Concrete appearance beautifying agent and preparation method thereof

By reasonably proportioning components such as gas induction agents and defoaming agents in concrete, uniform and tiny bubbles are formed, the apparent quality of concrete is solved, the construction performance and mechanical properties are improved, and production costs are reduced.

CN119059755APending Publication Date: 2024-12-03GUIZHOU TIANWEI BUILDING MATERIALS TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411186167.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The prior art cannot effectively solve the apparent quality problems of concrete, especially the uneven distribution of bubble cells and the large number of large bubbles, resulting in high construction costs and poor results.

Method used

A concrete appearance beautifier is used to form uniform and tiny bubbles by reasonably proportioning gas induction agents, defoaming agents, thickening agents, water-soluble organic matters and viscosity modifiers, which inhibit the generation of large bubbles and increase the flow of concrete. and viscosity, stabilize bubble structure.

Benefits of technology

Significantly improve the apparent quality of concrete, reduce the number of harmful large bubbles, maintain stable gas content, enhance construction and mechanical properties, and reduce production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119059755A_ABST
    Figure CN119059755A_ABST
Patent Text Reader

Abstract

The invention discloses a concrete appearance beautifying agent and a preparation method thereof. The concrete appearance beautifying agent comprises the following components in percentage by mass: 0.05-0.1% of an air entraining agent, 0.1-0.2% of a defoaming agent, 0.04-0.08% of a thickening agent, 1-2% of a water-soluble organic matter, 2-4% of a viscosity modifier and the balance of water. The concrete appearance beautifying agent disclosed by the invention can optimize the structural form of bubbles in concrete and inhibit the generation of large bubbles and secondary large bubbles, so that the formed bubbles are tiny and good in stability; the concrete appearance beautifying agent is simple in preparation method, low in cost and easy for industrial production; the concrete using the concrete appearance beautifying agent has the characteristics of good appearance quality and stable working performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a concrete additive and a preparation method thereof, in particular to a concrete surface beautifying agent and a preparation method thereof. Background Art

[0002] With the improvement of construction level in the construction industry, people have put forward higher and higher requirements on the appearance quality of concrete components. At present, concrete solid components such as tunnels and bridges in railway and highway projects generally have appearance quality problems, mainly manifested in large-area honeycomb surface, water marks, sand marks, bubble holes, rough and uneven surface, etc.

[0003] The most prominent and frequent of these problems is the apparent quality of concrete bubbles. This problem has not been effectively solved. Expensive release agents are widely used to improve it, or later repairs and modifications are used to remedy it. The implementation cost is high and the effect does not meet expectations. The relevant solutions cannot solve the problems of bubble aggregation inside the concrete, uneven pore size distribution, and a large number of large bubbles. Therefore, the apparent quality of concrete cannot be solved from the source of the problem.

[0004] Therefore, it is imperative to develop a concrete surface beautifier modified material that can optimize the bubble structure morphology inside the concrete system. Summary of the invention

[0005] In order to solve the above technical problems, the present invention provides a concrete surface beautifier and a preparation method thereof. The concrete surface beautifier of the present invention can optimize the morphology and structure of bubbles in concrete, inhibit the generation of large bubbles and the formation of secondary harmful bubbles, make the formed bubbles uniform and small, and have good bubble stability; the preparation method of the concrete surface beautifier of the present invention is simple, low-cost, and easy to industrialize; concrete using the surface beautifier of the present invention has the characteristics of good surface quality and stable working performance.

[0006] One of the technical solutions of the present invention:

[0007] A concrete surface beautifying agent comprises, by mass percentage, 0.05-0.1% of an air entraining agent, 0.1-0.2% of a defoaming agent, 0.04-0.08% of a thickener, 1-2% of a water-soluble organic matter, 2-4% of a viscosity modifier, and the balance is water.

