Polyvinyl alcohol-nanocellulose crystal composite hydrogel interface evaporator as well as preparation method and application thereof
Through the combination of polyvinyl alcohol-nanocellulose crystal composite hydrogel and reduced graphene oxide, the problems of insufficient mechanical strength, seawater desalination and wastewater purification performance in the prior art are solved, and efficient seawater desalination and Wastewater purification and improves the efficiency of light and heat conversion.
Patent Information
- Application Number
- CN202411285427.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-12-03
AI Technical Summary
The existing hydrogel interface evaporators are difficult to have excellent mechanical strength, seawater desalination performance and wastewater purification performance, and there are shortcomings in the photothermal conversion efficiency.
Using polyvinyl alcohol-nanocellulose crystal composite hydrogel, reducing graphene oxide (rGO) was introduced through nanocomposite strategy, combined with PVA and CNC, an interface evaporator with wide spectrum absorption, excellent mechanical strength and salt resistance was prepared. .
The multifunctionality of polyvinyl alcohol-nanocellulose crystal composite hydrogel interface evaporator is realized, with efficient seawater desalination and wastewater purification performance, and the photothermal conversion efficiency is improved through wide spectrum absorption.
Smart Images

Figure CN119059595A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of solar interface evaporation materials, and in particular relates to a polyvinyl alcohol-nano cellulose crystal composite hydrogel interface evaporator and a preparation method and application thereof. Background Art
[0002] The scarcity of fresh water resources and the energy crisis have seriously affected the sustainable development of human society. Only 2.5% of the fresh water resources on the earth are available. According to statistics, 2.4 billion people in the world face serious water shortages all year round. With the increase in population, climate change and freshwater pollution, nearly 80% of the world's population is facing a high level of water security threats. To solve this problem, an environmentally friendly, efficient and fast method of fresh water production is urgently needed. Solar energy has become an advanced technology for seawater desalination and sewage treatment. However, solar fresh water production requires a lot of energy input. Therefore, it is urgent to develop an interfacial evaporation material that can be used in conjunction with a light absorbing material to improve the solar thermal conversion efficiency and increase the evaporation efficiency.
[0003] Hydrogel is a functional material with a three-dimensional network structure that is rich in water due to the cross-linking of polymer molecular chains under physical or chemical effects. The physicochemical properties of hydrogels can be well adjusted according to the diversity of polymer networks, cross-linking sites and preparation methods. In addition, the hydrophilic polymer network of hydrogels gives them excellent water absorption capacity, which makes hydrogels a suitable choice for interfacial evaporants. Hydrogels also have a porous structure that facilitates the transmission of water to the evaporation surface. When used in combination with light-absorbing materials, this structure can convert the absorption of sunlight into heat energy, thereby promoting water evaporation. The hydrogel polymer network captures water molecules simultaneously through electrostatic effects and hydrogen bonds, regulates the hydrogen bond network and intermolecular forces inside the hydrogel, thereby adjusting the state and phase change behavior of water, and then reducing the evaporation enthalpy of water.
[0004] Cellulose is one of the most abundant, renewable and biodegradable natural polymers. Cellulose nanocrystals (CNC) prepared from cellulose have abundant hydroxyl groups, which can form hydrogen bonds with a variety of molecules, providing abundant attachment sites for light-absorbing materials. CNC can be used as a reinforcing agent and rheological regulator through surface modification to improve the mechanical properties of hydrogels. Although there are many composite hydrogel interface evaporators at present, it is difficult to simultaneously meet the requirements of excellent mechanical strength, seawater desalination performance and wastewater purification performance. Summary of the invention
[0005] In view of the fact that the existing hydrogel interfacial evaporator is difficult to have multifunctional characteristics, its application scope is limited. In order to solve the above problems, the present invention develops a CNC composite hydrogel with excellent mechanical strength, seawater desalination performance and wastewater purification performance. In addition, after introducing photothermal material reduced graphene oxide (rGO) composite through nanocomposite strategy, the composite hydrogel interfacial evaporator can be endowed with wide spectrum absorption (250-2500nm) performance.
