Fireproof air duct and preparation process thereof
A fireproof air duct with a blend of magnesium oxide, talc, periclase-spinel-Al refractory material, and microcapsule self-healing polymer addresses aging and mechanical weaknesses, enhancing fire resistance and durability, suitable for environments requiring high safety and cleanliness.
Patent Information
- Application Number
- CN202411216325.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-12-03
AI Technical Summary
Current fireproof air ducts face issues such as aging, cracking, insufficient adhesion and mechanical strength, complexity in installation, and potential release of harmful gases, which compromise fireproof performance and environmental safety.
A fireproof air duct composed of a blend of magnesium oxide, talc, wood shavings, periclase-spinel-Al refractory material, aerogel, and microcapsule self-healing polymer, along with specific flame retardants and anti-corrosion coatings, enhancing fire resistance, thermal insulation, mechanical strength, and antibacterial properties.
The duct exhibits improved fire resistance, thermal stability, mechanical durability, and antibacterial performance, reducing maintenance costs and extending service life while ensuring safety and air quality.
Smart Images

Figure CN119059761A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of fireproof air ducts, and in particular to a fireproof air duct and a preparation process thereof. Background Art
[0002] Air ducts are widely used in commercial buildings, industrial facilities, residential buildings, public places and special places to transport and distribute air and ensure indoor air quality and comfort. With the development of construction technology and the improvement of people's requirements for air quality, the air duct system is also constantly developing, moving towards a more efficient, energy-saving and environmentally friendly direction. Among them, fire-resistant air ducts, also known as fire-resistant air ducts, are air duct systems specially designed to maintain structural integrity and functionality in the event of a fire. They are widely used in high-rise buildings, underground facilities, tunnels and other places with strict fire protection requirements; the main function of fire-resistant air ducts is to prevent flames and harmful gases from spreading through the air ducts when a fire occurs, protect personnel safety and reduce property losses.
[0003] With the improvement of building fire protection standards and people's safety awareness, the technology of fire-resistant air ducts is also developing. From traditional metal air ducts coated with fire-resistant materials to modern high-performance composite air ducts, the performance and application range of fire-resistant air ducts have been significantly improved.
[0004] However, during the use of current fireproof air ducts, some fireproof coatings may age, crack or fall off during long-term use, affecting the fireproof performance; and the adhesion and mechanical strength of the coating and insulation materials are insufficient, and may be damaged under the impact of fire. Traditional metal fireproof air ducts are heavy and complex to install, which increases the difficulty and cost of construction, and some fireproof materials may release harmful gases at high temperatures, posing a threat to the environment and human health. Summary of the invention
[0005] Based on this, it is necessary to provide a fireproof air duct and its preparation process to address the above technical problems.
[0006] In a first aspect, the present invention provides a fireproof air duct, which comprises the following raw materials in parts by weight:
[0007] 35-55 parts of fire-resistant toughness substrate, 2-4 parts of polystyrene, 5-10 parts of emulsified oil, 8-14 parts of solid composite material, 2-4 parts of blended flame retardant, 3-8 parts of aerogel, 0.5-1 parts of ultraviolet stabilizer, 1-2 parts of antibacterial additive, 3-7 parts of self-healing material and 1-4 parts of anti-corrosion coating.
[0008] Furthermore, the refractory toughness substrate includes the following raw materials in parts by weight:
[0009] 20-30 parts of magnesium oxide, 10-15 parts of talc and 5-10 parts of wood shavings.
[0010] Among them, magnesium oxide (MgO) is the main component, providing high strength and fire resistance. Talc is used to enhance the toughness and processing properties of the material. Sawdust is used to increase the structural strength of the material while reducing weight.
[0011] Furthermore, the solid composite material is a periclase-spinel-Al refractory material.
[0012] Among them, periclase-spinel-Al refractory (MgO-Al2O3-Al) is a high-performance refractory material, in which special additives such as magnesium aluminum nitride (MgAlON) significantly improve the comprehensive performance of the material. MgAlON material has excellent high temperature performance, chemical corrosion resistance and high mechanical strength.
