Thin-body ceramic and firing process thereof
By adding specific minerals and ceramic reinforcement to the thin-body ceramic blast material, combined with grouting and glaze spraying technology, the problems of low strength and complex preparation of thin-body ceramics are solved, and the ultra-thin impact-resistant ceramics are efficiently prepared, reducing the efficiency of the preparation of ultra-thin impact-resistant ceramics. Cost increases the practical value of the product.
Patent Information
- Application Number
- CN202310641557.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-01
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-06-01
AI Technical Summary
The existing thin-tied ceramics have light and low strength, which can easily break, which affects practical value, and are complex in the preparation process and high cost, which leads to expensive products, which is not conducive to popularization.
Kaolin, mullite and manganese dolomite are used as base material, and silica, zirconium oxide and gallium oxide are added, and ceramic reinforcement agents of sodium tripolyphosphate, vinyl acetate and hydroxyethyl starch are prepared through grouting process. The porcelain blank is made of glaze spraying and a one-time firing process to improve the bending strength and impact resistance of the ceramic.
It realizes the preparation of thinner and transparent ceramic embryos, improves the impact resistance and hardness of ceramics, simplifies the firing process, reduces the preparation cost, and has good application prospects.
Smart Images

Figure CN119059796A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of thin-body ceramic production, and specifically discloses a thin-body ceramic and a firing process thereof. Background Art
[0002] Thin-bodied ceramics are also called "de-bodied porcelain" and "eggshell porcelain". It is one of the most prestigious special craft products among traditional porcelain varieties in Jingdezhen, Jiangxi, Dapu County, Guangdong and other places. The characteristics are that the porcelain body is as thin as an eggshell and translucent. Common products include vases, lampshades, tea sets, pen holders, etc., which are light, beautiful, thin and transparent, and are deeply loved by people. However, due to the thin porcelain body, thin-bodied porcelain has low product strength. When used in daily utensils such as complete sets of tea sets, it is easy to break, which greatly affects the practical value of thin-bodied porcelain. CN201911067481.7 discloses a drop-resistant prestressed reinforced thin-bodied ceramic and a preparation method thereof, which consists of a thin-bodied ceramic body and a coating applied to the surface of the body; the coating is composed of a bottom coating and a face coating superimposed to form a gradient coating with a decreasing thermal expansion coefficient and an increasing elastic modulus from the bottom of the body to the surface. By introducing double-layer compressive stress on the surface of the thin-walled ceramic body, the tensile stress generated by the ceramic body breaking when subjected to external loads is offset, thereby significantly improving the strength of the thin-walled ceramics, preventing them from being impacted, achieving a drop-resistant effect, and enhancing the service life of the thin-walled ceramics, and effectively improving the safety of actual use. However, the above invention requires two coatings, the cost of the coating components is high, agate crystals need to be added, and the preparation process is complicated, resulting in the high price of the produced thin-walled ceramics, which is not conducive to the popularization of thin-walled ceramic products. Summary of the invention
[0003] In order to solve the above problems, the present invention discloses a thin-body ceramic and a firing process thereof.
[0004] The present invention includes the following technical solutions:
[0005] A thin-body ceramic is made of the following raw materials in parts by weight:
[0006] a.Blank material:
[0007]
[0008] b. Glaze:
[0009]
[0010]
[0011] Preferably, the above-mentioned thin-body ceramic is made of the following raw materials in parts by weight:
[0012] a.Blank material:
[0013]
[0014] b. Glaze:
[0015]
[0016] Furthermore, the firing process of the above-mentioned thin-walled ceramic comprises the following steps:
[0017] 1) forming the green material into a ceramic green body;
[0018] 2) applying the glaze on the ceramic body,
[0019] 3) Firing to obtain the thin-body ceramic.
[0020] Furthermore, in the above-mentioned firing process of a thin-walled ceramic, the step 1) comprises the following steps:
[0021] Step a: the raw materials in the blank are mixed according to the formula, crushed, ball-milled, and 0.5-0.7 times the mass of deionized water is added to make mud, and a ceramic reinforcing agent is added to the mud;
[0022] Step b: preparing a ceramic body by using the slurry prepared in step a and a slip injection process, wherein the thickness of the ceramic body is 0.6-0.9 mm. Before slip injection of the body, a layer of talcum powder is applied in the mold cavity used for slip injection. After slip injection of the body, cold air is continuously injected into the slip injection port to rapidly cool the body until the body is formed and a gap of 0.1-0.2 mm is formed with the inner cavity of the mold. The wind speed when injecting cold air is 3-4 m / S, and the air injection port is aligned with the position where the body and the mold cavity are combined.
