High-solid-phase strong-stability goaf solid waste filling slurry, preparation system and preparation method
By combining powder-grained coal gangue powder and fine-grained coal gangue powder, a high-solid-phase strong stable slurry with harmful substance curing agent and stabilizer is prepared, which solves the poor stability of coal gangue powder slurry in the filling of goaf and short pumping distance of coal gangue powder slurry. The problem of this has achieved efficient and stable goaf filling and pollution control.
Patent Information
- Application Number
- CN202411173207.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-12-03
AI Technical Summary
The existing coal gangue powder slurry has problems such as poor stability, short pumping distance and low filling efficiency when filling goafs, which cannot meet the needs of efficient filling goafs.
The solid waste filling slurry of high-solid-phase strong stable goaf prepared by combining powder-grained coal gangue powder and fine-grained coal gangue powder, and harmful substance curing agents, dispersants and stabilizers. Through the combination of particle size grading and combination agents, Achieve long-distance pumping and efficient filling.
The stability and filling efficiency of the slurry are improved, and the residual cracks and holes in the goaf can be effectively filled, the risk of groundwater pollution is reduced, and the fluidity and diffusion distance of the slurry are improved.
Smart Images

Figure CN119059792A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of coal gangue solid waste disposal and coal mine goaf filling, and specifically to a high-solid phase and highly stable goaf solid waste filling slurry, a preparation system and a preparation method. Background Art
[0002] Coal mining in western my country has left behind a large number of goafs. Geological disasters in goafs such as ground collapse and ground fissures seriously threaten the safety of ground structures. At the same time, coal gangue produced by coal mining is the solid waste with the largest annual emission, the largest land occupation, and the most serious environmental pollution among various industrial waste residues in my country. At present, my country's coal gangue is growing at an annual emission rate of 150 to 200 million tons, which has brought severe challenges to the ecological and environmental protection of mining areas. The residual voids (including cavities, fissures and pores) in coal mine goafs and overburden are complex. The goafs were partially filled after the overburden broke and collapsed; at the same time, some mining-induced fissures were closed under the action of mine pressure. Due to the presence of overburden collapse accumulation in the goafs, there is a clear difference between coal mine goafs and open voids such as abandoned tunnels and karst caves.
[0003] Gangue powder slurry is the main slurry material for filling goaf with coal gangue. It is made of gangue powder, water and additives. Since coal gangue contains heavy metals such as lead, mercury, arsenic and other harmful substances, direct slurry filling has the risk of groundwater pollution. On the other hand, gangue powder is a granular material. The suspension ability of gangue powder particles in slurry is poor, and it is very easy to separate and precipitate, causing pipe blockage. At the same time, in the cracks, due to the existence of the permeability effect, the diffusion distance of the granular gangue powder slurry is small. In order to improve the stability of gangue powder slurry, existing additives include bentonite, coal slime, xanthan gum and other materials. However, while the stability of the slurry is improved, its fluidity becomes worse, making it difficult to pump the gangue powder slurry over long distances, accumulating too quickly in the goaf, and the injection volume of a single hole is too low, resulting in low grouting filling efficiency.
[0004] In summary, it was found in production practice that ordinary gangue powder slurry has problems such as poor stability, short pumping distance, low filling efficiency and groundwater pollution when filling goaf, and cannot meet the needs of returning gangue powder solid waste slurry to the well to efficiently fill goaf. Summary of the invention
[0005] To this end, the technical problem to be solved by the present invention is to provide a high-solid phase and highly stable goaf solid waste filling slurry, a preparation system and a preparation method with long pumping distance, good stability and high filling efficiency.
[0006] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0007] A high-solid phase and highly stable solid waste filling slurry for goaf areas, composed of the following components: powdered coal gangue powder, fine-grained coal gangue powder, a harmful substance curing agent, a dispersant, a stabilizer and water; the weight parts of each component in the solid waste filling slurry are: 200-500 weight parts of powdered coal gangue powder, 300-600 weight parts of fine-grained coal gangue powder, 5-30 weight parts of harmful substance curing agent, 3-15 weight parts of dispersant, 0.75-20 weight parts of stabilizer, and 600-800 weight parts of water.