[0013] Periclase (MgO) has a high melting point (about 2800℃), good refractory properties and chemical corrosion resistance. It is the basic component of many refractory materials and provides basic high-temperature stability and thermal shock resistance. Spinel (MgAl2O3) is a composite oxide with high hardness, good thermal shock resistance and low thermal expansion coefficient. It has excellent refractory properties and can maintain structural stability under high temperature environments. Aluminum (Al) as an additive can generate new refractory phases (such as MgAlON) through reaction to improve the overall performance of the material. The introduction of aluminum can enhance the material's resistance to reducing atmospheres and chemical corrosion. Magnesium aluminum nitride (MgAlON) is a nitrogen-containing compound with high hardness, excellent wear resistance and thermal shock resistance. It is stable under high temperature environments and has strong resistance to both oxidizing and reducing atmospheres.
[0014] Furthermore, the blended flame retardant includes an organic flame retardant and an inorganic flame retardant in a mass ratio of 1:1;
[0015] The organic flame retardant includes at least one of ammonium polyphosphate, dimethyl methylphosphonate and melamine polyphosphate; the inorganic flame retardant includes at least one of expanded vermiculite, montmorillonite, zinc borate, expandable graphite and ferric oxide.
[0016] Furthermore, the aerogel includes at least one of alginate-calcium carbonate composite aerogel, polyvinyl alcohol aerogel and pectin aerogel.
[0017] Further, the ultraviolet stabilizer includes at least one of a UV stabilizer or diphenyl phosphite.
[0018] Furthermore, the antibacterial additive includes at least one of a silver ion compound, a zinc ion compound, ammonium persulfate and a mustard extract.
[0019] Furthermore, the self-healing material includes microcapsule self-healing polymer.
[0020] Among them, microcapsule self-healing polymer is a kind of smart material, which contains tiny capsules in the material to realize self-healing function. When the material is damaged, these capsules will break and release the repair agent inside to repair the cracks or damage. Microcapsule self-healing polymer includes microcapsules and body materials. Microcapsules include shell materials and new materials. Commonly used shell materials include polymers such as polyurea, polyurethane, phenolic resin, etc., which need to have sufficient mechanical strength and chemical stability to ensure that they are not destroyed prematurely during use. The core material, that is, the repair agent, includes monomers (such as epoxy resin, cyanate resin), catalysts or other chemicals.
[0021] Matrix Material is the main material in which the microcapsules are embedded, usually a polymer material such as epoxy resin, polyester resin or other high molecular materials.
[0022] Furthermore, the anti-corrosion coating includes epoxy resin coating, stainless steel powder and Teflon powder in a mass ratio of 5:1:1.
[0023] In a second aspect, the present invention further provides a preparation process for a fireproof air duct, the preparation process comprising the following steps:
[0024] S1. Weigh various types of raw materials according to their mass fractions;
[0025] S2, adding the fire-resistant toughness substrate, polystyrene, emulsified oil, solid composite material and solvent into the mixer, and mixing them thoroughly with a high-speed mixer to obtain a uniformly mixed main material;
[0026] S3. Gradually add the blended flame retardant, aerogel, UV stabilizer, antibacterial additive and self-healing material to the uniformly mixed main material, and continue stirring until completely mixed to obtain a paste-like mixture;
[0027] S4, pour the paste mixture on the surface of the acrylic board, spread it evenly to a preset size, and spread fiberglass cloth on the surface of the paste mixture, and move it to a drying room for dehydration;
[0028] S5, taking out the paste mixture that has been dehydrated to form a plate-like solid, cutting it into a preset size, and combining and fixing it with angle steel to obtain a finished air duct;
[0029] S6. Use anti-corrosion paint to spray evenly on the surface of the finished air duct to prepare a fireproof air duct.
[0030] The beneficial effects of the present invention are:
[0031] 1. The comprehensive performance of the air duct is significantly improved by the comprehensive application of fire-resistant tough substrate, polystyrene, emulsified oil, solid composite material, blended flame retardant, aerogel, UV stabilizer, antibacterial additive, self-healing material and anti-corrosion coating. Firstly, the addition of fire-resistant tough substrate and blended flame retardant makes the air duct show excellent fire resistance in high temperature environment, which can effectively prevent the spread of fire and improve the safety of buildings. Aerogel further enhances the thermal insulation performance of the air duct, ensuring that the internal temperature can be kept stable under extreme high temperature conditions to protect internal equipment and pipelines. Secondly, polystyrene and solid composite materials give the air duct high mechanical strength and impact resistance, increasing the durability and service life of the air duct. Emulsified oil improves the processability and surface finish of the material, making the air duct more convenient in the manufacturing and installation process. The application of UV stabilizer significantly improves the anti-aging performance of the air duct and prolongs its service life in outdoor exposure environment. Antibacterial additives ensure that the inner wall of the air duct has long-term antibacterial and mildew-proof functions to maintain air quality, which is particularly suitable for hospitals, laboratories and other places with high requirements for air cleanliness.