[0023] Step c, trimming, placing the ceramic body on a trimming machine for trimming, and trimming the body to a surface thickness of 0.4-0.6 mm.
[0024] Furthermore, in the above-mentioned firing process of thin-body ceramics, the ceramic reinforcing agent is a mixture of sodium tripolyphosphate, vinyl acetate and hydroxyethyl starch.
[0025] Preferably, in the firing process of the above-mentioned thin-body ceramic, calculated by weight, the components include 15-20 parts of sodium tripolyphosphate, 5-10 parts of vinyl acetate, and 3-6 parts of hydroxyethyl starch.
[0026] Furthermore, in the above-mentioned firing process of a thin-walled ceramic, the step 2) comprises the following steps:
[0027] I. After mixing the glaze slurry according to the formula, crush it, ball mill it, and pass it through a standard sieve of 800 meshes, and the residue on the sieve is controlled at 0.1-0.2%; add deionized water to make the moisture content of the glaze slurry between 35-41%, and remove iron three times with an iron remover with a magnetic field strength of 10,000 gauss; the glaze is aged for 3-6 days;
[0028] II. Applying the glaze on the ceramic body by spraying glaze, the thickness of the glaze layer is 0.05-0.1mm.
[0029] Furthermore, in the firing process of the above-mentioned thin-bodied ceramic, the step 3) includes the following steps: placing the ceramic body after applying the glaze into a kiln for firing and forming, the firing temperature is 1950-2050°C, the firing time is 6-12h, and after one firing, a thin-bodied ceramic with an overall thickness of 0.25-0.35mm is obtained.
[0030] Furthermore, the firing process of the above-mentioned thin-walled ceramic comprises the following steps:
[0031] 1) Forming the green material into a ceramic green body:
[0032] Step a: the raw materials in the blank are mixed according to the formula, crushed, ball-milled, and 0.5-0.7 times the mass of deionized water is added to make mud, and a ceramic reinforcing agent is added to the mud;
[0033] Step b: preparing a ceramic body by using the slurry prepared in step a and a slip injection process, wherein the thickness of the ceramic body is 0.5-0.7 mm. Before slip injection of the body, a layer of talcum powder is applied in the mold cavity used for slip injection. After slip injection of the body, cold air is continuously injected into the slip injection port to rapidly cool the body until the body is formed and a gap of 0.1-0.2 mm is formed with the inner cavity of the mold. The wind speed when injecting cold air is 3-4 m / S, and the air injection port is aligned with the position where the body and the mold cavity are combined.
[0034] Step c, trimming, placing the ceramic body on a trimming machine for trimming, and trimming the body to a surface thickness of 0.3-0.5 mm;
[0035] 2) applying the glaze on the ceramic body:
[0036] I. After mixing the glaze slurry according to the formula, crush it, ball mill it, and pass it through a standard sieve of 800 meshes, and the residue on the sieve is controlled at 0.1-0.2%; add deionized water to make the moisture content of the glaze slurry between 35-41%, and remove iron three times with an iron remover with a magnetic field strength of 10,000 gauss; the glaze is aged for 3-6 days;
[0037] II. Applying the glaze on the ceramic body, using a spray glaze process, the glaze thickness is 0.05-0.1mm;
[0038] 3) Firing to obtain the thin ceramic:
[0039] The ceramic body after applying the glaze is placed in a kiln for firing and forming, the firing temperature is 1950-2050°C, the firing time is 6-12h, and then the temperature is reduced to 650-700°C and kept for 4-6h to obtain a thin-body ceramic with an overall thickness of 0.25-0.35mm.