[0008] The above-mentioned high-solid phase strong stable goaf solid waste filling slurry, the preparation method of the powdered coal gangue powder is: the coal gangue is crushed into stone particles, and then the powder is ground by a grinding device and then sieved to obtain the powder; the particle size of the coal gangue after the coal gangue is crushed is not more than 30mm, the grinding device adopts a vertical roller mill, and the particle size is controlled to be 10-50μm;
[0009] The preparation method of fine-grained coal gangue powder is as follows: the coal gangue is crushed into stone particles, and then the powder is ground by a grinding device and then sieved to obtain the powder; the particle size of the crushed coal gangue is not greater than 30 mm, the grinding device adopts a Raymond mill, and the particle size is controlled to be 50-100 μm.
[0010] By utilizing the particle size grading of powdered coal gangue powder and fine-grained coal gangue powder, the application scope of the solid waste filling slurry of the present application can be expanded. It can not only fill the residual voids in the goaf such as the waste tunnels in the large space and the overlying rock strata, but also fill the residual voids in the residual cracks caused by mining and the small gaps in the goaf caving areas.
[0011] The combination of powdered coal gangue powder and fine-grained coal gangue powder, dispersants and stabilizers can not only achieve long-distance pumping, but also effectively fill cracks of different apertures. According to the specific filling needs and pumping distance, the ratio of powdered coal gangue powder and fine-grained coal gangue powder, the amount and order of dispersants and stabilizers can be adjusted to achieve low-cost and efficient filling.
[0012] In the above-mentioned high solid phase strong stable goaf solid waste filling slurry, the harmful substance curing agent is one or a mixture of two or more of kaolin powder, polysilicon iron zinc, and diatomaceous earth; the mass ratio of kaolin powder, diatomaceous earth, and polysilicon iron zinc is 0-5:0-1:3-4. Kaolin and diatomaceous earth are heavy metal adsorbents that can adsorb heavy metal elements such as mercury, lead, cadmium, chromium, and copper. Polysilicon iron zinc is a coagulant that can treat heavy metal elements such as lead, cadmium, chromium, and copper.
[0013] The above-mentioned high-solid phase and highly stable solid waste filling slurry in goaf has a dispersant of one or two of sodium sulfonated humate and sodium polycarboxylate, and the mass ratio of sodium sulfonated humate and sodium polycarboxylate is 1:0.5-1.
[0014] The above-mentioned high-solid phase strongly stable goaf solid waste filling slurry, the stabilizer is one or a mixture of two or more of polyacrylamide, sodium tripolyphosphate and high-viscosity carboxymethyl cellulose, and the mass ratio of polyacrylamide, sodium tripolyphosphate and high-viscosity carboxymethyl cellulose is 0-0.6:0-0.1:1-10. At present, xanthan gum and bentonite are mostly used as stabilizers in the industry. Xanthan gum solution has the characteristics of low concentration and high viscosity and is widely used; however, the prices of xanthan gum and bentonite are relatively high. This application can achieve better stabilization effect by adjusting the dosage ratio of polyacrylamide, sodium tripolyphosphate and high-viscosity carboxymethyl cellulose.
[0015] Both sodium sulfonated humate and sodium polycarboxylate have good dispersibility and surface activity. The function of the dispersant is to allow the powder to mix quickly with water to form a suspension, reduce the amount of water to a certain extent, and increase the proportion of solid phase.
[0016] However, dispersants cannot ensure the stability of the slurry. If stirring is stopped, solid particles will precipitate, which can easily cause pipe blockage during long-distance pumping. Therefore, dispersants and stabilizers need to be used together. Stabilizers and dispersants will affect the viscosity of the finished slurry. Stabilizers are used to increase viscosity and prevent solid particles from settling too quickly, while dispersants can reduce viscosity. When dispersants or stabilizers are used alone, it is difficult to ensure the stability and dispersibility of the slurry.
