Nano calcium phosphate oligomer for reinforcing cultural relics as well as preparation method and application of nano calcium phosphate oligomer
Through the preparation method of nano calcium phosphate oligomer, the problems of insufficient reinforcement strength and calcium source requirements of inorganic cultural relics reinforcement materials are solved, the high-strength reinforcement and simplification process of cultural relics are achieved, and the hardness and bonding strength are improved.
Patent Information
- Application Number
- CN202411112524.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-14
AI Technical Summary
Existing inorganic cultural relic reinforcement materials such as alkaline earth metal nanohydroxide reinforcement have insufficient reinforcement strength and require a long and slow process. Calcium phosphate reinforcement requires a calcium source, which poses a risk of introducing harmful substances.
Using the preparation method of nano calcium phosphate oligomer, by placing ethanol solutions of calcium chloride, arginine and phosphoric acid, adding triethylamine and stirring, forming nano calcium phosphate oligomers, without additional calcium sources applied to the surface of cultural relics. It is converted into hydroxyapatite with poor crystallinity for reinforcement.
High-strength reinforcement of cultural relics has been achieved, and the hardness and surface bonding strength have been increased by 50%-80%, without providing a calcium source, simplifying the reinforcement process and reducing potential damage to cultural relics.
Smart Images

Figure CN119059751A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of cultural relic protection materials and relates to a nano calcium phosphate oligomer for reinforcing cultural relics and a preparation method and application thereof. Background Art
[0002] Cultural relics reinforcement materials are mainly divided into two categories: organic materials and inorganic materials. Organic materials, such as polyacrylic resin, have strong bonding strength and little effect on the surface color of cultural relics. They are currently the most widely used cultural relics reinforcement materials. However, with the widespread application of this material, problems gradually emerge: yellowing, brittleness, and even failure after a long time. These problems are inherent disadvantages of organic materials. In contrast, inorganic materials show better aging resistance and excellent compatibility with murals, and are the current research direction and hotspot of cultural heritage reinforcement and protection materials. (J. Colloid Interface Sci. 2013, 392, 42-49.). Currently reported inorganic cultural relics reinforcement materials include: alkaline earth metal nanohydroxides (such as nano calcium hydroxide, nano barium hydroxide, etc.), calcium phosphate, etc. (Const. Build. Mater., 2024, 431, 136551). Among them, alkaline earth metal nanohydroxides are the most studied and partially commercialized inorganic nano-cultural relics reinforcement materials. However, this type of material mainly achieves the reinforcement of cultural relics through carbonation (J.Cult.Herit.2021,50,25-42.), and the process is slow (usually takes 1 to 2 weeks). In addition, there is an inherent disadvantage of insufficient reinforcement strength. In comparison, calcium phosphate is more effective because it is eventually converted into higher-strength hydroxyapatite in cultural relics, which can achieve high-strength reinforcement of cultural relics. However, at present, calcium phosphate reinforcement of cultural relics either requires a calcium source (such as marble) in the reinforced object, or directly introduces harmful calcium sources (such as calcium chloride) into the cultural relics. In short, calcium phosphate reinforcement of cultural relics must provide a calcium source. Summary of the invention
[0003] Technical issues to be solved
[0004] In order to avoid the shortcomings of the prior art, the present invention provides a nano calcium phosphate oligomer for reinforcing cultural relics and a preparation method and application thereof.
[0005] Technical Solution
[0006] A method for preparing nano calcium phosphate oligomers for reinforcing cultural relics, characterized by the following steps:
[0007] Step 1: Prepare calcium chloride ethanol solution, arginine aqueous solution and phosphoric acid ethanol solution:
[0008] Calcium chloride dihydrate is dissolved in ethanol to obtain an ethanol solution A of calcium chloride;
[0009] Add arginine into purified water to prepare arginine aqueous solution B;
[0010] The phosphoric acid solution is added into ethanol to prepare the phosphoric acid ethanol solution C;
[0011] Step 2: Preparation of nano calcium phosphate oligomers:
[0012] Step 2.1: adding arginine aqueous solution B dropwise into calcium chloride ethanol solution A to obtain calcium chloride solution D containing arginine;
[0013] Step 2.2: adding triethylamine to the calcium chloride solution D containing arginine to obtain a solution E containing triethylamine;
[0014] Step 2.3: Add phosphoric acid ethanol solution C dropwise to solution E containing triethylamine and stir; after stirring, centrifuge and wash with ethanol solution to obtain nano calcium phosphate oligomers.