[0008] Preferably, the aforementioned concrete surface beautifier comprises, by mass percentage, 0.08% of air entraining agent, 0.15% of defoaming agent, 0.06% of thickener, 1.5% of water-soluble organic matter and 3% of viscosity modifier, with the balance being water.

[0009] Preferably, in the aforementioned concrete surface beautifying agent, the air entraining agent is a polyether air entraining agent.

[0010] Preferably, in the aforementioned concrete surface beautifying agent, the defoaming agent is a polysiloxane defoaming agent.

[0011] Preferably, in the aforementioned concrete surface beautifying agent, the thickener is a polyacrylic thickener.

[0012] Preferably, in the aforementioned concrete surface beautifying agent, the water-soluble organic matter is a mixture of diethanolamine and triethanolamine.

[0013] Preferably, in the aforementioned concrete surface beautifying agent, the mixing mass ratio of diethanolamine to triethanolamine is 1:1.

[0014] The second technical solution of the present invention:

[0015] A method for preparing a concrete surface beautifier comprises the following steps:

[0016] (1) Weigh air entraining agent, defoamer, thickener, water-soluble organic matter, viscosity modifier and water according to the above ratio;

[0017] (2) placing water-soluble organic matter in a reaction kettle, adding a thickener and a defoamer, and stirring evenly to obtain liquid A;

[0018] (3) Place water in another reaction kettle, add viscosity modifier, stir evenly at 35-45°C, then add air entraining agent, continue stirring evenly, and obtain liquid B;

[0019] (4) Add liquid A to liquid B, raise the temperature to 55-65°C while stirring at a speed of 50-150 r / min, continue stirring for 20-40 min, then stir at a speed of 150-250 r / min for 10-20 min, cool down after stirring, and obtain a concrete surface beautifier.

[0020] Preferably, in the aforementioned method for preparing the concrete surface beautifier, in the step (3), the temperature during stirring is 40°C.

[0021] Preferably, in the method for preparing the aforementioned concrete surface beautifier, in step (4), the temperature is first raised to 60° C. by stirring at a speed of 100 r / min, stirring is continued for 30 min, and then stirring is continued at a speed of 200 r / min for 15 min.

[0022] Beneficial effects of the present invention:

[0023] 1. The concrete surface beautifying agent of the present invention is prepared by mixing air entraining agent, defoaming agent, thickener, water-soluble organic matter, viscosity modifier and water in a reasonable ratio; wherein the air entraining agent is preferably selected to introduce gas to form micro-foam bubbles, thereby avoiding the generation of harmful large bubbles in concrete and improving the fluidity of concrete; and the defoaming agent is preferably selected to eliminate large bubbles among the air entraining agent while introducing a large number of bubbles, thereby inhibiting the generation of large bubbles and secondary large bubbles, thereby retaining micro-foam bubbles, forming uniform and tiny pores, and improving the surface quality of concrete; and the addition of the thickener can stabilize the bubbles, avoid the disappearance of tiny bubbles, thereby obtaining stable bubbles, reducing the loss of concrete air content over time, and enhancing the stability of concrete construction performance; in addition, the viscosity modifier is added to enhance the cohesiveness of the concrete, making the concrete mixture slurry fine and rich, thereby improving the workability of the concrete.

[0024] 2. The concrete surface beautifier of the present invention needs to be prepared by the above method. Although the method is special, the raw materials are all conventional raw materials, the cost is low, and the whole process is simple and easy to industrialize. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Attached Figure 1 It is the apparent quality of hardened concrete after adding the concrete surface beautifying agent of the present invention.

[0026] Attached Figure 2 It is the apparent quality of hardened concrete without adding concrete surface beautifier. DETAILED DESCRIPTION

[0027] The present invention will be further described below in conjunction with the embodiments, but they are not intended to limit the present invention.

