment agent product.
[0033] Example 3 This embodiment provides a water treatment agent and a preparation method thereof, the preparation method comprising the following steps: Aluminum mud is the aluminum mud filter cake from the aluminum profile processing plant, in which the soluble aluminum oxide content is 10.56%, the attached water content is 80%, and the mass concentration of hydrochloric acid is 30.1%; The materials are added in a mass ratio of hydrochloric acid, bauxite, aluminum mud and calcium aluminate of 13:1:16:3. First, hydrochloric acid is added to the reactor, then bauxite is added first, and then aluminum mud is added. The reaction is carried out for 3 hours to obtain the primary aluminum chloride liquid. The basicity of the primary liquid is adjusted to -15~10%, and the acid content is 0~1.5%. Calcium aluminate powder is added to the primary liquid, and the reaction is carried out for 1.5 hours. After filtering through a plate and frame filter press, the water treatment agent product is obtained.
[0034] Example 4 This embodiment provides a water treatment agent and a preparation method thereof, the preparation method comprising the following steps: The aluminum sludge is aluminum sludge filter cakes A and B from an aluminum profile processing plant, where the soluble aluminum oxide content of aluminum sludge filter cake A is 10.56% and the attached water content is 80%; the soluble aluminum oxide content of aluminum sludge filter cake B is 12.14% and the attached water content is 78%; the mass concentration of hydrochloric acid is 30.1%; The mass ratio of hydrochloric acid, bauxite, aluminum mud A, aluminum mud B, and calcium aluminate is 13:1:10.5:5:3. First, add hydrochloric acid to the reactor, then add bauxite, then add aluminum mud, react for 3 hours, and obtain aluminum chloride primary liquid. Adjust the primary liquid basicity to -15~10%, and the acid content to 0~1.5%. Add calcium aluminate powder to the primary liquid, react for 1.5 hours, and filter through a plate and frame filter press to obtain a water treatment agent product.
[0035] Example 5 This embodiment provides a water treatment agent and a preparation method thereof, the preparation method comprising the following steps: Aluminum mud is the aluminum mud filter cake from the aluminum profile processing plant, in which the soluble aluminum oxide content is 12.14%, the attached water content is 78%, and the mass concentration of hydrochloric acid is 28.5%; The mass ratio of hydrochloric acid, bauxite, aluminum mud and calcium aluminate is 10.5:2:10:3. First, add hydrochloric acid to the reactor, then add bauxite, then add aluminum mud, react for 3 hours, and obtain the primary aluminum chloride liquid. Adjust the primary liquid salt base degree to -15~10%, and the acid content to 0~1.5%. Add calcium aluminate powder to the primary liquid, react for 1.5 hours, and filter through a plate and frame filter press to obtain the water treatment agent product.
[0036] Example 6 This embodiment provides a water treatment agent and a preparation method thereof, the preparation method comprising the following steps: The aluminum sludge is aluminum sludge filter cakes A and B from an aluminum profile processing plant, where the soluble aluminum oxide content of aluminum sludge filter cake A is 12.14% and the attached water content is 78%; the soluble aluminum oxide content of aluminum sludge filter cake B is 20.16% and the attached water content is 55%; the mass concentration of hydrochloric acid is 28.5%; The mass ratio of hydrochloric acid, bauxite, aluminum mud A, aluminum mud B, and calcium aluminate is 15:1:12:2:3. First, add hydrochloric acid to the reactor, then add bauxite, then aluminum mud, and react for 3 hours to obtain aluminum chloride primary liquid. Adjust the primary liquid salt base degree to -15~10%, and the acid content to 0~1.5%. Add calcium aluminate powder to the primary liquid, react for 1.5 hours, and filter through a plate and frame filter press to obtain a water treatment agent product.
[0037] Example 7 This embodiment provides a water treatment agent and a preparation method thereof. The preparation method is the same as that of Example 1. The difference from Example 1 is that the content of soluble alumina in the aluminum mud in this embodiment is 7%.
[0038] Example 8 This embodiment provides a water treatment agent and a preparation method thereof. The preparation method is the same as that of Example 1. The difference from Example 1 is that in this embodiment, the order of adding aluminum mud and bauxite is reversed, that is, aluminum mud is added first, and then bauxite is added.