[0032] 2. The present invention is significantly superior to traditional air ducts in terms of fire resistance, thermal insulation, mechanical strength, durability, anti-aging, antibacterial, self-repairing and corrosion resistance. Its wide application can not only improve the safety and reliability of buildings and industrial facilities, but also bring significant economic benefits in reducing maintenance costs and extending service life, thus meeting the needs of modern buildings and industries for high-performance air ducts. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] The drawings described herein are used to provide a further understanding of the present invention and constitute a part of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:
[0034] Figure 1 The present invention is a flowchart of a process for preparing a fireproof air duct according to an embodiment of the present invention. DETAILED DESCRIPTION
[0035] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0036] Embodiment 1
[0037] A fireproof air duct, comprising the following raw materials in parts by weight:
[0038] 35g fire-resistant tough substrate, 2g polystyrene, 5g emulsified oil, 8g solid composite material, 2g blended flame retardant, 3g aerogel, 0.5g UV stabilizer, 1g antibacterial additive, 3g self-healing material and 1g anti-corrosion coating.
[0039] The fire-resistant toughness base material includes the following raw materials in parts by mass: 20 g of magnesium oxide, 10 g of talcum powder and 5 g of wood chaff.
[0040] The solid composite material is periclase-spinel-Al refractory material.
[0041] The blended flame retardant includes an organic flame retardant and an inorganic flame retardant in a mass ratio of 1:1;
[0042] Among them, the organic flame retardant is ammonium polyphosphate; the inorganic flame retardant is expanded vermiculite.
[0043] The aerogel is alginate-calcium carbonate composite aerogel.
[0044] UV stabilizers are UV stabilizers.
[0045] The antibacterial additive is a silver ion compound.
[0046] The self-healing material is a microcapsule self-healing polymer.
[0047] The anti-corrosion coating comprises epoxy resin coating, stainless steel powder and Teflon powder in a mass ratio of 5:1:1.
[0048] According to Figure 1 As shown, a preparation process of a fireproof air duct comprises the following steps:
[0049] S1. Weigh various types of raw materials according to their mass fractions;
[0050] S2, adding the fire-resistant toughness substrate, polystyrene, emulsified oil, solid composite material and solvent into the mixer, and mixing them thoroughly with a high-speed mixer to obtain a uniformly mixed main material;
[0051] S3. Gradually add the blended flame retardant, aerogel, UV stabilizer, antibacterial additive and self-healing material to the uniformly mixed main material, and continue stirring until completely mixed to obtain a paste-like mixture;
[0052] S4, pour the paste mixture on the surface of the acrylic board, spread it evenly to a preset size, and spread fiberglass cloth on the surface of the paste mixture, and move it to a drying room for dehydration;
[0053] S5, taking out the paste mixture that has been dehydrated to form a plate-like solid, cutting it into a preset size, and combining and fixing it with angle steel to obtain a finished air duct;
[0054] S6. Use anti-corrosion paint to spray evenly on the surface of the finished air duct to prepare a fireproof air duct.
[0055] Embodiment 2
[0056] A fireproof air duct, comprising the following raw materials in parts by weight:
[0057] 40g fire-resistant tough substrate, 2-4g polystyrene, 7g emulsified oil, 10g solid composite material, 3g blended flame retardant, 5g aerogel, 0.7g UV stabilizer, 1.3g antibacterial additive, 5g self-healing material and 2g anti-corrosion coating.
[0058] The fire-resistant toughness base material includes the following raw materials in parts by mass: 22 parts of magnesium oxide, 10 parts of talcum powder and 8 parts of wood chaff.
[0059] The solid composite material is periclase-spinel-Al refractory material.
[0060] The blended flame retardant includes an organic flame retardant and an inorganic flame retardant in a mass ratio of 1:1;
[0061] Among them, the organic flame retardant is ammonium polyphosphate; the inorganic flame retardant is expanded vermiculite.
[0062] The aerogel is alginate-calcium carbonate composite aerogel.
[0063] UV stabilizers are UV stabilizers.
[0064] The antibacterial additive is a silver ion compound.
[0065] The self-healing material is a microcapsule self-healing polymer.