[0028] Embodiments of the present invention

[0029] The polyether air-entraining agent used in the embodiment of the present invention is prepared by the following method: fatty alcohol polyoxyethylene ether (AEO), aminosulfonic acid, and urea (UREA) are added to a four-necked flask in sequence and stirred evenly, heated and stirred to 100° C., and kept at a constant temperature for 4 hours; cooled to 60° C., and hot water is added for dilution; cooled to 40° C., and modified silicone resin polyether emulsion (MPS) is added, and stirred evenly to obtain a polyether air-entraining agent.

[0030] The siloxane defoamer used in the embodiment of the present invention is prepared by the following method: methacrylic acid (MA), 2-dodecyl acrylate, hydrogenated silicone oil, dimethyl silicone oil (PDMS) and toluene are added to a four-necked flask in sequence and stirred evenly, condensed and refluxed, and heated and stirred to 55° C.; after 30 minutes, chloroplatinic acid catalyst is added dropwise; the temperature is raised to 95° C., allyl alcohol polyoxyethylene polyoxyene ether is added dropwise, and hydrophilic silica is added; reduced pressure distillation is performed, and the reaction is carried out for 2 hours to obtain a polysiloxane defoamer.

[0031] The polyacrylic acid thickener used in the embodiment of the present invention is prepared by the following method: Preparation of component A: Add acrylic acid (AA) into a beaker, neutralize with ammonia water, adjust the pH to 5.0-6.0, add acrylamide (AM), a crosslinking agent (butyl acrylate (BA), N,N'-methylenebisacrylamide, 2-naphthalenesulfonic acid formaldehyde polymer sodium salt (NNO)), potassium persulfate and deionized water to obtain component A. The continuous phase (white oil, odorless kerosene, aviation kerosene), sorbitan monooleate (Span-80), and n-dodecyl mercaptan are sequentially added into a four-necked flask, and 1 / 10A component is added, and the temperature is raised to 65°C at 200 r / min with stirring, and condensed and refluxed; the remaining 9 / 10A component and isooctyl acrylate (2-EHA) are poured into a separatory funnel and all are added dropwise within 2 hours; the temperature is raised after 0.5 hours, and a white viscous emulsion is obtained after being kept at 75°C, an appropriate amount of polysorbate (Tween-80) is added, and ammonia water is added to adjust the pH to 7.0, and the polyacrylic acid thickener is obtained by stirring at room temperature for 45 minutes.

[0032] The viscosity modifier used in the embodiment of the present invention is a viscosity modifier such as a conventional natural organic polymer, a water-soluble organic flocculant, an organic latex material, a water-swellable inorganic material, and a non-water-swellable inorganic material.

[0033] The air entraining agent, defoaming agent, thickener, viscosity modifier, etc. mentioned above may be commercially available products.

[0034] Example 1

[0035] A concrete surface beautifier comprises, by mass percentage, 0.05% of a polyether air entraining agent, 0.1% of a polysiloxane defoaming agent, 0.04% of a polyacrylic acid thickener, 1% of a mixture of diethanolamine and triethanolamine in a mass ratio of 1:1, and 2% of a viscosity modifier, and the balance is water, with a total amount of 100%.

[0036] Example 2

[0037] A concrete surface beautifier comprises, by mass percentage, 0.06% of a polyether air entraining agent, 0.1% of a polysiloxane defoaming agent, 0.06% of a polyacrylic thickener, 1% of a mixture of diethanolamine and triethanolamine in a mass ratio of 1:1, and 3% of a viscosity modifier, and the balance is water, with a total amount of 100%.

[0038] Example 3

[0039] A concrete surface beautifier comprises, by mass percentage, 0.08% of a polyether air entraining agent, 0.2% of a polysiloxane defoamer, 0.06% of a polyacrylic thickener, 2% of a mixture of diethanolamine and triethanolamine in a mass ratio of 1:1, and 3% of a viscosity modifier, and the balance is water, with a total amount of 100%.