[0017] A preparation system for high-solid-phase and highly stable solid waste filling slurry in goafs, comprising a gangue crushing system, a gangue powder grinding and screening system, and a gangue powder storage system arranged in a gangue continuous crushing and screening workshop; a material weighing and metering system, a high-solid-phase gangue powder-based slurry preparation system, and a high-solid-phase and highly stable solid waste slurry preparation system arranged in a digital pulping workshop; the gangue crushing system is a gangue crusher, and the gangue powder storage system comprises a vertical roller mill and a Raymond mill; the gangue powder storage system comprises a fine-grained gangue powder storage tank and a powdered gangue powder storage tank; the material weighing and metering system comprises a screw feeder and a metering and weighing device; the high-solid-phase gangue powder-based slurry preparation system comprises a clear water tank, a primary stirring tank, and an ultrasonic dispersing mixer; the high-solid-phase and highly stable solid waste slurry preparation system comprises a secondary stirring tank and a high-speed vortex mixer;
[0018] The gangue crusher crushes the gangue to obtain crushed stone particles, which are respectively sent to the vertical roller mill and the Raymond mill for grinding and screening to obtain powdered gangue powder and fine-grained gangue powder. The powdered gangue powder and fine-grained gangue powder are respectively transferred to the powdered gangue powder storage tank and the fine-grained gangue powder storage tank for storage; the powdered gangue powder in the powdered gangue powder storage tank and the fine-grained gangue powder in the fine-grained gangue powder storage tank are respectively fed into the The mixture is weighed on a metering weighing device, and a harmful substance curing agent is added to obtain a mixture. After weighing, the mixture is sent to a primary stirring tank, clean water is pumped into the clean water tank, and after adding a dispersant, it is stirred using an ultrasonic disperser to obtain a high-solid phase coal gangue powder-based slurry. The high-solid phase coal gangue powder-based slurry is transferred to a secondary stirring tank, and after adding a stabilizer, it is stirred using a high-speed vortex mixer to obtain a high-solid phase and strongly stable solid waste filling slurry.
[0019] The method for preparing the high-solid-phase and highly stable solid waste filling slurry for goaf area mentioned above adopts the above-mentioned preparation system to prepare the high-solid-phase and highly stable solid waste filling slurry for goaf area, comprising the following steps:
[0020] (A) Crushing, grinding, screening and storage of gangue raw materials: A continuous gangue crushing and screening workshop is built near the gangue mountain or gangue silo; the gangue raw materials are sent to the gangue crusher for crushing, and the gangue is graded and crushed to obtain crushed stone particles with a particle size of 0 to 30 mm; the crushed stone particles are respectively sent to the vertical roller mill and Raymond mill for grinding and screening to obtain powdered gangue powder and fine-grained gangue powder, and the powdered gangue powder and fine-grained gangue powder are respectively transferred to the powdered gangue powder storage tank and the fine-grained gangue powder storage tank for storage;
[0021] (B) Conveying, metering and mixing pretreatment of powdered gangue powder and fine-grained gangue powder: the powdered gangue powder in the powdered gangue powder storage tank and the fine-grained gangue powder in the fine-grained gangue powder storage tank are respectively fed into the metering weighing device through a screw feeder for weighing, and the harmful substance curing agent is added to the metering weighing device for weighing; then, the pretreatment is carried out by using an ultrasonic mixer to mix uniformly to obtain a mixture;
[0022] (C) primary stirring to prepare high solid phase coal gangue powder based slurry: the mixture is sent from an ultrasonic mixer into a primary stirring tank, and then pumped into water in a clean water tank, a dispersant is added, and an ultrasonic dispersing mixer is used to stir and slurry to obtain a high solid phase coal gangue powder based slurry;
[0023] (D) Secondary stirring to prepare high-solid phase highly stable solid waste filling slurry: The high-solid phase coal gangue powder-based slurry is transferred to the secondary stirring tank, and after adding the stabilizer, it is stirred and slurried using a high-speed vortex mixer to obtain a high-solid phase highly stable solid waste filling slurry.
[0024] The harmful substance curing agent, dispersant and stabilizer are added in steps. On the one hand, because there is a potential reaction process between the dispersant and the stabilizer, adding them at the same time will affect the dispersion of the gangue powder particles; on the other hand, the powder of the harmful substance curing agent is first mixed with the powdered coal gangue powder and the fine-grained coal gangue powder, and then the dispersant is added to prepare a high-solid coal gangue powder-based slurry. Then, the type and amount of the stabilizer need to be selected according to the requirements of coal gangue consumption, filling grouting requirements, slurry pumping distance, etc., so as to cooperate with the powdered coal gangue powder and fine-grained coal gangue powder of different particle sizes and the dispersant to obtain a high-solid phase and strongly stable solid waste filling slurry with controllable pumping distance and filling requirements.
[0025] In the above-mentioned method for preparing a high-solid phase and highly stable solid waste filling slurry for goaf areas, in step (A), a powdered coal gangue powder with a particle size range of 10 to 50 μm is obtained after grinding with a vertical roller mill; and a fine-grained coal gangue powder with a particle size range of 50 to 100 μm is obtained after grinding with a Raymond mill.