[0040] Compared with the prior art, the present invention has the following beneficial effects: the present invention uses kaolin, mullite and manganese dolomite as basic raw materials in the thin-bodied ceramic blank, so that the basic raw materials have good workability and molding performance, and a combination of silicon dioxide, zirconium dioxide and gallium oxide is added on the basis thereof to enhance its hardness and thermal stability, and a ceramic reinforcing agent composed of sodium tripolyphosphate, vinyl acetate and hydroxyethyl starch is added to greatly improve the bending strength and impact resistance of the ceramic product. Combining the above advantages, it is possible to prepare a thinner and more transparent ceramic blank, and with the high-hardness glaze disclosed in the present invention, ultra-thin and impact-resistant thin-bodied ceramics can be prepared, and the firing process of the present invention is simple, the firing is completed in one time, the preparation cost is low, and it has good application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 Transverse comparative performance test of thin-wall ceramics, impact strength (center position), J / m 2 ;
[0042] Figure 2 It is the lateral comparative performance test of thin-walled ceramics, bending strength (Mpa);
[0043] Figure 3 It is a lateral comparative performance test of thin-body ceramics and thermal stability (number of times they can last without cracking). DETAILED DESCRIPTION
[0044] A thin-body ceramic is made from the following raw materials in parts by weight:
[0045] a.Blank material:
[0046]
[0047] b. Glaze:
[0048]
[0049] The firing process of the above-mentioned thin-body ceramics consists of the following steps:
[0050] 1) Forming the green material into a ceramic green body:
[0051] Step a: the raw materials in the blank are mixed according to the formula, crushed, ball-milled, and 0.5-0.7 times the mass of deionized water is added to make mud, and a ceramic reinforcing agent is added to the mud;
[0052] Step b: preparing a ceramic body by using the slurry prepared in step a and a slip injection process, wherein the thickness of the ceramic body is 0.5-0.7 mm. Before slip injection of the body, a layer of talcum powder is applied in the mold cavity used for slip injection. After slip injection of the body, cold air is continuously injected into the slip injection port to rapidly cool the body until the body is formed and a gap of 0.1-0.2 mm is formed with the inner cavity of the mold. The wind speed when injecting cold air is 3-4 m / S, and the air injection port is aligned with the position where the body and the mold cavity are combined.
[0053] Step c, trimming, placing the ceramic body on a trimming machine for trimming, and trimming the body to a surface thickness of 0.3-0.5 mm;
[0054] 2) applying the glaze on the ceramic body:
[0055] I. After mixing the glaze slurry according to the formula, crush it, ball mill it, and pass it through a standard sieve of 800 meshes, and the residue on the sieve is controlled at 0.1-0.2%; add deionized water to make the moisture content of the glaze slurry between 35-41%, and remove iron three times with an iron remover with a magnetic field strength of 10,000 gauss; the glaze is aged for 3-6 days;
[0056] II. applying the glaze on the ceramic body by spraying glaze, with a glaze layer thickness of 0.05-0.1 mm;
[0057] 3) Firing to obtain the thin ceramic:
[0058] The ceramic body after applying the glaze is placed in a kiln for firing and forming, the firing temperature is 1950-2050°C, the firing time is 6-12h, and then the temperature is reduced to 650-700°C and kept for 4-6h to obtain a thin-body ceramic with an overall thickness of 0.25-0.35mm.
[0059] The ceramic reinforcing agent is a mixture of sodium tripolyphosphate, vinyl acetate and hydroxyethyl starch; calculated by weight, the sodium tripolyphosphate is 15-20 parts, the vinyl acetate is 5-10 parts, and the hydroxyethyl starch is 3-6 parts.
[0060] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0061] Kaolin was purchased from Jiangxi Tuoan New Materials Co., Ltd., calcined kaolin, 1250-8000 mesh, purity 99%.
[0062] Mullite was purchased from Henan Hongtai Kiln Refractory Material Co., Ltd., fused mullite.
[0063] Manganese dolomite was purchased from Haicheng Mileda Mineral Products Sales Co., Ltd.
[0064] Example 1
[0065] A thin-body ceramic is made from the following raw materials in parts by weight:
[0066] a.Blank material:
[0067]
[0068] b. Glaze:
[0069]
[0070] The firing process of the above-mentioned thin-body ceramics consists of the following steps:
[0071] 1) Forming the green material into a ceramic green body:
[0072] Step a: the raw materials in the blank are mixed according to the formula, crushed, ball-milled, and 0.5-0.7 times the mass of deionized water is added to make mud, and a ceramic reinforcing agent is added to the mud;
[0073] Step b: preparing a ceramic body by using the slurry prepared in step a and a slip injection process, wherein the thickness of the ceramic body is 0.5-0.7 mm. Before slip injection of the body, a layer of talcum powder is applied in the mold cavity used for slip injection. After slip injection of the body, cold air is continuously injected into the slip injection port to rapidly cool the body until the body is formed and a gap of 0.1-0.2 mm is formed with the inner cavity of the mold. The wind speed when injecting cold air is 3-4 m / S, and the air injection port is aligned with the position where the body and the mold cavity are combined.