[0040] Example 4

[0041] A concrete surface beautifier comprises, by mass percentage, 0.1% of a polyether air entraining agent, 0.2% of a polysiloxane defoaming agent, 0.08% of a polyacrylic thickener, 2% of a mixture of diethanolamine and triethanolamine in a mass ratio of 1:1, and 4% of a viscosity modifier, and the balance is water, with a total amount of 100%.

[0042] Example 5

[0043] A method for preparing a concrete surface beautifier comprises the following steps:

[0044] (1) Weigh an air entraining agent, a defoamer, a thickener, a water-soluble organic matter, a viscosity modifier and water according to any of the proportions in Examples 1-4;

[0045] (2) placing water-soluble organic matter in a reaction kettle, adding a thickener and a defoamer, and stirring evenly to obtain liquid A;

[0046] (3) Place water in another reaction kettle, add viscosity modifier, stir evenly at 40°C, then add air entraining agent, continue stirring evenly, and obtain liquid B;

[0047] (4) Liquid A was added to liquid B, and the mixture was heated to 60°C while stirring at a speed of 100 r / min, and the stirring was continued for 30 min. Then, the mixture was stirred at a speed of 200 r / min for 15 min. After the stirring was completed, the mixture was cooled to obtain a concrete surface beautifier.

[0048] Example 6

[0049] A method for preparing a concrete surface beautifier comprises the following steps:

[0050] (1) Weigh an air entraining agent, a defoamer, a thickener, a water-soluble organic matter, a viscosity modifier and water according to any of the proportions in Examples 1-4;

[0051] (2) placing water-soluble organic matter in a reaction kettle, adding a thickener and a defoamer, and stirring evenly to obtain liquid A;

[0052] (3) Place water in another reaction kettle, add viscosity modifier, stir evenly at 35°C, then add air entraining agent, continue stirring evenly, and obtain liquid B;

[0053] (4) Add liquid A to liquid B, raise the temperature to 55-65°C while stirring at a speed of 50 r / min, continue stirring for 40 min, then stir at a speed of 150 r / min for 20 min, cool down after stirring, and obtain a concrete surface beautifier.

[0054] Example 7

[0055] A method for preparing a concrete surface beautifier comprises the following steps:

[0056] (1) Weigh an air entraining agent, a defoamer, a thickener, a water-soluble organic matter, a viscosity modifier and water according to any of the proportions in Examples 1-4;

[0057] (2) placing water-soluble organic matter in a reaction kettle, adding a thickener and a defoamer, and stirring evenly to obtain liquid A;

[0058] (3) Place water in another reaction kettle, add viscosity modifier, stir evenly at 45°C, then add air entraining agent, continue stirring evenly, and obtain liquid B;

[0059] (4) Liquid A was added to liquid B, and the temperature was raised to 65°C while stirring at a speed of 150 r / min, and the stirring was continued for 20 min, and then stirred at a speed of 250 r / min for 10 min. After the stirring was completed, the temperature was lowered to obtain a concrete surface beautifier.

[0060] Example 8

[0061] The concrete mix ratio is shown in Table 1, wherein the formulations of the surface beautifiers are respectively those of Examples 1-4, and the preparation method is the method shown in Example 5. The experimental results of the surface quality of the obtained hardened concrete are shown in Table 2, which are respectively recorded as Example 1, Example 2, Example 3, and Example 4.

[0062] Table 1 Concrete mix ratio (C35) Unit: Kg / m 3

[0063] cement Fly ash sand Xiaoshi Zhongshi Dashi water Water reducing agent Surface beautifier 293 120 826 185 381 381 161 4.13 4.13

[0064] Table 2 Test results of concrete surface beautifier (C35)

[0065]

[0066]

[0067] a Number of large bubbles: the number of bubbles in hardened concrete with apparent bubble diameter greater than 2mm.

[0068] b Bubble count: the number of all bubbles on the surface of hardened concrete.