[0006] The first aspect of the present invention is to provide a method for preparing a polyvinyl alcohol-nanocellulose crystal composite hydrogel interface evaporator, comprising the following steps:
[0007] Nanocrystalline cellulose, polyvinyl alcohol, and acid solution are added to water and mixed, and heated to dissolve the polyvinyl alcohol to obtain a hydrogel precursor solution; preferably, the acid solution is hydrochloric acid; the heating temperature is 95°C; the concentration of PVA in the hydrogel precursor solution is 8-12%, preferably 10%, and the role of PVA is to make the composite hydrogel have a certain mechanical strength; the concentration of nanocrystalline cellulose is 0.15wt%-0.5wt%; the nanocrystalline cellulose is configured into a solution of a certain concentration before use, and then emulsified, mixed and used. Further preferably, the emulsification treatment conditions are: emulsification at room temperature and 12000rpm for 30 minutes; the purpose of the emulsification treatment is to make the nanocrystalline cellulose uniformly dispersed in water.
[0008] Add reduced graphene oxide and a cross-linking agent to a hydrogel precursor solution, mix well to obtain a mixed solution, and freeze-dry the mixed solution after gelation to obtain a polyvinyl alcohol-nanocellulose crystal composite hydrogel interface evaporator. Preferably, ultrasonic treatment can be used to mix to obtain a uniformly mixed mixed solution; the concentration of reduced graphene oxide in the mixed solution is 0.1-1%; the cross-linking agent is aldehydes (glutaraldehyde), boric acid, epichlorohydrin or a heavy metal salt that can form a gel with polyvinyl alcohol through coordination complexation; the gelation temperature is 60-80°C and the time is 2-3h.
[0009] The second aspect of the present invention is to provide a polyvinyl alcohol-nanocellulose crystal composite hydrogel interface evaporator, which is prepared by the preparation method described in the first aspect above.
[0010] The third aspect of the present invention is to provide the use of the polyvinyl alcohol-nanocellulose crystal composite hydrogel interface evaporator as described in the second aspect in seawater desalination or wastewater purification.
[0011] The present invention has at least the following beneficial effects:
[0012] (1) In the polyvinyl alcohol-nanocellulose crystal composite hydrogel interface evaporator provided by the present invention, CNC is used as the physical cross-linking site, PVA is used as the chemical cross-linking network, and rGO is used as the light absorbing material. In the cellulose-based hydrogel, the polyvinyl alcohol-nanocellulose crystal composite hydrogel interface evaporator prepared by using CNC, PVA and rGO exhibits multifunctional characteristics. The composite strategy of polyvinyl alcohol-nanocellulose crystals in the preparation method of the present invention is simple and low-cost, and the obtained polyvinyl alcohol-nanocellulose crystal composite hydrogel has excellent mechanical strength, good recycling and salt and acid resistance.
[0013] (2) In the present invention, rGO is used to impart excellent wide-spectrum absorption and photothermal conversion properties to the composite hydrogel; PVA enables the composite hydrogel to have excellent mechanical strength, and CNC affects the evaporation rate of the product. The present invention prepares a product with excellent comprehensive performance by compounding CNC, PVA and rGO in a certain amount.
[0014] (3) The present invention combines polyvinyl alcohol and nanocellulose crystals to form a composite hydrogel that exhibits a stable evaporation rate and salt resistance for seawater of different concentrations; the composite hydrogel exhibits a stable purification rate for wastewater of different concentrations. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 This is a flow chart for preparing the polyvinyl alcohol-nanocellulose crystal composite hydrogel interface evaporator provided in Example 1 of the present invention.
[0016] Figure 2 Schematic diagram of reducing water evaporation enthalpy by using a hydrogel cross-linked network provided by the invention.
[0017] Figure 3 This is a SEM image of the composite hydrogel interface evaporator provided in Example 2 of the present invention and Comparative Example 1.
[0018] Figure 4 The solar light absorption spectra of the products prepared in the embodiments and comparative examples of the present invention are shown in FIG.
[0019] Figure 5 rGO 0.1% , storage modulus (G′) and loss modulus (G″) of PCr2 composite hydrogel.
[0020] Figure 6 The Na content of 3.5% seawater simulated solution before and after desalination by PCr2 composite hydrogel + Mg 2+ ,K + ,Ca 2+ Changes in the concentrations of the four major ions. DETAILED DESCRIPTION
[0021] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0022] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.
[0023] In order to enable those skilled in the art to more clearly understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below in conjunction with specific embodiments.