[0066] The anti-corrosion coating comprises epoxy resin coating, stainless steel powder and Teflon powder in a mass ratio of 5:1:1.
[0067] According to Figure 1 As shown, a preparation process of a fireproof air duct comprises the following steps:
[0068] S1. Weigh various types of raw materials according to their mass fractions;
[0069] S2, adding the fire-resistant toughness substrate, polystyrene, emulsified oil, solid composite material and solvent into the mixer, and mixing them thoroughly with a high-speed mixer to obtain a uniformly mixed main material;
[0070] S3. Gradually add the blended flame retardant, aerogel, UV stabilizer, antibacterial additive and self-healing material to the uniformly mixed main material, and continue stirring until completely mixed to obtain a paste-like mixture;
[0071] S4, pour the paste mixture on the surface of the acrylic board, spread it evenly to a preset size, and spread fiberglass cloth on the surface of the paste mixture, and move it to a drying room for dehydration;
[0072] S5, taking out the paste mixture that has been dehydrated to form a plate-like solid, cutting it into a preset size, and combining and fixing it with angle steel to obtain a finished air duct;
[0073] S6. Use anti-corrosion paint to spray evenly on the surface of the finished air duct to prepare a fireproof air duct.
[0074] Embodiment 3
[0075] A fireproof air duct, comprising the following raw materials in parts by weight:
[0076] 50 parts of fire-resistant toughness substrate, 3 parts of polystyrene, 8 parts of emulsified oil, 12 parts of solid composite material, 3 parts of blended flame retardant, 6 parts of aerogel, 0.8 parts of UV stabilizer, 1.8 parts of antibacterial additive, 6 parts of self-healing material and 3 parts of anti-corrosion coating.
[0077] The fire-resistant toughness base material includes the following raw materials in parts by weight: 25 g of magnesium oxide, 15 g of talcum powder and 10 g of wood chaff.
[0078] The solid composite material is periclase-spinel-Al refractory material.
[0079] The blended flame retardant includes an organic flame retardant and an inorganic flame retardant in a mass ratio of 1:1;
[0080] Among them, the organic flame retardant is ammonium polyphosphate; the inorganic flame retardant is expanded vermiculite.
[0081] The aerogel is alginate-calcium carbonate composite aerogel.
[0082] UV stabilizers are UV stabilizers.
[0083] The antibacterial additive is a silver ion compound.
[0084] The self-healing material is a microcapsule self-healing polymer.
[0085] The anti-corrosion coating comprises epoxy resin coating, stainless steel powder and Teflon powder in a mass ratio of 5:1:1.
[0086] According to Figure 1 As shown, a preparation process of a fireproof air duct comprises the following steps:
[0087] S1. Weigh various types of raw materials according to their mass fractions;
[0088] S2, adding the fire-resistant toughness substrate, polystyrene, emulsified oil, solid composite material and solvent into the mixer, and mixing them thoroughly with a high-speed mixer to obtain a uniformly mixed main material;
[0089] S3. Gradually add the blended flame retardant, aerogel, UV stabilizer, antibacterial additive and self-healing material to the uniformly mixed main material, and continue stirring until completely mixed to obtain a paste-like mixture;
[0090] S4, pour the paste mixture on the surface of the acrylic board, spread it evenly to a preset size, and spread fiberglass cloth on the surface of the paste mixture, and move it to a drying room for dehydration;
[0091] S5, taking out the paste mixture that has been dehydrated to form a plate-like solid, cutting it into a preset size, and combining and fixing it with angle steel to obtain a finished air duct;
[0092] S6. Use anti-corrosion paint to spray evenly on the surface of the finished air duct to prepare a fireproof air duct.
[0093] Embodiment 4
[0094] A fireproof air duct, comprising the following raw materials in parts by weight:
[0095] 55g fire-resistant tough substrate, 4g polystyrene, 10g emulsified oil, 14g solid composite material, 4g blended flame retardant, 8g aerogel, 1g UV stabilizer, 2g antibacterial additive, 7g self-healing material and 4g anti-corrosion coating.
[0096] The fire-resistant toughness base material includes the following raw materials in parts by weight: 30 g of magnesium oxide, 15 g of talcum powder and 10 g of wood chaff.
[0097] The solid composite material is periclase-spinel-Al refractory material.
[0098] The blended flame retardant includes an organic flame retardant and an inorganic flame retardant in a mass ratio of 1:1;
[0099] Among them, the organic flame retardant is ammonium polyphosphate; the inorganic flame retardant is expanded vermiculite.