[0026] In the above-mentioned method for preparing a high-solid phase and highly stable solid waste filling slurry for goaf areas, in step (B), the amount of powdered coal gangue powder added is 200 to 500 parts by weight, and the amount of fine-grained coal gangue powder added is 200 to 600 parts by weight; the amount of harmful substance curing agent added is 5 to 30 parts by weight; the harmful substance curing agent is one or a mixture of two or more of kaolin powder, polysilicon iron zinc, and diatomaceous earth; the mass ratio of kaolin powder, polysilicon iron zinc, and diatomaceous earth is 0:3:1 to 5:4:0.
[0027] In the above-mentioned method for preparing a high-solid phase and highly stable solid waste filling slurry for goaf areas, in step (C), the amount of the dispersant added is 3 to 15 parts by weight; the amount of water added is 600 to 800 parts by weight; the dispersant is one or both of sulfonated sodium humate and sodium polycarboxylate, and the mass ratio of sulfonated sodium humate to sodium polycarboxylate is 1:0.5 to 1:1;
[0028] In step (D), the amount of stabilizer added is 0.75 to 20 parts by weight; the stabilizer is one or a mixture of two or more of polyacrylamide, sodium tripolyphosphate and high-viscosity carboxymethyl cellulose, and the mass ratio of polyacrylamide, sodium tripolyphosphate and high-viscosity carboxymethyl cellulose is 0:0:10 to 0.6:0.1:1.
[0029] The technical solution of the present invention achieves the following beneficial technical effects:
[0030] 1. The high-solid phase highly stable solid waste slurry does not require the addition of cement-based cementitious materials, has the advantages of good stability, low water separation rate and long diffusion distance, and can effectively fill the residual cracks and holes in the goaf. The high-solid phase highly stable solid waste slurry and its preparation process are suitable for filling goaf areas and coal gangue solid waste disposal in western my country, realizing green mining of coal mines.
[0031] 2. The high-solid phase and highly stable solid waste slurry prepared in this application can be used to fill residual cavities in coal mine goafs, such as abandoned tunnels, goaf caving areas, mining fissures, and overburden delamination.
[0032] 3. This application uses two types of coal gangue powder as raw materials: powdered coal gangue powder with a particle size range of 10 to 50 μm and fine-grained coal gangue powder with a particle size range of 50 to 100 μm; a harmful substance solidifier is used to eliminate toxic and harmful substances such as heavy metals in the coal gangue powder.
[0033] In the slurry preparation process, dispersants are used to increase the solid content in the slurry, and stabilizers are used to improve the stability of the slurry. At the same time, the slurry is made by two-stage stirring. The first stage of slurrying uses ultrasonic dispersing mixer to beat the slurry, combining ultrasonic energy with mechanical stirring to avoid powder agglomeration under the action of cavitation effect and mechanical shearing, so that the gangue powder is better dispersed. The second stage is high-speed vortex slurrying. The high-solid gangue powder-based slurry prepared in the first stage is transferred to the second-stage mixing tank, stabilizer is added, and high-speed vortex slurry is used to finally obtain the finished product of high-solid and highly stable coal gangue powder solid waste slurry.
[0034] 4. Two kinds of coal gangue powder with different particle sizes take into account the plastic strength of fine-grained coal gangue powder and the excellent filling permeability of fine-grained coal gangue powder;
[0035] Using sodium sulfonated humate and sodium polycarboxylate as dispersants, they have the advantage of high surface activity, adsorbing on the surface of coal gangue powder particles and reducing the interaction between coal gangue powder particles, reducing agglomeration, and increasing the proportion of coal gangue powder solid phase in the slurry;
[0036] Using polyacrylamide, sodium tripolyphosphate and high-viscosity carboxymethyl cellulose as stabilizers has the advantage of good suspension performance, which can effectively prevent the solid phase particles of gangue powder from settling in the pipeline, realize the long-distance pumping of high-solid phase coal gangue powder slurry, increase the diffusion filling distance, and improve the filling efficiency.
[0037] Dispersants and stabilizers are used together. Stabilizers and dispersants will affect the viscosity of the finished slurry. Stabilizers are used to increase viscosity and prevent solid particles from settling too quickly, while dispersants can reduce viscosity. Dispersants and stabilizers need to be used together, and the amount and order of added dispersants and stabilizers should be adjusted to ensure that the filling slurry has good dispersibility and a certain viscosity, which can achieve long-distance pumping and effective filling and diffusion. When dispersants or stabilizers are used alone, it is difficult to ensure the stability and dispersibility of the slurry.