[0015] The preparation ratio of the calcium chloride ethanol solution A is 2.2-4.4 grams of calcium chloride dihydrate and 50-100 mL of ethanol.
[0016] The preparation ratio of the arginine aqueous solution B is 0.3-0.8 g arginine and 10 mL pure water.
[0017] The phosphoric acid ethanol solution C is prepared in a ratio of 0.7 mL to 2.8 mL of phosphoric acid solution to 10 mL to 40 mL of ethanol.
[0018] When the arginine aqueous solution B is mixed with the calcium chloride ethanol solution A in step 2.1, the mixing ratio of each portion is a mixture of the components of claim 2 and claim 3.
[0019] The amount of triethylamine added in step 2.2 is 50 mL-100 mL.
[0020] When adding the phosphoric acid ethanol solution C in step 2.3, stir for 12-24 hours.
[0021] The amount of phosphoric acid ethanol solution C added to each portion of the mixing in step 2.3 is the amount of claim 4.
[0022] An application of the nano calcium phosphate oligomer obtained by the preparation method according to any one of claims 1 to 8, characterized in that it is used for the reinforcement of ancient murals and stone cultural relics.
[0023] The nano-calcium phosphate oligomer is ultrasonically dispersed in ethanol to obtain an ethanol solution of the nano-calcium phosphate oligomer with a concentration of 10-20 mg / mL; the solution is sprayed on the surface of ancient murals and stone cultural relics until no more absorption occurs, and then the excess solution on the surface is wiped off with absorbent cotton; and then the ancient murals and stone cultural relics with the nano-calcium phosphate oligomer applied are placed in an environment with room temperature and a humidity of 75%-90% for 48-60 hours.
[0024] Beneficial Effects
[0025] The present invention proposes a nano-calcium phosphate oligomer for the reinforcement of cultural relics, and its preparation method and application. The nano-calcium phosphate oligomer is prepared by adding an ethanol solution of calcium chloride, then adding arginine, and finally adding triethylamine to the mixture. Phosphoric acid is added and stirred for 12-24 hours to obtain the nano-calcium phosphate oligomer. The synthesis method is simple and easy to operate. More importantly, the nano-calcium phosphate oligomer synthesized by the method is applied to the reinforcement of cultural relics without providing an additional calcium source, and there is no requirement for whether the reinforcement object contains a calcium source. After being applied to ancient murals and stone cultural relics, it was found that the nano-calcium phosphate oligomer prepared by the present invention has good permeability in both and is converted into hydroxyapatite with poor crystallinity that is interconnected within 48-60 hours.