[0100] The aerogel is alginate-calcium carbonate composite aerogel.
[0101] UV stabilizers are UV stabilizers.
[0102] The antibacterial additive is a silver ion compound.
[0103] The self-healing material is a microcapsule self-healing polymer.
[0104] The anti-corrosion coating comprises epoxy resin coating, stainless steel powder and Teflon powder in a mass ratio of 5:1:1.
[0105] According to Figure 1 As shown, a preparation process of a fireproof air duct comprises the following steps:
[0106] S1. Weigh various types of raw materials according to their mass fractions;
[0107] S2, adding the fire-resistant toughness substrate, polystyrene, emulsified oil, solid composite material and solvent into the mixer, and mixing them thoroughly with a high-speed mixer to obtain a uniformly mixed main material;
[0108] S3. Gradually add the blended flame retardant, aerogel, UV stabilizer, antibacterial additive and self-healing material to the uniformly mixed main material, and continue stirring until completely mixed to obtain a paste-like mixture;
[0109] S4, pour the paste mixture on the surface of the acrylic board, spread it evenly to a preset size, and spread fiberglass cloth on the surface of the paste mixture, and move it to a drying room for dehydration;
[0110] S5, taking out the paste mixture that has been dehydrated to form a plate-like solid, cutting it into a preset size, and combining and fixing it with angle steel to obtain a finished air duct;
[0111] S6. Use anti-corrosion paint to spray evenly on the surface of the finished air duct to prepare a fireproof air duct.
[0112] Comparative Example 1
[0113] This comparative example provides a fireproof air duct, which is made of the following raw materials in parts by weight:
[0114] 55g fire-resistant tough substrate, 4g polystyrene, 10g emulsified oil, 14g solid composite material, 1g UV stabilizer, 2g antibacterial additive, 7g self-healing material and 4g anti-corrosion coating.
[0115] Comparative Example 2
[0116] This comparative example provides a fireproof air duct, which is made of the following raw materials in parts by weight:
[0117] 55g fire-resistant tough substrate, 4g polystyrene, 10g emulsified oil, 4g blended flame retardant, 8g aerogel, 1g UV stabilizer, 2g antibacterial additive and 7g self-healing material.
[0118] The fireproof air ducts prepared in Examples 1, 2, 3, 4 and Comparative Examples 1 and 2 were subjected to performance tests, mainly including physical properties such as appearance and weight. The specific test results are shown in Table 1.
[0119] Table 1: Performance test table of examples and comparative examples
[0120] Appearance Tolerance temperature / ℃ Embodiment 1 The surface of the air duct is smooth, without cracks or falling pieces. 2436 Embodiment 2 The surface of the air duct is smooth, without cracks or falling pieces. 2445 Embodiment 3 The surface of the air duct is smooth, without cracks or falling pieces. 2502 Embodiment 4 The surface of the air duct is smooth, without cracks or falling pieces. 2561 Comparative Example 1 There are cracks on the surface of the air duct 1556 Comparative Example 2 There are cracks and pieces falling off on the duct surface, and the surface is rough. 1962
[0121] It can be seen from the above results that the fireproof air duct of the present invention, thanks to the advantages of mixing multiple materials, has the characteristics of smooth surface, strong adhesion and stable structure, and has excellent heat resistance and thermal stability.
[0122] In summary, with the help of the above technical scheme of the present invention, the comprehensive performance of the air duct is significantly improved by comprehensively applying the fire-resistant tough substrate, polystyrene, emulsified oil, solid composite material, blended flame retardant, aerogel, ultraviolet stabilizer, antibacterial additive, self-healing material and anti-corrosion coating; firstly, the addition of the fire-resistant tough substrate and the blended flame retardant enables the air duct to exhibit excellent fire resistance in a high temperature environment, which can effectively prevent the spread of fire and improve the safety of the building; the aerogel further enhances the thermal insulation performance of the air duct, ensuring that the internal temperature can remain stable under extreme high temperature conditions and protect the internal equipment and pipelines; secondly, polystyrene and solid composite materials enable the air duct to have higher mechanical strength and impact resistance, and increase the durability and service life of the air duct; the emulsified oil improves the processability and surface finish of the material, making the air duct more convenient in the manufacturing and installation process; the application of ultraviolet stabilizer significantly improves the anti-aging performance of the air duct and extends its service life in outdoor exposure environment; the antibacterial additive ensures that the inner wall of the air duct has a long-term antibacterial and mildew-proof function to maintain air quality, which is particularly suitable for hospitals, laboratories and other places with high requirements for air cleanliness. The present invention is significantly superior to traditional air ducts in terms of fire resistance, heat insulation, mechanical strength, durability, anti-aging, antibacterial, self-repairing and corrosion resistance. Its wide application can not only improve the safety and reliability of buildings and industrial facilities, but also bring significant economic benefits in reducing maintenance costs and extending service life, thus meeting the needs of modern buildings and industries for high-performance air ducts.