[0024] Example 1
[0025] refer to Figure 1 , a method for preparing a polyvinyl alcohol-nanocellulose crystal composite hydrogel interface evaporator, comprising the following steps:
[0026] (1) Preparation of hydrogel precursor solution: Prepare 0.5 wt% CNC solution with nanocrystalline cellulose and then emulsify it. The emulsification conditions are: emulsify at room temperature and 12000 rpm for 30 min, mix well and set aside. Mix 1 g PVA, 3 mL 0.5 wt% CNC solution and 7 mL deionized water in a glass bottle, add 1 mL 1.2 mol·L -1 hydrochloric acid, and placed it in an oil bath at 95 °C for magnetic stirring for 0.5 h until the PVA was completely melted to obtain a hydrogel precursor solution.
[0027] (2) Light absorption material treatment: rGO was added to the hydrogel precursor solution with a mass fraction of 0.1%, and placed in an ultrasonic cleaner for 0.5 h. After being taken out, it was placed in a magnetic stirrer and stirred for 10 min to ensure uniform mixing.
[0028] (3) Preparation of polyvinyl alcohol-nanocellulose crystal composite hydrogel interface evaporator: Continue to add 250 μL of glutaraldehyde and mix well to obtain a mixed solution. The mixed solution is gelled at 60°C for 2 h to obtain a hydrogel. The hydrogel is placed in a -25°C refrigerator and frozen for 12 h, and then freeze-dried for 48 h. The obtained hydrogel sample is fully swollen and then subjected to an evaporation test. The obtained composite hydrogel is named PCr1.
[0029] Example 2
[0030] A method for preparing a polyvinyl alcohol-nanocellulose crystal composite hydrogel interface evaporator comprises the following steps:
[0031] (1) Preparation of hydrogel precursor solution: Prepare 0.5 wt% CNC solution with nanocrystalline cellulose and then emulsify it. The emulsification conditions are: emulsify at room temperature and 12000 rpm for 30 min, mix well and set aside. Mix 1 g PVA, 5 mL 0.5 wt% CNC solution and 5 mL deionized water in a glass bottle, add 1 mL 1.2 mol·L -1 hydrochloric acid, and placed it in an oil bath at 95 °C for magnetic stirring for 0.5 h until the PVA was completely melted to obtain a hydrogel precursor solution.
[0032] (2) Light absorption material treatment: rGO was added to the hydrogel precursor solution with a mass fraction of 0.1%, and placed in an ultrasonic cleaner for 0.5 h. After being taken out, it was placed in a magnetic stirrer and stirred for 10 min to ensure uniform mixing.
[0033] (3) Preparation of polyvinyl alcohol-nanocellulose crystal composite hydrogel interface evaporator: Continue to add 250 μL of glutaraldehyde and mix well to obtain a mixed solution. The mixed solution is gelled at 60°C for 2 h to obtain a hydrogel. The hydrogel is placed in a -25°C refrigerator and frozen for 12 h, and then freeze-dried for 48 h. The obtained hydrogel sample is fully swollen and then subjected to an evaporation test. The obtained composite hydrogel is named PCr2.
[0034] Example 3
[0035] A method for preparing a polyvinyl alcohol-nanocellulose crystal composite hydrogel interface evaporator comprises the following steps:
[0036] (1) Preparation of hydrogel precursor solution: Prepare 0.5 wt% CNC solution with nanocrystalline cellulose and then emulsify it. The emulsification conditions are: emulsify at room temperature and 12000 rpm for 30 min, mix well and set aside. Mix 1 g PVA and 10 mL 0.5 wt% CNC solution in a glass bottle, add 1 mL 1.2 mol·L -1 hydrochloric acid, and placed it in an oil bath at 95 °C for magnetic stirring for 0.5 h until the PVA was completely melted to obtain a hydrogel precursor solution.
[0037] (2) Light absorption material treatment: rGO was added to the hydrogel precursor solution with a mass fraction of 0.1%, and placed in an ultrasonic cleaner for 0.5 h. After being taken out, it was placed in a magnetic stirrer and stirred for 10 min to ensure uniform mixing.
[0038] (3) Preparation of polyvinyl alcohol-nanocellulose crystal composite hydrogel interface evaporator: Continue to add 250 μL of glutaraldehyde and mix well to obtain a mixed solution. The mixed solution is gelled at 60°C for 2 h to obtain a hydrogel. The hydrogel is placed in a -25°C refrigerator and frozen for 12 h, and then freeze-dried for 48 h. The obtained hydrogel sample is fully swollen and then subjected to an evaporation test. The obtained composite hydrogel is named PCr3.