[0038] This application utilizes the combination of different powdered coal gangue powders and fine-grained coal gangue powders, adjusts the weight, ratio and addition order of the dispersant and stabilizer, and adds a harmful substance solidifier to eliminate the potential risk of groundwater pollution. The prepared high-solid phase and highly stable goaf solid waste filling slurry can be pumped over long distances, with a pumping distance of more than 4,500 meters, a diffusion distance of more than 60 meters, and a continuous grouting time of up to 50 hours without any pipe blockage accidents caused by coal gangue powder precipitation. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 A schematic structural diagram of a system for preparing a high-solid-phase, highly stable goaf solid waste filling slurry according to the present invention.
[0040] The reference numerals in the figure are as follows: 1-coal gangue crusher; 2-vertical roller mill; 3-Raymond mill; 4-powdered coal gangue powder storage tank; 5-fine-grained coal gangue powder storage tank; 6-screw feeder; 7-harmful substance solidifying agent; 8-metering and weighing device; 9-dispersant; 10-primary stirring tank; 11-ultrasonic dispersing mixer; 12-clear water tank; 13-stabilizer; 14-secondary stirring tank; 15-high-speed vortex mixer. DETAILED DESCRIPTION
[0041] Example 1: High-solid-phase strongly stable coal gangue powder solid waste slurry and slurry making process for the filling project of the caving zone in a coal mine goaf in the west
[0042] The high-solid phase strongly stable coal gangue powder solid waste slurry used in this embodiment is composed of 500kg of powdered coal gangue powder, 300kg of fine coal gangue powder, 10kg of harmful substance curing agent, 5kg of dispersant, 0.75kg of stabilizer and 750kg of clean water. The components are detailed in Table 1.
[0043] The harmful substance curing agent is polysilicon zinc iron and diatomaceous earth, and the mass ratio of polysilicon zinc iron and diatomaceous earth is 3:1; the dispersant is sodium sulfonated humate; the stabilizer is a mixture of polyacrylamide, sodium tripolyphosphate and high-viscosity carboxymethyl cellulose, and the mass ratio of polyacrylamide, sodium tripolyphosphate and high-viscosity carboxymethyl cellulose is 0.2:0.07:1.
[0044] Table 1
[0045] Components Powdered coal gangue powder Fine coal gangue powder Hazardous substance curing agent Dispersants Stabilizer Shimizu Dosage / kg 500 300 10 5 0.75 750
[0046] The process for preparing high solid phase strong stable coal gangue powder solid waste slurry for filling the caving zone of coal mine goaf includes the following steps:
[0047] (A) Crushing, grinding, screening and storage of gangue raw materials: A continuous gangue crushing and screening workshop is established near the gangue mountain or gangue silo; the gangue raw materials are sent to the gangue crusher 1 for crushing, and the gangue is graded and crushed to obtain crushed stone particles with a particle size of 0 to 30 mm; the crushed stone particles are respectively sent to the vertical roller mill 2 and the Raymond mill 3 for grinding and screening to obtain powdered gangue powder and fine-grained gangue powder, and the powdered gangue powder and fine-grained gangue powder are respectively transferred to the powdered gangue powder storage tank 4 and the fine-grained gangue powder storage tank 5 for storage; after grinding in the vertical roller mill 2, powdered gangue powder with a particle size range of 10 to 50 μm is obtained; after grinding in the Raymond mill 3, fine-grained gangue powder with a particle size range of 50 to 100 μm is obtained.
[0048] (B) Conveying, metering and mixing pretreatment of powdered coal gangue powder and fine-grained coal gangue powder: The powdered coal gangue powder in the powdered coal gangue powder storage tank 4 and the fine-grained coal gangue powder in the fine-grained coal gangue powder storage tank 5 are fed by a screw feeder 6 and sent to a metering weighing device 8 for weighing, with 500 kg of powdered coal gangue powder and 300 kg of fine-grained coal gangue powder; 10 kg of harmful substance curing agent 7 is added; then, an ultrasonic mixer is used for pretreatment and mixing to obtain a mixture.
