Preparation method of flaky hydroxyl cobalt oxide
By reacting the cobalt solution with complexing agent and alkali solution under normal temperature and pressure, a sheet-like cobalt hydroxyl oxide with a high specific surface area was prepared, which solved the problem of insufficient performance of traditional block materials and improved electrochemical performance and catalytic activity. , reduces preparation cost and energy consumption.
Patent Information
- Application Number
- CN202411103235.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-12-03
AI Technical Summary
The surface area of traditional bulk cobalt hydroxyoxide materials is low, which limits its electrochemical properties and has problems such as insufficient reactive activity and poor structural stability in catalytic applications.
By reacting the cobalt solution with complexing agent and alkali solution under normal temperature and pressure, aging, filtration, washing and drying, a sheet-like cobalt hydroxyl oxide with a higher specific surface area than the traditional method is prepared to control cobalt ions and The molar ratio, reaction pH and flow rate of the complexing agent are used to improve the sheet dispersion and reactivity of the product.
The specific surface area of sheet-shaped cobalt hydroxyoxide is achieved above 63m2/g, which improves electrochemical performance and catalytic activity, reduces preparation energy consumption and cost, is simple to operate and mild conditions.
Smart Images

Figure CN119059574A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of cobalt material preparation, and in particular to a method for preparing flaky cobalt oxyhydroxide. Background Art
[0002] Cobalt oxyhydroxide (CoOOH) is a transition metal oxide that is widely used in electrochemical energy storage, catalysis, and optoelectronic devices, and has important application potential. Its excellent conductivity, catalytic activity, and chemical stability make it outstanding in water splitting, lithium-ion batteries, and supercapacitors.
[0003] At present, cobalt oxyhydroxide is commonly found in block and flake structures. Among them, the traditional block cobalt oxyhydroxide material usually has a low specific surface area (less than 30m 2 / g), which limits its electrochemical performance. At the same time, in catalytic applications, the traditional cobalt oxyhydroxide has the problems of insufficient reaction activity and poor structural stability. The sheet-like cobalt oxyhydroxide, due to its high specific surface area and unique two-dimensional structure, can provide more active sites, improve charge transfer efficiency and reaction rate. Therefore, it is particularly important to study how to prepare sheet-like cobalt oxyhydroxide at low cost and low energy consumption. Summary of the invention
[0004] In view of the shortcomings of the above-mentioned related technologies, the present application provides a method for preparing flaky cobalt hydroxide oxide. The flaky cobalt hydroxide oxide is obtained by reacting a cobalt solution, a complexing agent and an alkaline solution at room temperature and pressure, and then aging, filtering, washing and drying. The flaky cobalt hydroxide oxide has distinct layers and good dispersion, and the specific surface area reaches 63m 2 / g or more, the preparation process is simple to operate, the conditions are mild, and the energy consumption and cost of preparation are reduced.
[0005] The present application provides a method for preparing flaky cobalt oxyhydroxide using the following technical solution: A method for preparing flaky cobalt oxyhydroxide comprises the following steps: preparing a cobalt solution and an alkaline solution, mixing the cobalt solution with a complexing agent to obtain a mixed solution; adding a base solution into a reaction container and adjusting the pH to 10-12, flowing the mixed solution and the alkaline solution into the reaction container in parallel to react for 30-60 minutes and then aging, and finally filtering, washing and drying to obtain the flaky cobalt oxyhydroxide.
[0006] Preferably, the method comprises the following steps: preparing a cobalt solution and an alkaline solution, mixing the cobalt solution with a complexing agent to obtain a mixed solution; adding a base solution to a reaction container and adjusting the pH to 11, flowing the mixed solution and the alkaline solution into the reaction container in parallel to react for 40 minutes and then aging, and finally filtering, washing and drying to obtain the flaky cobalt hydroxide oxide.
[0007] Preferably, the cobalt ion concentration in the cobalt solution is 1-2 mol / L.
[0008] Preferably, the cobalt ion concentration in the cobalt solution is 2 mol / L.
[0009] Preferably, the cobalt solution is made of one or more of cobalt chloride, cobalt sulfate and cobalt nitrate.