[0039] Comparative Example 1
[0040] A method for preparing a polyvinyl alcohol composite hydrogel interface evaporator comprises the following steps:
[0041] (1) Preparation of hydrogel precursor solution: 1 g PVA and 10 mL deionized water were mixed in a glass bottle, and 1 mL 1.2 mol·L -1 hydrochloric acid, and placed it in an oil bath at 95 °C for magnetic stirring for 0.5 h until the PVA was completely melted to obtain a hydrogel precursor solution.
[0042] (2) Light absorption material treatment: rGO was added to the hydrogel precursor solution with a mass fraction of 0.1%, and placed in an ultrasonic cleaner for 0.5 h. After being taken out, it was placed in a magnetic stirrer and stirred for 10 min to ensure uniform mixing.
[0043] (3) Preparation of polyvinyl alcohol composite hydrogel interface evaporator: Continue to add 250 μL of glutaraldehyde and mix well to obtain a mixed solution. The mixed solution is gelled at 60°C for 2 h to obtain a hydrogel. The hydrogel is placed in a -25°C refrigerator for 12 h and then freeze-dried for 48 h. The obtained hydrogel sample is fully swollen and then subjected to an evaporation test. The obtained composite hydrogel is named rGO 0.1% .
[0044] Comparative Example 2
[0045] A method for preparing a polyvinyl alcohol composite hydrogel interface evaporator comprises the following steps:
[0046] (1) Preparation of hydrogel precursor solution: 1 g PVA and 10 mL deionized water were mixed in a glass bottle, and 1 mL 1.2 mol·L -1 hydrochloric acid, and placed it in an oil bath at 95 °C for magnetic stirring for 0.5 h until the PVA was completely melted to obtain a hydrogel precursor solution.
[0047] (2) Treatment of light absorbing materials: rGO was added to the hydrogel precursor solution with a mass fraction of 0.2%, and placed in an ultrasonic cleaner for 0.5 h. After being taken out, it was placed in a magnetic stirrer and stirred for 10 min to ensure uniform mixing.
[0048] (3) Preparation of polyvinyl alcohol composite hydrogel interface evaporator: Continue to add 250 μL of glutaraldehyde and mix well to obtain a mixed solution. The mixed solution is gelled at 60°C for 2 h to obtain a hydrogel. The hydrogel is placed in a -25°C refrigerator for 12 h and then freeze-dried for 48 h. The obtained hydrogel sample is fully swollen and then subjected to an evaporation test. The obtained composite hydrogel is named rGO 0.2% .
[0049] Comparative Example 3
[0050] A method for preparing a polyvinyl alcohol composite hydrogel interface evaporator comprises the following steps:
[0051] (1) Preparation of hydrogel precursor solution: 1 g PVA and 10 mL deionized water were mixed in a glass bottle, and 1 mL 1.2 mol·L -1 hydrochloric acid, and placed it in an oil bath at 95 °C for magnetic stirring for 0.5 h until the PVA was completely melted to obtain a hydrogel precursor solution.
[0052] (2) Light absorption material treatment: rGO was added to the hydrogel precursor solution with a mass fraction of 0.4%, and placed in an ultrasonic cleaner for 0.5 h. After being taken out, it was placed in a magnetic stirrer and stirred for 10 min to ensure uniform mixing.
[0053] (3) Preparation of polyvinyl alcohol composite hydrogel interface evaporator: Continue to add 250 μL of glutaraldehyde and mix well to obtain a mixed solution. The mixed solution is gelled at 60°C for 2 h to obtain a hydrogel. The hydrogel is placed in a -25°C refrigerator for 12 h and then freeze-dried for 48 h. The obtained hydrogel sample is fully swollen and then subjected to an evaporation test. The obtained composite hydrogel is named rGO 0.4% .
[0054] Comparative Example 4
[0055] A method for preparing a polyvinyl alcohol composite hydrogel interface evaporator comprises the following steps:
[0056] (1) Preparation of hydrogel precursor solution: 1 g PVA and 10 mL deionized water were mixed in a glass bottle, and 1 mL 1.2 mol·L -1 hydrochloric acid, and placed it in an oil bath at 95 °C for magnetic stirring for 0.5 h until the PVA was completely melted to obtain a hydrogel precursor solution.