[0049] (C) Primary stirring to prepare high solid phase coal gangue powder based slurry: the mixed powder in step (B) is sent from the ultrasonic mixer to the primary stirring tank 10, and then pumped into 750 kg of water in the clear water tank 12, 5 kg of dispersant sodium sulfonated humate is added, and the mixture is stirred and slurried by an ultrasonic dispersing mixer 11 to obtain a high solid phase coal gangue powder based slurry;
[0050] (D) Secondary stirring, preparation of high-solid phase highly stable solid waste filling slurry: The high-solid phase coal gangue powder-based slurry prepared in step (C) is transferred to the secondary stirring tank 14, and after adding the stabilizer, it is stirred and slurried by a high-speed vortex mixer 15 to obtain a high-solid phase highly stable solid waste filling slurry. The high-solid phase highly stable coal gangue powder solid waste slurry prepared in Example 1 is used for the filling project of the caving zone in the goaf area. The test results show that the slurry funnel viscosity is 55s and the 24h water separation rate is 0.8%. The slurry pumping distance is 3500m, the continuous grouting time is 50h, and there is no pipe blockage accident caused by coal gangue powder precipitation in the slurry pipeline; the slurry diffusion distance exceeds 40m, and the single injection volume exceeds 1200m 3 The test mold was used to retain the sample, and the 28-day compressive strength of the slurry consolidation body was 2.8 MPa (the 28-day compressive strength of the goaf filling is required to be greater than 2.5 MPa).
[0051] Example 2: High-solid-phase and highly stable coal gangue powder solid waste slurry and slurry making process for filling the separation zone of a coal mine goaf in the west
[0052] The high solid phase strongly stable coal gangue powder solid waste slurry used in this embodiment is composed of 250kg of powdered coal gangue powder, 550kg of fine coal gangue powder, 25kg of harmful substance curing agent, 6.5kg of dispersant, 3.5kg of stabilizer and 750kg of clean water. The components are detailed in Table 2.
[0053] The heavy metal curing agent is polysilicon iron zinc and kaolin, and the mass ratio of polysilicon iron zinc to kaolin is 2:3; the dispersant is a mixture of sulfonated sodium humate and sodium polycarboxylate, and the mass ratio of sulfonated sodium humate and sodium polycarboxylate is 1:0.625; the stabilizer is high-viscosity carboxymethyl cellulose.
[0054] Table 2
[0055] Components Powdered coal gangue powder Fine coal gangue powder Hazardous substance curing agent Dispersants Stabilizer Shimizu Dosage / kg 250 550 25 6.5 3.5 750
[0056] The process for preparing high-solid-phase strongly stable coal gangue powder solid waste slurry in the mine goaf separation zone filling project is the same as that in Example 1.
[0057] The high solid phase and strong stable coal gangue powder solid waste slurry prepared in Example 2 was used for the filling project of the goaf separation zone. The test showed that the slurry funnel viscosity was 52s and the 24h water separation rate was 1.2%. The slurry pumping distance exceeded 4000m, the continuous grouting time was 50h, and there was no pipe blocking accident caused by coal gangue powder precipitation in the slurry pipeline; the slurry diffusion distance exceeded 50m, and the single injection volume exceeded 1500m 3 The 28d compressive strength of the slurry consolidation body was 3.3MPa by retaining the sample in the test mold.
[0058] Example 3: Slurry preparation process of high solid phase strong stable coal gangue powder solid waste slurry in abandoned tunnel filling project of a coal mine goaf in the west
[0059] The high-solid phase strongly stable coal gangue powder solid waste slurry used in this embodiment is composed of 200kg of powdered coal gangue powder, 600kg of fine coal gangue powder, 25kg of heavy metal curing agent, 5.5kg of dispersant, 3.0kg of stabilizer and 750kg of clean water. The components are detailed in Table 3.
[0060] The heavy metal curing agent is polysilicon zinc iron and kaolin, and the mass ratio of polysilicon zinc iron and kaolin is 2:3; the dispersant is sodium sulfonated humate; the stabilizer is polyacrylamide and high-viscosity carboxymethyl cellulose, and the mass ratio of polyacrylamide and high-viscosity carboxymethyl cellulose is 0.5:1.
[0061] Table 3
[0062] Components Powdered coal gangue powder Fine coal gangue powder Hazardous substance curing agent Dispersants Stabilizer Shimizu Dosage / kg 200 600 25 5.5 3.0 750
[0063] The process for preparing high-solid phase strongly stable coal gangue powder solid waste slurry for the abandoned tunnel filling project in the coal mine goaf area is the same as that in Example 1.
[0064] The high solid phase strong stable coal gangue powder solid waste slurry prepared in Example 3 was used for the filling project of the waste tunnel in the goaf area. The test showed that the slurry funnel viscosity was 48s and the 24h water separation rate was 1.5% (the water separation rate is used to evaluate the fluidity and stability of the material). The slurry pumping distance exceeded 4500m, the continuous grouting time was 50h, and there was no pipe blocking accident caused by coal gangue powder precipitation in the slurry pipeline; the slurry diffusion distance exceeded 60m, and the single injection volume exceeded 1500m 3 The slurry consolidation body was tested and the 28d compressive strength was 2.5MPa.