[0010] Preferably, the cobalt solution is made of cobalt chloride.
[0011] Preferably, in the mixed solution, the concentration of the complexing agent is 0.005-0.01 mol / L.
[0012] Preferably, in the mixed solution, the concentration of the complexing agent is 0.008 mol / L.
[0013] Preferably, the complexing agent includes one or both of disodium ethylenediaminetetraacetate and ethylenediaminetetraacetic acid.
[0014] Preferably, the complexing agent is disodium ethylenediaminetetraacetate.
[0015] Preferably, in the mixed solution, the molar ratio of the complexing agent to the cobalt ions is 1:100-400.
[0016] Preferably, in the mixed solution, the molar ratio of the complexing agent to the cobalt ions is 1:250.
[0017] Preferably, the alkaline solution is made of one or both of sodium hydroxide and potassium hydroxide.
[0018] Preferably, the alkaline solution is a sodium hydroxide solution.
[0019] Preferably, the concentration of the alkaline solution is 8-11 mol / L.
[0020] Preferably, the concentration of the alkaline solution is 10 mol / L.
[0021] Preferably, during the reaction, the flow rate of the mixed solution is 40-60 g / min, and the reaction pH is 10.5-11.5.
[0022] Preferably, during the reaction, the flow rate of the mixed solution is 48 g / min and the reaction pH is 11.
[0023] Preferably, the specific surface area of the flaky cobalt oxyhydroxide is 60-90 m 2 / g.
[0024] In summary, the present application includes at least one of the following beneficial technical effects: 1. The present invention uses a cobalt solution, a complexing agent and an alkaline solution to react under normal temperature and pressure, and then obtains flaky cobalt hydroxide oxide by aging, filter pressing, washing and drying. The flaky cobalt hydroxide oxide has distinct layers and good dispersibility. The preparation process is simple to operate and the conditions are mild, which reduces the energy consumption and cost of the preparation. 2. The morphology of the product is controlled by controlling the molar ratio of cobalt ions and complexing agent, and the specific surface area of the obtained flaky cobalt hydroxide oxide reaches 63m 2 / g or more, increasing the specific surface area of flaky cobalt oxyhydroxide; 3. By controlling the flow rate of the cobalt solution and the pH of the reaction, the reaction activity is improved. Combined with the complexing agent, the cobalt hydroxide oxide prepared under the comprehensive effect is in the form of flakes. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 is a scanning electron microscope image of the flaky cobalt oxyhydroxide prepared by the preparation method of Example 1; Figure 2 is a scanning electron microscope image of the flaky cobalt oxyhydroxide prepared by the preparation method of Example 2; Figure 3 is a scanning electron microscope image of the flake cobalt oxyhydroxide prepared by the preparation method of Example 3; Figure 4 is a scanning electron microscope image of the flake cobalt oxyhydroxide prepared by the preparation method of Comparative Example 1; Figure 5 is a scanning electron microscope image of the flake cobalt oxyhydroxide prepared by the preparation method of Comparative Example 2; Figure 6 is a scanning electron microscope image of the flake cobalt oxyhydroxide prepared by the preparation method of Comparative Example 3; Figure 7 This is a scanning electron microscope image of the flaky cobalt hydroxide oxide prepared by the preparation method of Comparative Example 4. DETAILED DESCRIPTION
[0026] The present application is further described in detail below in conjunction with examples. The following examples are only used to illustrate the present invention and should not be construed as limiting the scope of the present invention. In the following examples, if specific conditions are not specified, they are carried out according to normal conditions or conditions recommended by the manufacturer. The methods used are conventional methods known in the art unless otherwise specified, and the consumables and reagents used are commercially available unless otherwise specified. Unless otherwise specified, the professional and scientific terms used herein have the same meaning as those familiar to those skilled in the art. In addition, any method or material similar or equivalent to the recorded content may also be applied to the present invention.
[0027] The raw materials used in the examples and comparative examples can all be obtained commercially.