[0123] It should be understood that, although the steps in the flowchart of the accompanying drawings are displayed in sequence as indicated by the arrows, these steps are not necessarily executed in sequence in the order indicated by the arrows. Unless otherwise specified herein, there is no strict order restriction on the execution of these steps, and they can be executed in other orders. Moreover, at least a part of the steps in the flowchart of the accompanying drawings may include multiple sub-steps or multiple stages, and these sub-steps or stages are not necessarily executed at the same time, but can be executed at different times, and their execution order is not necessarily sequential, but can be executed in turn or alternately with other steps or at least a part of the sub-steps or stages of other steps.
Claims
1. A fireproof air duct, characterized in that: The fireproof air duct includes the following raw materials by mass: 35-55 parts of fire-resistant toughness substrate, 2-4 parts of polystyrene, 5-10 parts of emulsified oil, 8-14 parts of solid composite material, 2-4 parts of blended flame retardant, 3-8 parts of aerogel, 0.5-1 parts of ultraviolet stabilizer, 1-2 parts of antibacterial additive, 3-7 parts of self-healing material and 1-4 parts of anti-corrosion coating.
2. A fireproof air duct according to claim 1, characterized in that: The refractory toughness substrate comprises the following raw materials in parts by mass: 20-30 parts of magnesium oxide, 10-15 parts of talc and 5-10 parts of wood shavings.
3. A fireproof air duct according to claim 1, characterized in that: The solid composite material is a periclase-spinel-Al refractory material.
4. A fireproof air duct according to claim 1, characterized in that: The blended flame retardant comprises an organic flame retardant and an inorganic flame retardant in a mass ratio of 1:1; The organic flame retardant includes at least one of ammonium polyphosphate, dimethyl methylphosphonate and melamine polyphosphate; the inorganic flame retardant includes at least one of expanded vermiculite, montmorillonite, zinc borate, expandable graphite and ferric oxide.
5. A fireproof air duct according to claim 1, characterized in that: The aerogel includes at least one of alginate-calcium carbonate composite aerogel, polyvinyl alcohol aerogel and pectin aerogel.
6. A fireproof air duct according to claim 1, characterized in that: The ultraviolet stabilizer includes at least one of a UV stabilizer or diphenyl phosphite.
7. A fireproof air duct according to claim 1, characterized in that: The antibacterial additive includes at least one of a silver ion compound, a zinc ion compound, ammonium persulfate and a mustard extract.
8. The fireproof air duct according to claim 1, characterized in that: The self-healing material comprises a microcapsule self-healing polymer.
9. The fireproof air duct according to claim 1, characterized in that: The anti-corrosion coating comprises epoxy resin coating, stainless steel powder and Teflon powder in a mass ratio of 5:1:
1.
10. A process for preparing a fireproof air duct, used for preparing the fireproof air duct according to any one of claims 1 to 9, characterized in that: The preparation process comprises the following steps: S1. Weigh various types of raw materials according to their mass fractions; S2, adding the fire-resistant toughness substrate, polystyrene, emulsified oil, solid composite material and solvent into the mixer, and mixing them thoroughly with a high-speed mixer to obtain a uniformly mixed main material; S3. Gradually add the blended flame retardant, aerogel, UV stabilizer, antibacterial additive and self-healing material to the uniformly mixed main material, and continue stirring until completely mixed to obtain a paste-like mixture; S4, pour the paste mixture on the surface of the acrylic board, spread it evenly to a preset size, and spread fiberglass cloth on the surface of the paste mixture, and move it to a drying room for dehydration; S5, taking out the paste mixture that has been dehydrated to form a plate-like solid, cutting it into a preset size, and combining and fixing it with angle steel to obtain a finished air duct; S6. Use anti-corrosion paint to spray evenly on the surface of the finished air duct to prepare a fireproof air duct.