[0039] The results showed that by changing the order of adding aluminum mud and bauxite, the temperature of the reaction liquid rose slowly and could not reach 65°C, and the obtained aluminum chloride primary liquid did not react completely.
[0040] Example 9 This embodiment provides a water treatment agent and a preparation method thereof. The preparation method is the same as that of Example 1. The difference from Example 1 is that in this embodiment, the basicity of the aluminum chloride primary liquid is adjusted to 20% and the acid content is 2%.
[0041] The results show that if the basicity and acid content of the primary aluminum chloride solution are not within the range of the present invention, the prepared water treatment agent cannot be filtered by a plate and frame filter press.
[0042] Performance Testing The water treatment agents prepared in the examples were tested respectively: 1. Determination of alumina content 1.1 Method Summary The sample was depolymerized with nitric acid, and when the pH value was about 3, an excess of disodium ethylenediaminetetraacetate solution was added to make it complex with aluminum ions. With xylenol orange as an indicator, the excess disodium ethylenediaminetetraacetate solution was back-titrated with a standard zinc chloride titration solution.
[0043] 1.2 Analysis steps: Weigh about 8 g of liquid sample or 2.5 g of solid sample to an accuracy of 0.2 g. Dissolve it with deionized water, transfer it into a 250 mL volumetric flask, dilute to the mark, and shake well. The supernatant is sample A.
[0044] Pipette 10 mL of sample A solution and place it in a 250 mL conical flask. Add 10 mL of nitric acid solution and boil for one minute. After cooling to room temperature, add 20 mL of EDTA, add 3-4 drops of thymol blue solution, neutralize with ammonia solution until the solution changes from red to yellow, and boil for two minutes. After cooling, add 10 mL of acetic acid-sodium acetate buffer solution and 2 drops of xylenol orange indicator, add 50 mL of water, and titrate with zinc chloride standard solution until the solution changes from light yellow to slightly red. At the same time, make a blank.
[0045] 1.3. Calculation of results:
[0046] In the formula : Blank volume of zinc chloride consumed, mL; : Volume of zinc chloride consumed by the sample, mL; : Concentration of zinc chloride titration solution, mol / L; : mass of the sample, g; : Molar mass of aluminum oxide, g / moL ( =101.96); : Volume of sample A removed, mL ( =5); : Total volume of sample A, mL, ( =250).
[0047] 2. Determination of basicity content 2.1 Method Summary Add excess hydrochloric acid solution to the sample, use potassium fluoride to mask aluminum ions and iron ions, and back-titrate the excess hydrochloric acid solution with a standard sodium hydroxide solution.
[0048] 2.2 Analysis steps Take 25 mL of water treatment agent (test solution A) and place it in a 250 mL conical flask. Add 20 mL of hydrochloric acid standard solution, cover with a watch glass, heat on an electric stove until boiling, then remove immediately and cool to room temperature. Add 20 mL of potassium fluoride solution, shake well, add five drops of phenolphthalein indicator solution, and immediately titrate with sodium hydroxide standard titration solution until the solution turns slightly red, which is the end point. At the same time, use water without carbon dioxide for a blank test.
[0049] 2.3. Calculation of results:
[0050] Where: -The volume of sodium hydroxide standard titration solution consumed in the blank test (mL); -The volume of sodium hydroxide standard titration solution consumed by the sample, (mL); -The exact value of the actual concentration of the sodium hydroxide standard titration solution (mol / L); - numerical value of the molar mass of hydroxide, (g / mol), ( =16.99); - numerical value of the mass of the sample, (g); -The mass fraction of aluminum oxide measured above, %; -The volume of test solution A pipetted, (mL), ( =25); -The total volume of test solution A, (mL), ( =250); - numerical value of the molar mass of aluminum, (g / mol), ( =26.98); - numerical value of the molar mass of aluminum oxide, (g / mol), ( =101.96).
[0051] 3. Determination of P and S content: 3.1 Determination of phosphorus content 3.1.1 Sample pretreatment (1) Take 12.5 mL of water treatment agent (if necessary, take less and add water to 12.5 mL so that the phosphorus content does not exceed 30 μg) in a 25 mL stoppered tube, add 2 mL of 5% potassium persulfate, wrap a small piece of gauze around the tube mouth after stoppering and tie it tightly with cotton thread to prevent the glass stopper from rushing out during heating. Place the stoppered tube in a large beaker, heat it in an autoclave, digest it at 120℃ for 30 minutes, take it out and let it cool, add water to make up to 25.0 mL (if the solution is turbid, filter it).