[0026] Compared with the prior art, the preparation method of the nano calcium phosphate oligomer provided by the present invention is simple. During the synthesis process, arginine is modified on the surface of calcium phosphate so that it is dispersed in a solution to form nano particles (50-300nm) without agglomeration. In terms of application, there is no requirement that the reinforced cultural relic object must contain a calcium source. It is found that the nano calcium phosphate oligomer prepared by the present invention has good permeability in the murals and stone cultural relics, which can reach the centimeter level, and is converted into a mutually connected film within 48-60 hours, thereby connecting the loose structure in the cultural relics and playing a reinforcing role. The film is composed of hydroxyapatite with poor crystallinity. The reinforcement strength test shows that the hardness and surface bonding strength of ancient murals and stone cultural relics applied with the material are increased by 50%-80% and 4-6 times respectively. Compared with the ancient murals and stone cultural relics reinforced by the traditional method of ammonium dihydrogen phosphate, calcium chloride and ammonium dihydrogen phosphate, the hardness and surface bonding strength are comparable, but for ammonium dihydrogen phosphate, it is necessary to select cultural relics objects containing calcium sources, for calcium chloride and ammonium dihydrogen phosphate, soluble calcium chloride has potential damage to cultural relics, and the time process needs to apply calcium chloride and ammonium dihydrogen phosphate in sequence, which increases the risk of damage to cultural relics. In addition, the two methods of ammonium dihydrogen phosphate, calcium chloride and ammonium dihydrogen phosphate form flaky calcium phosphate with good crystallinity in cultural relics, which is not formed as the continuous film-like hydroxyapatite of the material of the present invention, which is unfavorable for reinforcement in the long run. The nano calcium phosphate prepared by the present invention has great application prospects in the reinforcement of cultural relics. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1This is a dynamic light scattering test result of nano calcium phosphate oligomers. The horizontal axis is the particle size, and the vertical axis is the particle size ratio. It can be seen from the figure that the particle size range of nano calcium phosphate oligomers is 50-300nm, and the 80nm size particles account for the largest proportion (the vertex corresponds to the size). DETAILED DESCRIPTION
[0028] The present invention will now be further described with reference to the embodiments and the accompanying drawings:
[0029] The purpose of the present invention is to provide a nano calcium phosphate oligomer for the reinforcement of ancient cultural relics and a preparation method thereof. The present invention first prepares an ethanol solution of calcium chloride, then adds arginine, and finally adds triethylamine to the above mixture, adds phosphoric acid and stirs for 12-24 hours to prepare the nano calcium phosphate oligomer. The synthesis method is simple and easy to operate. More importantly, the nano calcium phosphate oligomer synthesized by the method is applied to the reinforcement of cultural relics without providing an additional calcium source, and there is no requirement for whether the reinforcement object contains a calcium source. After being applied to ancient murals and stone cultural relics, it is found that the nano calcium phosphate oligomer prepared by the present invention has good permeability in both and is transformed into hydroxyapatite with poor crystallinity that is interconnected within 48-60 hours. The reinforcement strength test shows that the hardness and surface bonding strength of the ancient murals and stone cultural relics applied with the material are increased by 50%-80% and 4-6 times respectively. Compared with the ancient murals and stone cultural relics reinforced by the traditional method of diammonium phosphate, calcium chloride and diammonium phosphate, the hardness and surface bonding strength are equivalent. The material breaks through the restrictions on the objects of cultural relics reinforcement and has good promotion prospects.
[0030] Preparation method steps:
[0031] Step 1, prepare calcium chloride ethanol solution, arginine aqueous solution, and phosphoric acid ethanol solution: first, add 2.2-4.4 grams of calcium chloride dihydrate in 50-100 mL of ethanol to obtain a calcium chloride ethanol solution; add 0.3-0.8 g of arginine to 10 mL of pure water to prepare an arginine aqueous solution; add 0.7 mL-2.8 mL of phosphoric acid solution to 10 mL-40 mL of ethanol to prepare a phosphoric acid ethanol solution.
[0032] Step 2, preparation of nano calcium phosphate oligomers: adding the arginine solution of step 1 dropwise into the ethanol solution of calcium chloride to obtain a calcium chloride solution containing arginine; after completion, adding 50mL-100mL of triethylamine to the solution containing arginine; finally, adding the ethanol solution of phosphoric acid dropwise into the mixed solution of triethylamine, arginine and calcium chloride and stirring for 12-24h; after stirring, centrifuging and washing with ethanol solution to obtain nano calcium phosphate oligomers.
[0033] Application steps:
[0034] Ancient murals and stone cultural relics reinforcement method: The prepared nano calcium phosphate oligomers are re-ultrasonic dispersed in ethanol to obtain an ethanol solution of nano calcium phosphate oligomers with a concentration of 10-20 mg / mL. The solution is sprayed on the surface of ancient murals and stone cultural relics until it is no longer absorbed, and then the excess solution on the surface is wiped off with absorbent cotton. Then the ancient murals and stone cultural relics with nano calcium phosphate oligomers are placed in an environment with room temperature and humidity of 75%-90% for 48-60 hours.