[0028] Example 1 Example 1 of the present application provides a method for preparing flaky cobalt oxyhydroxy, and the specific steps are as follows: taking cobalt chloride to prepare a cobalt solution with a cobalt ion concentration of 1 mol / L, adding disodium ethylenediaminetetraacetate to the cobalt solution and stirring evenly to obtain a mixed solution with a concentration of disodium ethylenediaminetetraacetate of 0.008 mol / L, and preparing a 10 mol / L sodium hydroxide solution; adding 24 L of pure water as a base liquid into a 50 L reactor, stirring is started at a speed of 600 r / min, adding sodium hydroxide solution to the base liquid, adjusting the pH to 11, and then flowing the mixed liquid in parallel to react with NaOH solution, the flow rate of the mixed liquid is 48 g / min, and the reaction pH is controlled to be 11±0.05 by controlling the flow rate of NaOH solution, and the reaction is carried out for 40 minutes; after the reaction is completed, stirring is stopped, aging is carried out for one hour, and then pressure filtration, washing, and drying at 80° C. are obtained. flaky cobalt oxyhydroxy
[0029] In this embodiment, disodium ethylenediaminetetraacetate is a complexing agent.
[0030] Example 2 Example 2 of the present application provides a method for preparing flaky cobalt hydroxide oxide. The difference between Example 2 and Example 1 is that the concentration of cobalt ions in the cobalt solution in Example 2 is 2 mol / L, and the concentration of disodium ethylenediaminetetraacetate is 0.01 mol / L.
[0031] Example 3 Example 3 of the present application provides a method for preparing flaky cobalt hydroxide oxide. The difference between Example 3 and Example 1 is that the flow rate of the mixed liquid during the reaction process of Example 3 is 60 g / min.
[0032] Comparative Example 1 Comparative Example 1 provides a method for preparing flaky cobalt oxyhydroxide. The difference between Comparative Example 1 and Example 1 is that in Comparative Example 1, no complexing agent is added to the cobalt solution.
[0033] Comparative Example 2 Comparative Example 2 provides a method for preparing flaky cobalt oxyhydroxide. The difference between Comparative Example 2 and Example 1 is that the concentration of disodium ethylenediaminetetraacetate in the mixed solution prepared in Comparative Example 2 is 0.001 mol / L.
[0034] Comparative Example 3 Comparative Example 3 provides a method for preparing flaky cobalt oxyhydroxide. The difference between Comparative Example 3 and Example 1 is that the concentration of disodium ethylenediaminetetraacetate in the mixed solution prepared in Comparative Example 3 is 0.02 mol / L.
[0035] Comparative Example 4 Comparative Example 4 provides a method for preparing flaky cobalt hydroxide oxide. The difference between Comparative Example 4 and Example 1 is that in Comparative Example 4, when preparing the mixed solution, nitrilotriacetic acid is used instead of disodium ethylenediaminetetraacetate.
[0036] Test and Inspection (1) The specific surface area was measured by a static nitrogen adsorption method. The specific surface areas of the flaky cobalt oxyhydroxide prepared by the preparation methods of Examples 1-3 and Comparative Examples 1-4 were measured, as shown in Table 1 below.
[0037] Table 1:
[0038] (2) Scanning electron microscope imaging was performed on the flake cobalt oxyhydroxide prepared by the preparation methods of Examples 1-3 and Comparative Examples 1-4. Figure 1-7 shown.
[0039] Results Analysis The following combines Table 1 and Figure 1-7 The experimental data provided are used to explain this application in detail.
[0040] Referring to Table 1, the specific surface area of the flaky cobalt oxyhydroxide obtained by the preparation method of Examples 1-3 reaches 63 m 2 / g or above, refer to Figure 1-3 In the scanning electron microscope images of the flaky cobalt hydroxide oxide prepared by the preparation methods of Examples 1-3, the cobalt hydroxide oxide is in a lamellar structure, has no particle structure, and has no agglomeration phenomenon. The lamellar structure dispersion of the flaky cobalt hydroxide oxide prepared by the preparation method of Example 1 is higher than that of the flaky cobalt hydroxide oxide prepared by the preparation methods of Examples 2-3, indicating that controlling the molar ratio of the cobalt ion concentration to the complexing agent to be 1:250 and the flow rate of the mixed solution to be 48 g / min during the production process is conducive to improving the dispersion of the flaky cobalt hydroxide oxide flaky structure.