[0052] (2) The reagent blank and standard solution series are also subjected to the same digestion operation.
[0053] 3.1.2 Sample determination (1) Drawing of standard curve Prepare a 2.00 μg / mL standard solution by taking 0 mL, 0.25 mL, 0.5 mL, 1.5 mL, 2.5 mL, 5 mL, and 7.5 mL of the above solution and adding water to make up to 25 mL; (2) Color development: Add 0.5 mL of 10% ascorbic acid solution to the colorimetric tube and mix well. After 30 seconds, add 1 mL of molybdate solution and mix well. Let stand for 15 minutes.
[0054] (3) Measurement: Use 10 mm and 30 mm cuvettes to measure the absorbance at 700 nm with zero concentration solution as reference.
[0055] 3.1.3 Calculation Total phosphorus (P, mg / L) = 10M × 0.001 Where, M-phosphate concentration found from the directrix curve (µg / L); 10-dilution factor.
[0056] 3.2 Determination of sulfur content The determination was carried out using the methylene blue spectrophotometric method HJ 1226-2021.
[0057] The results of the alumina content, basicity, P content, S content, insoluble matter content and pH in each water treatment agent are shown in Table 1: Table 1
[0058] It can be found from Table 1 that the water treatment agent prepared by the present invention has an aluminum oxide content of 8-12%, a basicity of 50%-75%, low sulfur and phosphorus contents, insoluble matter <0.3%, a pH (10 g / L solution) of 4-4.5, excellent performance indicators, and good water treatment effect.
[0059] From the comparison between Example 1 and Example 7, it can be found that if the aluminum oxide content in the aluminum mud is too low, the aluminum oxide index in the prepared water treatment agent is low, lower than the national standard, and the product is unqualified.
[0060] It should be noted that, in this article, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.
[0061] The above description is only a specific embodiment of the present invention, so that those skilled in the art can understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments described herein, but should conform to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing a water treatment agent by resource utilization of aluminum mud, characterized in that: The method comprises the following steps: (1) mixing bauxite, aluminum mud and hydrochloric acid to obtain a reaction solution, and reacting the reaction solution to obtain a primary aluminum chloride solution; (2) Adding calcium aluminate to the aluminum chloride primary liquid for reaction to obtain the water treatment agent.
2. The method according to claim 1, characterized in that The bauxite and aluminum mud are added to the hydrochloric acid in sequence and mixed to obtain the reaction solution.
3. The method according to claim 1 or 2, characterized in that: The basicity of the aluminum chloride primary solution is -15~10%; And / or, the acid content of the aluminum chloride primary solution is 0-1.5%.
4. The method according to claim 1 or 2, characterized in that: The aluminum mud is selected from aluminum mud produced by aluminum profile processing, wherein the soluble aluminum oxide content is 10-25% and the attached water content is 50-80%.
5. The method according to claim 1 or 2, characterized in that: The mass ratio of the aluminum mud to the hydrochloric acid is 1:(0.9-1.3); And / or, the mass concentration of the hydrochloric acid is 24-33%.
6. The method according to claim 1 or 2, characterized in that: The mass ratio of the bauxite to the aluminum mud is 1:(5-16).
7. The method according to claim 1 or 2, characterized in that: The mass ratio of the hydrochloric acid to the calcium aluminate is 3-7:
1.
8. The method according to claim 1 or 2, characterized in that: The reaction time of step (1) is 3 to 4 hours; And / or, the reaction time of step (2) is 1 to 1.5 h.
9. A water treatment agent, characterized in that: The water treatment agent is prepared by the method according to any one of claims 1 to 8.
10. Use of the water treatment agent according to claim 9 in sewage treatment.
Citation Information
Patent Citations
Method for preparing polyaluminium chloride water purifying agent from aluminum residues
CN107265581A
Method for preparing polyaluminum chloride from aluminum profile aluminum mud
CN117945445A
Cited By
Method for preparing sludge conditioner through resource utilization of aluminum sludge and sludge conditioner
CN119504114A
Method for preparing sludge conditioner from aluminum mud resources and sludge conditioner
CN119504114B