[0057] (2) Light absorption material treatment: rGO was added to the hydrogel precursor solution with a mass fraction of 0.6%, and placed in an ultrasonic cleaner for 0.5 h. After being taken out, it was placed in a magnetic stirrer and stirred for 10 min to ensure uniform mixing.
[0058] (3) Preparation of polyvinyl alcohol composite hydrogel interface evaporator: Continue to add 250 μL of glutaraldehyde and mix well to obtain a mixed solution. The mixed solution is gelled at 60°C for 2 h to obtain a hydrogel. The hydrogel is placed in a -25°C refrigerator for 12 h and then freeze-dried for 48 h. The obtained hydrogel sample is fully swollen and then subjected to an evaporation test. The obtained composite hydrogel is named rGO 0.6% .
[0059] Comparative Example 5
[0060] A method for preparing a polyvinyl alcohol composite hydrogel interface evaporator comprises the following steps:
[0061] (1) Preparation of hydrogel precursor solution: 1 g PVA and 10 mL deionized water were mixed in a glass bottle, and 1 mL 1.2 mol·L -1 hydrochloric acid, and placed it in an oil bath at 95 °C for magnetic stirring for 0.5 h until the PVA was completely melted to obtain a hydrogel precursor solution.
[0062] (2) Light absorption material treatment: rGO was added to the hydrogel precursor solution with a mass fraction of 0.8%, and placed in an ultrasonic cleaner for 0.5 h. After being taken out, it was placed in a magnetic stirrer and stirred for 10 min to ensure uniform mixing.
[0063] (3) Preparation of polyvinyl alcohol composite hydrogel interface evaporator: 250 μL of glutaraldehyde was added and mixed to obtain a mixed solution. The mixed solution was gelled at 60 °C for 2 h to obtain a hydrogel. The hydrogel was placed in a -25 °C refrigerator for 12 h and then freeze-dried for 48 h. The obtained hydrogel sample was fully swollen and then subjected to an evaporation test. The obtained composite hydrogel was named rGO. 0.8% .
[0064] Comparative Example 6
[0065] A method for preparing a polyvinyl alcohol composite hydrogel interface evaporator comprises the following steps:
[0066] (1) Preparation of hydrogel precursor solution: 1 g PVA and 10 mL deionized water were mixed in a glass bottle, and 1 mL 1.2 mol·L -1 hydrochloric acid, and placed it in an oil bath at 95 °C for magnetic stirring for 0.5 h until the PVA was completely melted to obtain a hydrogel precursor solution.
[0067] (2) Light absorption material treatment: rGO was added to the hydrogel precursor solution with a mass fraction of 1.0%, and it was placed in an ultrasonic cleaner for 0.5 h. After being taken out, it was placed in a magnetic stirrer and stirred for 10 min to ensure uniform mixing.
[0068] (3) Preparation of polyvinyl alcohol composite hydrogel interface evaporator: Continue to add 250 μL of glutaraldehyde and mix well to obtain a mixed solution. The mixed solution is gelled at 60°C for 2 h to obtain a hydrogel. The hydrogel is placed in a -25°C refrigerator for 12 h and then freeze-dried for 48 h. The obtained hydrogel sample is fully swollen and then subjected to an evaporation test. The obtained composite hydrogel is named rGO 1.0% .
[0069] Comparative Example 7
[0070] A method for preparing a polyvinyl alcohol hydrogel comprises the following steps:
[0071] (1) Preparation of hydrogel precursor solution: 1 g PVA and 10 mL deionized water were mixed in a glass bottle, and 1 mL 1.2 mol·L -1 hydrochloric acid, and placed it in an oil bath at 95 °C for magnetic stirring for 0.5 h until the PVA was completely melted to obtain a hydrogel precursor solution.
[0072] (2) Preparation of polyvinyl alcohol hydrogel: 250 μL of glutaraldehyde was added and mixed to obtain a mixed solution. The mixed solution was gelled at 60°C for 2 h to obtain a hydrogel. The hydrogel was placed in a -25°C refrigerator for 12 h and then freeze-dried for 48 h. After the obtained hydrogel sample was fully swollen, an evaporation test was performed. The obtained composite hydrogel was named PVA hydrogel.