[0035] Embodiment 1:
[0036] First, 2.2g of calcium chloride dihydrate is added to 50mL of ethanol to obtain an ethanol solution of calcium chloride; 0.3g of arginine is added to 10mL of pure water to prepare an arginine aqueous solution; 0.7mL of phosphoric acid solution is added to 10mL of ethanol to prepare an ethanol solution of phosphoric acid. The arginine solution is added dropwise to the ethanol solution of calcium chloride to obtain a calcium chloride solution containing arginine; after completion, 50mL of triethylamine is added to the solution containing arginine; finally, the ethanol solution of phosphoric acid is added dropwise to a mixed solution of triethylamine, arginine and calcium chloride and stirred for 12h; after stirring, the nano calcium phosphate oligomer is obtained by centrifugation and washing with the ethanol solution.
[0037] Ancient murals and stone cultural relics reinforcement method: The prepared nano calcium phosphate oligomers are re-ultrasonic dispersed in ethanol to obtain an ethanol solution of nano calcium phosphate oligomers with a concentration of 10 mg / mL. The solution is sprayed on the surface of ancient murals and stone cultural relics until it is no longer absorbed, and then the excess solution on the surface is wiped off with absorbent cotton. Then the ancient murals and stone cultural relics with nano calcium phosphate oligomers are placed in an environment with room temperature and 75% humidity for 48 hours.
[0038] The test results show that the nano calcium carbonate oligomer can be completely transformed into continuous film-like hydroxyapatite in 50 hours. For ancient murals, nano calcium carbonate oligomers can increase their hardness by 80% and their bonding strength by 5 times; for stone cultural relics, nano calcium carbonate oligomers can increase their hardness by 70% and their bonding strength by 6 times. The hardness and bonding strength of ancient murals and stone cultural relics treated with diammonium phosphate, calcium chloride and diammonium phosphate are comparable, but eventually form flaky hydroxyapatite.
[0039] Embodiment 2:
[0040] First, 3.6 g of calcium chloride dihydrate is added to 80 mL of ethanol to obtain an ethanol solution of calcium chloride; 0.5 g of arginine is added to 10 mL of pure water to prepare an arginine aqueous solution; 1.0 mL of phosphoric acid solution is added to 20 mL of ethanol to prepare an ethanol solution of phosphoric acid. The arginine solution is added dropwise to the ethanol solution of calcium chloride to obtain a calcium chloride solution containing arginine; after completion, 60 mL of triethylamine is added to the solution containing arginine; finally, the ethanol solution of phosphoric acid is added dropwise to a mixed solution of triethylamine, arginine and calcium chloride and stirred for 20 hours; after stirring, the nano calcium phosphate oligomer is obtained by centrifugation and washing with the ethanol solution.
[0041] Ancient murals and stone cultural relics reinforcement method: The prepared nano calcium phosphate oligomers are ultrasonically dispersed in ethanol to obtain an ethanol solution of nano calcium phosphate oligomers with a concentration of 15 mg / mL. The solution is sprayed on the surface of ancient murals and stone cultural relics until it is no longer absorbed, and then the excess solution on the surface is wiped off with absorbent cotton. Then the ancient murals and stone cultural relics with nano calcium phosphate oligomers are placed in an environment with room temperature and 85% humidity for 50 hours.
[0042] The test results show that the nano calcium carbonate oligomer can be completely transformed into continuous film hydroxyapatite in 50 hours. For ancient murals, nano calcium carbonate oligomers can increase their hardness by 80% and their bonding strength by 6 times; for stone cultural relics, nano calcium carbonate oligomers can increase their hardness by 70% and their bonding strength by 6 times. The hardness and bonding strength of ancient murals and stone cultural relics treated with diammonium phosphate, calcium chloride and diammonium phosphate are comparable, but eventually form flaky hydroxyapatite.