[0069] c Bubble area ratio: the ratio of the projected area of ​​all bubbles on the surface of hardened concrete to the area of ​​the measured area.

[0070] Example 9

[0071] The concrete mix ratio is shown in Table 3, wherein the formulations of the surface beautifiers are respectively those of Examples 1-4, and the preparation method is the method shown in Example 5. The experimental results of the surface quality of the obtained hardened concrete are shown in Table 4, which are respectively recorded as Example 1, Example 2, Example 3, and Example 4.

[0072] Table 3 Concrete mix ratio (C50) Unit: Kg / m 3

[0073]

[0074] Table 4 Test results of concrete surface beautifier (C50)

[0075]

[0076] a Number of large bubbles: the number of bubbles with a diameter greater than 2mm on the surface of hardened concrete.

[0077] b Bubble count: the number of all bubbles on the surface of hardened concrete.

[0078] c Bubble area ratio: the ratio of the projected area of ​​all bubbles on the surface of hardened concrete to the area of ​​the measured area.

[0079] It can be seen from the effects in Table 2 and Table 4 that the concrete surface beautifier prepared in Examples 1-4 can reduce the number of harmful large bubbles in concrete, maintain the stability of the air content of concrete, increase the fluidity of the concrete mixture, improve the workability of the concrete mixture, enhance the stability of the working performance of the concrete mixture, and can improve the mechanical properties of hardened concrete, optimize the morphology and structure of concrete bubbles, and improve the apparent quality of concrete.

[0080] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical solutions and inventive concepts of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A concrete surface beautifier, It is characterized in that Calculated by mass percentage, it comprises: 0.05-0.1% of air entraining agent, 0.1-0.2% of defoaming agent, 0.04-0.08% of thickener, 1-2% of water-soluble organic matter and 2-4% of viscosity modifier, and the balance is water.

2. The concrete surface beautifying agent according to claim 1, It is characterized in that Calculated by mass percentage, it includes: 0.08% of air entraining agent, 0.15% of defoaming agent, 0.06% of thickener, 1.5% of water-soluble organic matter and 3% of viscosity modifier, and the balance is water.

3. The concrete surface beautifying agent according to claim 1 or 2, Features: The air entraining agent is a polyether air entraining agent.

4. The concrete surface beautifying agent according to claim 1 or 2, Features: The defoamer is a polysiloxane defoamer.

5. The concrete surface beautifying agent according to claim 1 or 2, Features: The thickener is a polyacrylic acid thickener.

6. The concrete surface beautifying agent according to claim 1 or 2, Features: The water-soluble organic matter is a mixture of diethanolamine and triethanolamine.

7. The concrete surface beautifying agent according to claim 6, Features: The mixing mass ratio of the diethanolamine and triethanolamine is 1:

1.

8. A method for preparing the concrete surface beautifying agent according to any one of claims 1 to 7, It is characterized in that The steps include: (1) Weigh air entraining agent, defoamer, thickener, water-soluble organic matter, viscosity modifier and water according to the proportion; (2) placing water-soluble organic matter in a reaction kettle, adding a thickener and a defoamer, and stirring evenly to obtain liquid A; (3) Place water in another reaction kettle, add viscosity modifier, stir evenly at 35-45°C, then add air entraining agent, continue stirring evenly, and obtain liquid B; (4) Add liquid A to liquid B, raise the temperature to 55-65°C while stirring at a speed of 50-150 r / min, continue stirring for 20-40 min, then stir at a speed of 150-250 r / min for 10-20 min, cool down after stirring, and obtain a concrete surface beautifier.

9. The method for preparing the concrete surface beautifying agent according to claim 8, Features: In the step (3), the temperature during stirring is 40°C.

10. The method for preparing the concrete surface beautifying agent according to claim 8, Features: In the step (4), the temperature is first raised to 60° C. with stirring at a speed of 100 r / min, stirring is continued for 30 min, and then stirring is continued at a speed of 200 r / min for 15 min.