[0074] Step c, trimming, placing the ceramic body on a trimming machine for trimming, and trimming the body to a surface thickness of 0.3-0.5 mm;
[0075] 2) applying the glaze on the ceramic body:
[0076] I. After mixing the glaze slurry according to the formula, crush it, ball mill it, and pass it through a standard sieve of 800 meshes, and the residue on the sieve is controlled at 0.1-0.2%; add deionized water to make the moisture content of the glaze slurry between 35-41%, and remove iron three times with an iron remover with a magnetic field strength of 10,000 gauss; the glaze is aged for 3-6 days;
[0077] II. applying the glaze on the ceramic body by spraying glaze, with a glaze layer thickness of 0.05-0.1 mm;
[0078] 3) Firing to obtain the thin ceramic:
[0079] The ceramic body after applying the glaze is placed in a kiln for firing and forming, the firing temperature is 1950-2050°C, the firing time is 6-12h, and then the temperature is reduced to 650-700°C and kept for 4-6h to obtain a thin-body ceramic with an overall thickness of 0.25-0.35mm.
[0080] The ceramic reinforcing agent is a mixture of sodium tripolyphosphate, vinyl acetate and hydroxyethyl starch; calculated by weight, the mixture includes 15 parts of sodium tripolyphosphate, 5 parts of vinyl acetate and 3 parts of hydroxyethyl starch.
[0081] Example 2
[0082] A thin-body ceramic is made from the following raw materials in parts by weight:
[0083] a.Blank material:
[0084]
[0085] b. Glaze:
[0086]
[0087] The firing process of the above-mentioned thin-body ceramics consists of the following steps:
[0088] 1) Forming the green material into a ceramic green body:
[0089] Step a: the raw materials in the blank are mixed according to the formula, crushed, ball-milled, and 0.5-0.7 times the mass of deionized water is added to make mud, and a ceramic reinforcing agent is added to the mud;
[0090] Step b: preparing a ceramic body by using the slurry prepared in step a and a slip injection process, wherein the thickness of the ceramic body is 0.5-0.7 mm. Before slip injection of the body, a layer of talcum powder is applied in the mold cavity used for slip injection. After slip injection of the body, cold air is continuously injected into the slip injection port to rapidly cool the body until the body is formed and a gap of 0.1-0.2 mm is formed with the inner cavity of the mold. The wind speed when injecting cold air is 3-4 m / S, and the air injection port is aligned with the position where the body and the mold cavity are combined.
[0091] Step c, trimming, placing the ceramic body on a trimming machine for trimming, and trimming the body to a surface thickness of 0.3-0.5 mm;
[0092] 2) applying the glaze on the ceramic body:
[0093] I. After mixing the glaze slurry according to the formula, crush it, ball mill it, and pass it through a standard sieve of 800 meshes, and the residue on the sieve is controlled at 0.1-0.2%; add deionized water to make the moisture content of the glaze slurry between 35-41%, and remove iron three times with an iron remover with a magnetic field strength of 10,000 gauss; the glaze is aged for 3-6 days;
[0094] II. applying the glaze on the ceramic body by spraying glaze, with a glaze layer thickness of 0.05-0.1 mm;
[0095] 3) Firing to obtain the thin ceramic:
[0096] The ceramic body after applying the glaze is placed in a kiln for firing and forming, the firing temperature is 1950-2050°C, the firing time is 6-12h, and then the temperature is reduced to 650-700°C and kept for 4-6h to obtain a thin-body ceramic with an overall thickness of 0.25-0.35mm.
[0097] The ceramic reinforcing agent is a mixture of sodium tripolyphosphate, vinyl acetate and hydroxyethyl starch; calculated by weight, the mixture includes 18 parts of sodium tripolyphosphate, 8 parts of vinyl acetate and 4.5 parts of hydroxyethyl starch.
[0098] Example 3
[0099] A thin-body ceramic is made from the following raw materials in parts by weight:
[0100] a.Blank material:
[0101]
[0102] b. Glaze:
[0103]
[0104]
[0105] The firing process of the above-mentioned thin-body ceramics consists of the following steps:
[0106] 1) Forming the green material into a ceramic green body:
[0107] Step a: the raw materials in the blank are mixed according to the formula, crushed, ball-milled, and 0.5-0.7 times the mass of deionized water is added to make mud, and a ceramic reinforcing agent is added to the mud;
[0108] Step b: preparing a ceramic body by using the slurry prepared in step a and a slip injection process, wherein the thickness of the ceramic body is 0.5-0.7 mm. Before slip injection of the body, a layer of talcum powder is applied in the mold cavity used for slip injection. After slip injection of the body, cold air is continuously injected into the slip injection port to rapidly cool the body until the body is formed and a gap of 0.1-0.2 mm is formed with the inner cavity of the mold. The wind speed when injecting cold air is 3-4 m / S, and the air injection port is aligned with the position where the body and the mold cavity are combined.