[0065] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the claims of this patent application.
Claims
1. A high solid phase and strong stable goaf solid waste filling slurry, characterized in that: The solid waste filling slurry is composed of the following components: powdered coal gangue powder, fine-grained coal gangue powder, a harmful substance curing agent, a dispersant, a stabilizer and water; the weight proportions of the components in the solid waste filling slurry are: 200 to 500 weight proportions of powdered coal gangue powder, 300 to 600 weight proportions of fine-grained coal gangue powder, 5 to 30 weight proportions of harmful substance curing agent, 3 to 15 weight proportions of dispersant, 0.75 to 20 weight proportions of stabilizer and 600 to 800 weight proportions of water.
2. The high-solid phase and highly stable solid waste filling slurry for goaf area according to claim 1, characterized in that: The preparation method of the powdered coal gangue powder is as follows: the coal gangue is crushed into stone particles, and then the powder is ground by a grinding device and then sieved to obtain the powder; the particle size of the coal gangue after the coal gangue is crushed is not more than 30 mm, and the grinding device adopts a vertical roller mill, and the particle size is controlled to be 10-50 μm; The preparation method of fine-grained coal gangue powder is as follows: the coal gangue is crushed into stone particles, and then the powder is ground by a grinding device and then sieved to obtain the powder; the particle size of the crushed coal gangue is not greater than 30 mm, the grinding device adopts a Raymond mill, and the particle size is controlled to be 50-100 μm.
3. The high-solid phase and highly stable solid waste filling slurry for goaf area according to claim 1 is characterized in that: The harmful substance curing agent is one or a mixture of two or more of kaolin powder, polysilicon iron zinc and diatomaceous earth; the mass ratio of kaolin powder, diatomaceous earth and polysilicon iron zinc is 0-5:0-1:3-4.
4. The high-solid phase and highly stable solid waste filling slurry for goaf area according to claim 1, characterized in that: The dispersant is one or both of sulfonated sodium humate and sodium polycarboxylate, and the mass ratio of sulfonated sodium humate to sodium polycarboxylate is 1:0.5-1.
5. The high-solid phase and highly stable solid waste filling slurry for goaf according to claim 1 is characterized in that: The stabilizer is one or a mixture of two or more of polyacrylamide, sodium tripolyphosphate and high-viscosity carboxymethyl cellulose, and the mass ratio of polyacrylamide, sodium tripolyphosphate and high-viscosity carboxymethyl cellulose is 0-0.6:0-0.1:1-10.
6. A system for preparing high-solid phase and highly stable goaf solid waste filling slurry according to any one of claims 1 to 5, characterized in that: The invention comprises a gangue crushing system, a gangue powder grinding and screening system, and a gangue powder storage system installed in the gangue continuous crushing and screening workshop; a material weighing and metering system, a high-solid-phase gangue powder-based slurry preparation system, and a high-solid-phase highly stable solid waste slurry preparation system installed in the digital pulping workshop; the gangue crushing system is a gangue crusher (1); the gangue powder storage system includes a vertical roller mill (2) and a Raymond mill (3); the gangue powder storage The loading system includes a fine-grained gangue powder storage tank (5) and a powdered gangue powder storage tank (4); the material weighing and metering system includes a screw feeder (6) and a metering and weighing device (8); the high-solid-phase gangue powder-based slurry preparation system includes a clear water tank (12), a primary stirring tank (10) and an ultrasonic dispersing mixer (11); the high-solid-phase strongly stable solid waste slurry preparation system includes a secondary stirring tank (14) and a high-speed vortex mixer (15); The gangue crusher (1) crushes the gangue to obtain crushed stone particles, which are respectively sent to the vertical roller mill (2) and the Raymond mill (3) for grinding and screening to obtain powdered gangue powder and fine-grained gangue powder. The powdered gangue powder and fine-grained gangue powder are respectively transferred to the powdered gangue powder storage tank (4) and the fine-grained gangue powder storage tank (5) for storage; the powdered gangue powder in the powdered gangue powder storage tank (4) and the fine-grained gangue powder in the fine-grained gangue powder storage tank (5) are respectively sent to the The measuring and weighing device (8) is used for weighing, and a harmful substance solidifying agent (7) is added at the same time to obtain a mixture; after weighing, the mixture is sent to a primary stirring tank (10), clean water is pumped into the clean water tank (12), a dispersant is added, and then the mixture is stirred by an ultrasonic dispersing stirrer (11) to obtain a high-solid phase coal gangue powder-based slurry; the high-solid phase coal gangue powder-based slurry is transferred to a secondary stirring tank (14), a stabilizer is added, and then the mixture is stirred by a high-speed vortex stirrer (15) to obtain a high-solid phase strongly stable solid waste filling slurry.