[0073] Solar interface evaporation performance test
[0074] A xenon lamp was used to simulate sunlight, and the light intensity on the surface of the composite hydrogel interface evaporator was measured with an optical power meter to maintain it at 1 kW m -2 A layer of plastic wrap is covered on the surface of the evaporator to collect the evaporated water. Then the performance of the composite hydrogel interface evaporator can be measured by an electronic balance system and an infrared thermal imager.
[0075] Figure 3 rGO 0.1% The SEM morphology of PCr2 (a) and PCr2 (b) shows that the pores with a diameter of about 20 μm are evenly distributed in the figure. The existence of this porous structure and the large amount of hydroxyl groups in CNC make PCr2 composite hydrogel have excellent water absorption and water transport capabilities. In addition, the pores of PCr2 composite hydrogel are more uniform, which can provide more stable water transport capacity and ensure a stable evaporation rate. -2 ) were 1.3 kg m -2 h -1 , 1.40kg m -2 h -1, 1.62kg m -2 h -1 , 1.21kg m -2 h -1 ,It can be seen that when the CNC concentration is kept at 0.25%, the evaporation rate of the polyvinyl alcohol-nanocellulose crystal composite hydrogel interface evaporator is the highest.
[0076] This can also be proved by the effect of polyvinyl alcohol-nanocellulose crystal composite hydrogel on water evaporation enthalpy. The hydrogel polymer network captures water molecules through electrostatic action and hydrogen bonds, regulates the hydrogen bond network and intermolecular forces inside the hydrogel, thereby regulating the state and phase change behavior of water, and then reducing the evaporation enthalpy of water. There are three types of water under the action of polymer chains: bound water, free water, and intermediate water, such as Figure 2 As shown. The hydrophilic groups of the polymer chain and water molecules form bound water through strong intermolecular interactions. Free water refers to the part of water molecules connected to each other by hydrogen bonds. Intermediate water exists between free water and bound water. It is connected to bound water by weaker hydrogen bonds, and this weak force is lower than the hydrogen bonding between free water molecules, so it can be more easily freed from the constraints of weak hydrogen bonds, ultimately reducing the evaporation enthalpy. The evaporation enthalpy of water of the products prepared in Comparative Example 1 and Examples 1-3 is 1911 J g -1 , 1634 J g -1 , 1415 J g -1 , 2392 J g -1 , it can be seen that the polyvinyl alcohol-nanocellulose crystal composite hydrogel interface evaporator (PCr2) with a CNC concentration of 0.25% has the lowest evaporation enthalpy and is the easiest to evaporate, so the evaporation rate is the highest.
[0077] The product prepared by the present invention has a wide spectrum absorption performance, specifically Figure 4 As shown, Figure 4 The average light absorption rates of the products prepared in Example 1 and Comparative Examples 2-6 in the spectral absorption range of 250-2500nm are 95.05%, 95.19%, 94.85%, 94.41%, 94.68% and 94.74%, respectively. The reduced graphene oxide concentration in the products prepared in Examples 2-3 and Comparative Example 1 is 0.1%, and the average light absorption rates are the same as in Example 1, both being 95.05%.
[0078] Figure 5 rGO 0.1% The storage modulus (G′) and loss modulus (G″) of PCr2 composite hydrogel are Figure 5 It can be seen that the composite hydrogel product prepared by the present invention has excellent mechanical strength.
[0079] Application Example 1: Seawater Desalination
[0080] Using seawater to simulate the seawater environment, different concentrations of seawater simulation solutions (3.5%, 10%, and 20%) were poured into a beaker and placed on an electronic balance. The PCr2 composite hydrogel was prepared into a round shape through a mold. After being fully swollen, it floated in the seawater simulation solutions of different concentrations. The xenon lamp light source system was adjusted to a light intensity of 1 kW·m -2 The balance is connected to a computer to record the mass change in real time. The evaporated fresh water is collected by a collection device. After analyzing the desalinated seawater obtained by evaporation of PCr2, the removal rates of sodium ions, magnesium ions, potassium ions, and calcium ions in seawater are as high as 99%. The test results for the 3.5% concentration of seawater simulation solution are as follows Figure 6 As shown, it can be seen that the PCr2 composite hydrogel prepared by the present invention has a good desalination effect on seawater.