[0109] Step c, trimming, placing the ceramic body on a trimming machine for trimming, and trimming the body to a surface thickness of 0.3-0.5 mm;
[0110] 2) applying the glaze on the ceramic body:
[0111] I. After mixing the glaze slurry according to the formula, crush it, ball mill it, and pass it through a standard sieve of 800 meshes, and the residue on the sieve is controlled at 0.1-0.2%; add deionized water to make the moisture content of the glaze slurry between 35-41%, and remove iron three times with an iron remover with a magnetic field strength of 10,000 gauss; the glaze is aged for 3-6 days;
[0112] II. applying the glaze on the ceramic body by spraying glaze, with a glaze layer thickness of 0.05-0.1 mm;
[0113] 3) Firing to obtain the thin ceramic:
[0114] The ceramic body after applying the glaze is placed in a kiln for firing and forming, the firing temperature is 1950-2050°C, the firing time is 6-12h, and then the temperature is reduced to 650-700°C and kept for 4-6h to obtain a thin-body ceramic with an overall thickness of 0.25-0.35mm.
[0115] The ceramic reinforcing agent is a mixture of sodium tripolyphosphate, vinyl acetate and hydroxyethyl starch; calculated by weight, the mixture includes 20 parts of sodium tripolyphosphate, 10 parts of vinyl acetate and 6 parts of hydroxyethyl starch.
[0116] Comparative Example 1
[0117] No ceramic reinforcing agent is contained, and the rest is the same as in Example 2.
[0118] Comparative Example 2
[0119] The ceramic reinforcing agent only includes 18 parts of sodium tripolyphosphate and 8 parts of vinyl acetate, and does not include hydroxyethyl starch. Others are the same as in Example 2.
[0120] Comparative Example 3
[0121] Mullite is replaced by kaolin, and the rest is the same as in Example 2.
[0122] Comparative Example 4
[0123] Mullite and manganese dolomite are both replaced by kaolin, and the rest is the same as in Example 2.
[0124] Comparative Example 5
[0125] It does not contain zirconium dioxide and gallium oxide, and the rest is the same as in Example 2.
[0126] Comparative Example 6
[0127] Ordinary thin-walled ceramics were purchased commercially.
[0128] Test Example 1
[0129] The thin ceramic materials obtained in Examples 1-3 and Comparative Examples 1-6 were tested, wherein the bending strength was tested by a three-point method, the thermal stability test method was as follows: the ceramic profile was heated to 1500°C, then air-cooled to room temperature, and checked for cracks or fractures, and the impact resistance test was conducted in accordance with GB / T38494-2020 (ceramic impact resistance test method). The results are shown in Table 1 and Appendix. Figure 1 , Attachment Figure 2 and attached Figure 3 shown.
[0130] Table 1. Transverse comparative performance test of thin-body ceramics.
[0131]
[0132] It can be seen from the above data that the present invention uses kaolin, mullite and manganese dolomite as basic raw materials in the thin-body ceramic blank, so that the basic raw materials have good workability and molding performance, and a combination of silicon dioxide, zirconium dioxide and gallium oxide is added to the basis to enhance its hardness and thermal stability, and a ceramic reinforcing agent composed of sodium tripolyphosphate, vinyl acetate and hydroxyethyl starch is added to greatly improve the bending strength and impact resistance of the ceramic products.
[0133] The above embodiments are limited to several preferred implementations of the present invention, and their descriptions are relatively specific and detailed, but they cannot be understood as limiting the scope of the present invention. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention.
Claims
1. A thin-body ceramic, characterized in that: Made from the following raw materials in parts by weight; a.Blank material: b. Glaze:
2. A thin-body ceramic according to claim 1, characterized in that: Made from the following raw materials in parts by weight: a.Blank material: b. Glaze:
3. A firing process for thin-walled ceramics as claimed in claim 1 or 2, characterized in that: The following steps are involved: 1) forming the green material into a ceramic green body; 2) applying the glaze on the ceramic body, 3) Firing to obtain the thin-body ceramic.