7. The method for preparing a high-solid phase and highly stable goaf solid waste filling slurry according to any one of claims 1 to 5, characterized in that: The high-solid phase and highly stable goaf solid waste filling slurry according to any one of claims 1 to 5 is prepared by using the preparation system according to claim 6, comprising the following steps: (A) Crushing, grinding, screening and storage of gangue raw materials: a continuous gangue crushing and screening workshop is established near a gangue mountain or gangue silo; the gangue raw materials are fed into a gangue crusher (1) for crushing, and the gangue is graded and crushed to obtain crushed stone particles with a particle size of 0 to 30 mm; the crushed stone particles are respectively fed into a vertical roller mill (2) and a Raymond mill (3) for grinding and screening to obtain powdered gangue powder and fine-grained gangue powder, and the powdered gangue powder and fine-grained gangue powder are respectively transferred to a powdered gangue powder storage tank (4) and a fine-grained gangue powder storage tank (5) for storage; (B) Conveying, metering and mixing pretreatment of powdered gangue powder and fine-grained gangue powder: the powdered gangue powder in the powdered gangue powder storage tank (4) and the fine-grained gangue powder in the fine-grained gangue powder storage tank (5) are respectively fed to the metering weighing device (8) through a screw feeder (6) for weighing, and the harmful substance curing agent (7) is added to the metering weighing device (8) for weighing; then, the pretreatment is carried out by using an ultrasonic mixer to mix them uniformly to obtain a mixture; (C) primary stirring to prepare high solid phase coal gangue powder based slurry: the mixture is sent from the ultrasonic mixer to the primary stirring tank (10), then pumped into the water in the clean water tank (12), a dispersant is added, and the mixture is stirred and slurried by an ultrasonic dispersing mixer (11) to obtain a high solid phase coal gangue powder based slurry; (D) Secondary stirring to prepare high-solid phase highly stable solid waste filling slurry: The high-solid phase coal gangue powder-based slurry is transferred to the secondary stirring tank (14), and after adding a stabilizer, a high-speed vortex mixer (15) is used to stir and slurry to obtain a high-solid phase highly stable solid waste filling slurry.
8. The method for preparing a high-solid phase and highly stable goaf solid waste filling slurry according to claim 7, characterized in that: In step (A), the vertical roller mill (2) is used to grind the coal gangue powder to obtain a particle size range of 10 to 50 μm; and the Raymond mill (3) is used to grind the coal gangue powder to obtain a fine particle size range of 50 to 100 μm.
9. The method for preparing a high-solid phase and highly stable solid waste filling slurry for goaf areas according to claim 7, characterized in that: In step (B), the amount of powdered coal gangue powder added is 200-500 parts by weight, and the amount of fine-grained coal gangue powder added is 200-600 parts by weight; the amount of harmful substance curing agent added is 5-30 parts by weight; the harmful substance curing agent is one or a mixture of two or more of kaolin powder, polysilicon iron zinc, and diatomaceous earth; the mass ratio of kaolin powder, polysilicon iron zinc, and diatomaceous earth is 0:3:1-5:4:
0.
10. The method for preparing a high-solid phase and highly stable goaf solid waste filling slurry according to claim 7, characterized in that: In step (C), the amount of dispersant added is 3 to 15 parts by weight; the amount of water added is 600 to 800 parts by weight; the dispersant is one or both of sodium sulfonated humate and sodium polycarboxylate, and the mass ratio of sodium sulfonated humate to sodium polycarboxylate is 1:0.5 to 1:1; In step (D), the amount of stabilizer added is 0.75 to 20 parts by weight; the stabilizer is one or a mixture of two or more of polyacrylamide, sodium tripolyphosphate and high-viscosity carboxymethyl cellulose, and the mass ratio of polyacrylamide, sodium tripolyphosphate and high-viscosity carboxymethyl cellulose is 0:0:10 to 0.6:0.1:1.