[0043] Embodiment three:
[0044] First, 4.0 g of calcium chloride dihydrate is added to 90 mL of ethanol to obtain an ethanol solution of calcium chloride; 0.6 g of arginine is added to 10 mL of pure water to prepare an arginine aqueous solution; 2.0 mL of phosphoric acid solution is added to 30 mL of ethanol to prepare an ethanol solution of phosphoric acid. The arginine solution is added dropwise to the ethanol solution of calcium chloride to obtain a calcium chloride solution containing arginine; after completion, 80 mL of triethylamine is added to the solution containing arginine; finally, the ethanol solution of phosphoric acid is added dropwise to a mixed solution of triethylamine, arginine and calcium chloride and stirred for 22 hours; after stirring, the nano calcium phosphate oligomer is obtained by centrifugation and washing with the ethanol solution.
[0045] Ancient murals and stone cultural relics reinforcement method: The prepared nano calcium phosphate oligomers are re-ultrasonic dispersed in ethanol to obtain an ethanol solution of nano calcium phosphate oligomers with a concentration of 18 mg / mL. The solution is sprayed on the surface of ancient murals and stone cultural relics until it is no longer absorbed, and then the excess solution on the surface is wiped off with absorbent cotton. Then the ancient murals and stone cultural relics applied with nano calcium phosphate oligomers are placed in an environment with room temperature and 90% humidity for 60 hours.
[0046] The test results show that the nano calcium carbonate oligomer can be completely transformed into continuous film-like hydroxyapatite in 60 hours. For ancient murals, nano calcium carbonate oligomers can increase their hardness by 80% and their bonding strength by 5 times; for stone cultural relics, nano calcium carbonate oligomers can increase their hardness by 80% and their bonding strength by 6 times. The hardness and bonding strength of ancient murals and stone cultural relics treated with diammonium phosphate, calcium chloride and diammonium phosphate are comparable, but eventually form flaky hydroxyapatite.
[0047] Embodiment 4:
[0048] First, 4.4 g of calcium chloride dihydrate is added to 100 mL of ethanol to obtain an ethanol solution of calcium chloride; 0.8 g of arginine is added to 10 mL of pure water to prepare an arginine aqueous solution; 2.8 mL of phosphoric acid solution is added to 40 mL of ethanol to prepare an ethanol solution of phosphoric acid. The arginine solution is added dropwise to the ethanol solution of calcium chloride to obtain a calcium chloride solution containing arginine; after completion, 100 mL of triethylamine is added to the solution containing arginine; finally, the ethanol solution of phosphoric acid is added dropwise to a mixed solution of triethylamine, arginine and calcium chloride and stirred for 24 hours; after stirring, the nano calcium phosphate oligomer is obtained by centrifugation and washing with the ethanol solution.
[0049] Ancient murals and stone cultural relics reinforcement method: The prepared nano calcium phosphate oligomers are re-ultrasonic dispersed in ethanol to obtain an ethanol solution of nano calcium phosphate oligomers with a concentration of 20 mg / mL. The solution is sprayed on the surface of ancient murals and stone cultural relics until it is no longer absorbed, and then the excess solution on the surface is wiped off with absorbent cotton. Then the ancient murals and stone cultural relics applied with nano calcium phosphate oligomers are placed in an environment with room temperature and 85% humidity for 60 hours.
[0050] The test results show that the nano calcium carbonate oligomer can be completely transformed into continuous film-like hydroxyapatite in 60 hours. For ancient murals, nano calcium carbonate oligomers can increase their hardness by 70% and their bonding strength by 5 times; for stone cultural relics, nano calcium carbonate oligomers can increase their hardness by 80% and their bonding strength by 5 times. The hardness and bonding strength of ancient murals and stone cultural relics treated with diammonium phosphate, calcium chloride and diammonium phosphate are comparable, but eventually form flaky hydroxyapatite.
[0051] Although the content of the present invention has been described in detail through the above preferred embodiments, it should be appreciated that the above description should not be considered as a limitation of the present invention. After reading the above content, it will be apparent to those skilled in the art that various modifications and substitutions of the present invention will occur. Therefore, the protection scope of the present invention should be limited by the appended claims.