[0041] Taking Example 1 as a control, Comparative Examples 1-3 show the effects of not adding a complexing agent, adding too little complexing agent, or adding too much complexing agent on the morphology and specific surface area of the prepared cobalt hydroxide oxide in the process of preparing the flaky cobalt hydroxide oxide. Figure 4-6 It can be seen that in the scanning electron microscope image of the cobalt oxyhydroxide prepared when no complexing agent is added, the complexing agent content is too little or the complexing agent content is too high in the process of preparing the flaky cobalt oxyhydroxide, the flaky structure and the block structure of the cobalt oxyhydroxide coexist, and the purity of the flaky structure is low. Referring to Table 1, the specific surface area of the cobalt oxyhydroxide prepared by the preparation methods of Comparative Examples 1 and 2 is only 31m 2 / g and 35m 2 / g, and when the amount of complexing agent added in the preparation of flake cobalt hydroxide is too high, the specific surface area is only 51m 2 / g, which is much smaller than the specific surface area of the flaky cobalt oxyhydroxide prepared by the preparation method of Example 1. It shows that controlling the addition amount of the complexing agent to 0.005-0.01 mol / L is beneficial to improving the purity of the flaky structure in the prepared flaky cobalt oxyhydroxide and increasing the specific surface area of the prepared flaky cobalt oxyhydroxide.
[0042] Taking Example 1 as a control, Comparative Example 4 shows the effect of using other types of complexing agents on the morphology of the prepared cobalt hydroxide oxide in the process of preparing the flaky cobalt hydroxide oxide. Figure 7 It can be seen that when the complexing agent used in the preparation process is nitrilotriacetic acid, the prepared cobalt hydroxide oxide is still in the form of flakes, and the specific surface area reaches 66m 2 / g, but the flake structures are mutually adhered and agglomerated seriously. This indicates that when preparing flake cobalt oxyhydroxide, using disodium ethylenediaminetetraacetate as a complexing agent is beneficial to increasing the specific surface area of the obtained flake cobalt oxyhydroxide while reducing the agglomeration degree of the flake structure in the flake cobalt oxyhydroxide.
[0043] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A method for preparing flaky cobalt oxyhydroxide, characterized in that: The following steps are involved: A cobalt solution and an alkaline solution are prepared, and the cobalt solution is mixed with a complexing agent to obtain a mixed solution; a base solution is added to a reaction container, and the pH value is adjusted to 10-12, and the mixed solution and the alkaline solution are simultaneously introduced into the reaction container to react for 30-60 minutes and then aged, and finally filter pressed, washed, and dried to obtain the flaky cobalt hydroxide oxide.
2. The method for preparing a flaky cobalt oxyhydroxide according to claim 1, characterized in that: The cobalt ion concentration in the cobalt solution is 1-2 mol / L.
3. The method for preparing a flaky cobalt oxyhydroxide according to claim 1, characterized in that: The cobalt solution is made of one or more of cobalt chloride, cobalt sulfate and cobalt nitrate.
4. The method for preparing flaky cobalt oxyhydroxide according to claim 1, characterized in that: In the mixed solution, the concentration of the complexing agent is 0.005-0.01 mol / L.
5. The method for preparing flaky cobalt oxyhydroxide according to claim 1, characterized in that: The complexing agent includes one or both of disodium ethylenediaminetetraacetic acid and ethylenediaminetetraacetic acid.
6. The method for preparing flaky cobalt oxyhydroxide according to claim 1, characterized in that: In the mixed solution, the molar ratio of the complexing agent to the cobalt ions is 1:100-400.
7. The method for preparing flaky cobalt oxyhydroxide according to claim 1, characterized in that: The alkaline solution is made of one or both of sodium hydroxide and potassium hydroxide.
8. The method for preparing flaky cobalt oxyhydroxide according to claim 1, characterized in that: The concentration of the alkaline solution is 8-11 mol / L.
9. The method for preparing flaky cobalt oxyhydroxide according to claim 1, characterized in that: During the reaction, the flow rate of the mixed solution is 40-60 g / min, and the reaction pH is 10.5-11.