4. A firing process for thin-walled ceramics according to claim 3, characterized in that: The step 1) comprises the following steps: Step a: the raw materials in the blank are mixed according to the formula, crushed, ball-milled, and 0.5-0.7 times the mass of deionized water is added to make mud, and a ceramic reinforcing agent is added to the mud; Step b: preparing a ceramic body by using the slurry prepared in step a and a slip injection process, wherein the thickness of the ceramic body is 0.6-0.9 mm. Before slip injection of the body, a layer of talcum powder is applied in the mold cavity used for slip injection. After slip injection of the body, cold air is continuously injected into the slip injection port to rapidly cool the body until the body is formed and a gap of 0.1-0.2 mm is formed with the inner cavity of the mold. The wind speed when injecting cold air is 3-4 m / S, and the air injection port is aligned with the position where the body and the mold cavity are combined. Step c, trimming, placing the ceramic body on a trimming machine for trimming, and trimming the body to a surface thickness of 0.4-0.6 mm.
5. The firing process of a thin-walled ceramic according to claim 4, characterized in that: The ceramic reinforcing agent is a mixture of sodium tripolyphosphate, vinyl acetate and hydroxyethyl starch.
6. The firing process of a thin-walled ceramic according to claim 5, characterized in that: Calculated by mass, sodium tripolyphosphate 15-20 parts, vinyl acetate 5-10 parts, hydroxyethyl starch 3-6 parts.
7. The firing process of a thin-walled ceramic according to claim 3, characterized in that: The step 2) comprises the following steps: I. After mixing the glaze slurry according to the formula, crush it, ball mill it, and pass it through a standard sieve of 800 meshes, and the residue on the sieve is controlled at 0.1-0.2%; add deionized water to make the moisture content of the glaze slurry between 35-41%, and remove iron three times with an iron remover with a magnetic field strength of 10,000 gauss; the glaze is aged for 3-6 days; II. Applying the glaze on the ceramic body by spraying glaze, the thickness of the glaze layer is 0.05-0.1mm.
8. The firing process of a thin-walled ceramic according to claim 3, characterized in that: The step 3) comprises the following steps: placing the ceramic body after applying the glaze into a kiln for firing, the firing temperature is 1950-2050°C, the firing time is 6-12h, and after one firing, a thin-body ceramic with an overall thickness of 0.25-0.35mm is obtained.
9. The firing process of a thin-walled ceramic according to claim 3, characterized in that: It consists of the following steps: 1) Forming the green material into a ceramic green body: Step a: the raw materials in the blank are mixed according to the formula, crushed, ball-milled, and 0.5-0.7 times the mass of deionized water is added to make mud, and a ceramic reinforcing agent is added to the mud; Step b: preparing a ceramic body by using the slurry prepared in step a and a slip injection process, wherein the thickness of the ceramic body is 0.5-0.7 mm. Before slip injection of the body, a layer of talcum powder is applied in the mold cavity used for slip injection. After slip injection of the body, cold air is continuously injected into the slip injection port to rapidly cool the body until the body is formed and a gap of 0.1-0.2 mm is formed with the inner cavity of the mold. The wind speed when injecting cold air is 3-4 m / S, and the air injection port is aligned with the position where the body and the mold cavity are combined. Step c, trimming, placing the ceramic body on a trimming machine for trimming, and trimming the body to a surface thickness of 0.3-0.5 mm; 2) applying the glaze on the ceramic body: I. After mixing the glaze slurry according to the formula, crush it, ball mill it, and pass it through a standard sieve of 800 meshes, and the residue on the sieve is controlled at 0.1-0.2%; add deionized water to make the moisture content of the glaze slurry between 35-41%, and remove iron three times with an iron remover with a magnetic field strength of 10,000 gauss; the glaze is aged for 3-6 days; II. Applying the glaze on the ceramic body, using a spray glaze process, the glaze thickness is 0.05-0.1mm; 3) Firing to obtain the thin ceramic: The ceramic body after applying the glaze is placed in a kiln for firing and forming, the firing temperature is 1950-2050°C, the firing time is 6-12h, and then the temperature is reduced to 650-700°C and kept for 4-6h to obtain a thin-body ceramic with an overall thickness of 0.25-0.35mm.
Citation Information
Patent Citations
Thin and transparent white jade ceramic material
CN101265078A
Ceramic wine bottle colored glaze and glaze spraying method
CN103922806A
High-transmittance eggshell white ceramic product and making method thereof
CN109503126A
Once-firing unglazed ultra-thin porcelain and manufacturing technology thereof
CN109942281A
composition for the production of ceramics
FR82175E