[0081] Application Example 2 Wastewater Purification
[0082] Pulping waste liquid and concentrated pulping waste liquid (2 times, 3 times, and 4 times the original concentration) were poured into a beaker and placed on an electronic balance. The PCr2 composite hydrogel was prepared into a round shape through a mold. After sufficient swelling, it floated in the pulping waste liquid. The xenon lamp light source system was adjusted to a light intensity of 1 kW·m -2 , the balance is connected to the computer to record the mass change in real time. The evaporated purified water is collected together through a collection device. After analysis, the BOD and COD removal rates of the purified water obtained by evaporating different concentrated pulping wastewaters through PCr2 are as high as 99.9%, and the wastewater purification efficiency is excellent.
[0083] From the test results of the above two application examples, it can be seen that the polyvinyl alcohol-nanocellulose crystal composite hydrogel interface evaporator prepared by the present invention performs excellently in seawater desalination and wastewater purification, and has excellent salt resistance, seawater desalination ability, and wastewater purification ability.
[0084] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a polyvinyl alcohol-nanocellulose crystal composite hydrogel interface evaporator, characterized in that: The following steps are involved: Adding nanocrystalline cellulose, polyvinyl alcohol and acid solution into water, mixing, and heating to dissolve the polyvinyl alcohol to obtain a hydrogel precursor solution; Reduced graphene oxide and a cross-linking agent are added to a hydrogel precursor solution, and the mixture is uniformly mixed to obtain a mixed solution, and the mixed solution is gelled and then freeze-dried to obtain a polyvinyl alcohol-nanocellulose crystal composite hydrogel interface evaporator.
2. The method for preparing the polyvinyl alcohol-nanocellulose crystal composite hydrogel interface evaporator according to claim 1, characterized in that: The concentration of nano-microcrystalline cellulose in the hydrogel precursor solution is 0.15wt%-0.5wt%.
3. The method for preparing the polyvinyl alcohol-nanocellulose crystal composite hydrogel interface evaporator according to claim 1, characterized in that: The nano-microcrystalline cellulose is prepared into a solution of a certain concentration before use, and then emulsified and mixed evenly before use.
4. The method for preparing the polyvinyl alcohol-nanocellulose crystal composite hydrogel interface evaporator according to claim 1, characterized in that: The acid solution is hydrochloric acid.
5. The method for preparing the polyvinyl alcohol-nanocellulose crystal composite hydrogel interface evaporator according to claim 1, characterized in that: The concentration of reduced graphene oxide in the mixed solution is 0.1-1%.
6. The method for preparing the polyvinyl alcohol-nanocellulose crystal composite hydrogel interface evaporator according to claim 1, characterized in that: The cross-linking agent is aldehydes, boric acid, epichlorohydrin or a heavy metal salt that can form a gel through coordination complexation with polyvinyl alcohol.
7. The method for preparing the polyvinyl alcohol-nanocellulose crystal composite hydrogel interface evaporator according to claim 6, characterized in that: The aldehyde is glutaraldehyde.
8. The method for preparing a polyvinyl alcohol-nanocellulose crystal composite hydrogel interface evaporator according to any one of claims 1 to 7, characterized in that: The gelation temperature is 60-80°C and the time is 2-3h.
9. A polyvinyl alcohol-nanocellulose crystal composite hydrogel interface evaporator, characterized in that: The invention discloses a novel nanostructured carbon foam prepared by the preparation method described in any one of claims 1 to 8.
10. Use of the polyvinyl alcohol-nanocellulose crystal composite hydrogel interfacial evaporator as claimed in claim 9 in seawater desalination or wastewater purification.
Citation Information
Patent Citations
Preparation method of cellulose nanocrystal / graphene / polyvinyl alcohol aerogel
CN108579626A
PVA hydrogel-based photo-thermal evaporation material and preparation and application thereof
CN111171340A
Partially reduced graphene oxide-nanocellulose crystal-polyvinyl alcohol composite conductive hydrogel and preparation method and application thereof
CN112159535A
System and method for solar-powered desalination and water purification
US20230219829A1
Cited By
Composite hydrogel evaporator with chemical-photo-thermal synergistic antibacterial function and preparation of composite hydrogel evaporator
CN120607302A
Bamboo-based photothermal evaporation enrichment monitoring device, preparation method thereof and application of the device in monitoring drugs in river basin
CN122962069A