Claims
1. A method for preparing nano calcium phosphate oligomers for cultural relics reinforcement, characterized in that Here are the steps: Step 1: Prepare calcium chloride ethanol solution, arginine aqueous solution and phosphoric acid ethanol solution: Calcium chloride dihydrate is dissolved in ethanol to obtain an ethanol solution A of calcium chloride; Add arginine into purified water to prepare arginine aqueous solution B; The phosphoric acid solution is added into ethanol to prepare the phosphoric acid ethanol solution C; Step 2: Preparation of nano calcium phosphate oligomers: Step 2.1: adding arginine aqueous solution B dropwise into calcium chloride ethanol solution A to obtain calcium chloride solution D containing arginine; Step 2.2: adding triethylamine to the calcium chloride solution D containing arginine to obtain a solution E containing triethylamine; Step 2.3: Add phosphoric acid ethanol solution C dropwise to solution E containing triethylamine and stir; after stirring, centrifuge and wash with ethanol solution to obtain nano calcium phosphate oligomers.
2. The method for preparing the nano calcium phosphate oligomer for cultural relics reinforcement according to claim 1, wherein: The preparation ratio of the calcium chloride ethanol solution A is 2.2-4.4 grams of calcium chloride dihydrate and 50-100 mL of ethanol.
3. The method for preparing the nano calcium phosphate oligomer for cultural relics reinforcement according to claim 1, characterized in that: The preparation ratio of the arginine aqueous solution B is 0.3-0.8 g arginine and 10 mL pure water.
4. The method for preparing the nano calcium phosphate oligomer for cultural relics reinforcement according to claim 1, characterized in that: The phosphoric acid ethanol solution C is prepared in a ratio of 0.7 mL to 2.8 mL of phosphoric acid solution to 10 mL to 40 mL of ethanol.
5. The method for preparing the nano calcium phosphate oligomer for cultural relics reinforcement according to claim 1, characterized in that: When the arginine aqueous solution B is mixed with the calcium chloride ethanol solution A in step 2.1, the mixing ratio of each portion is a mixture of the components of claim 2 and claim 3.
6. The method for preparing the nano calcium phosphate oligomer for cultural relics reinforcement according to claim 1, characterized in that: The amount of triethylamine added in step 2.2 is 50 mL-100 mL.
7. The method for preparing the nano calcium phosphate oligomer for cultural relics reinforcement according to claim 1, characterized in that: When adding the phosphoric acid ethanol solution C in step 2.3, stir for 12-24 hours.
8. The method for preparing the nano calcium phosphate oligomer for cultural relics reinforcement according to claim 1, characterized in that: The amount of phosphoric acid ethanol solution C added to each portion of the mixing in step 2.3 is the amount of claim 4.
9. An application of the nano calcium phosphate oligomer obtained by the preparation method according to any one of claims 1 to 8, characterized in that: Used for the reinforcement of ancient murals and stone cultural relics.
10. The use according to claim 9, characterized in that: The nano-calcium phosphate oligomer is ultrasonically dispersed in ethanol to obtain an ethanol solution of the nano-calcium phosphate oligomer with a concentration of 10-20 mg / mL; the solution is sprayed on the surface of ancient murals and stone cultural relics until no more absorption occurs, and then the excess solution on the surface is wiped off with absorbent cotton; and then the ancient murals and stone cultural relics with the nano-calcium phosphate oligomer applied are placed in an environment with room temperature and a humidity of 75%-90% for 48-60 hours.
Citation Information
Patent Citations
Method for preparing beta-calcium phosphate or hydroxyapatite nanoparticles
CN101811685A
Method for preparing cationic amino acid-containing polypeptide-modified nano calcium phosphate gene vector
CN102031269A
Simple and efficient preparation method of nano calcium phosphate
CN106006593A
Sericin cross-linked calcium carbonate oligomer for reinforcing ancient murals, and preparation and application methods of sericin cross-linked calcium carbonate oligomer
CN117683378A
Process for the preparation of hydroxylapatite by using sol-gel veaction
KR1019970026901A