High-toughness rare earth tantalate ceramic material and preparation method thereof

By doping metal cations in rare earth tantalate ceramics and using hydrothermal method and discharge plasma sintering technology, the problem of insufficient material hardness and fracture toughness is solved, and ceramic materials with high toughness and high hardness are prepared, suitable for high-temperature environments thermal barrier coating application.

CN119059812APending Publication Date: 2024-12-03KUNMING UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411176833.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The hardness and fracture toughness of existing rare earth tantalate ceramic materials are not ideal, and it is difficult to meet the application needs in high temperature environments.

Method used

Doping metal cations such as Ti, Hf, Zr in RETa3O9 ceramics, the hydrothermal method and discharge plasma sintering process are used to improve the toughness and hardness of the material through solid solution strengthening and fine crystal strengthening mechanisms.

Benefits of technology

The prepared rare earth tantalate ceramic materials have high fracture toughness, low thermal conductivity and high hardness. They are suitable as high-temperature thermal barrier coating materials, extending the service life of engine components and improving engine performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119059812A_ABST
    Figure CN119059812A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of rare earth materials, and discloses a high-toughness rare earth tantalate ceramic material and a preparation method thereof, the chemical formula of the rare earth tantalate material is (MO2) x-(RETa3O9) 1-x, wherein M is a mixture of at least two metal cations of Ti, Zr and Hf, and has an equal molar ratio; rE is Y or Gd; 0 < X < 0.15; the ceramic material is prepared from TaCl5 powder, Y2O3 powder, Gd2O3 powder, TiCl4 powder, ZrCl4 powder and HfO2 powder through spark plasma sintering after a hydrothermal method is carried out on the TaCl5 powder, the Y2O3 powder, the Gd2O3 powder, the TiCl4 powder, the ZrCl4 powder and the HfO2 powder. According to the technical scheme, the material formula composition and the preparation process are integrally optimized, so that the prepared rare earth tantalate material is fine in grain and has the performance advantages of high fracture toughness and high hardness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of rare earth materials, and in particular to a high-toughness rare earth tantalate ceramic material and a preparation method thereof. Background Art

[0002] Technology is also constantly breaking new boundaries. In order to meet the needs of higher thrust-to-weight ratios and higher inlet temperatures, engine performance is constantly improving. It is reported that the intake temperature of the most advanced aircraft engines has reached an astonishing 1700°C or above. However, the limit application temperature of existing nickel-based alloy materials is only 1200°C, which is far from meeting such a high-temperature working environment. Therefore, finding a material that can withstand higher temperatures has become one of the important topics in the development of aircraft engine technology. In this context, thermal barrier coatings (TBCs) have received widespread attention due to their good thermal insulation, oxidation corrosion resistance, mechanical and chemical stability in complex engine environments. TBCs can effectively protect engine components at high temperatures, extend their service life, and improve the overall performance of the engine.

[0003] Yttria-stabilized zirconia (YSZ) has long been widely used as a thermal barrier coating material. However, recent studies have shown that rare earth tantalates RETa 3 O 9 Ceramics have shown unique advantages in crystal structure and magnetic properties. In particular, RETa 3 O 9 Distorted TaO in the ceramic lattice 6 The octahedral and up to 66.7% A-site cation vacancies, as well as its complex crystal structure, make RETa 3 O 9 Ceramic has lower thermal conductivity than the existing thermal barrier coating material YSZ, which means it can better insulate heat and provide better protection for engine components. 3 O 9 The low hardness and fracture toughness of ceramics limit their application in thermal barrier coatings. Therefore, the development of a new high-hardness, high-fracture-toughness ceramic material is of great significance to promote the advancement of aero-engine technology. Summary of the invention

[0004] The present invention aims to provide a high-toughness rare earth tantalate ceramic material and a preparation method thereof, so as to solve the problem of unsatisfactory hardness and fracture toughness of rare earth tantalate ceramic materials in the prior art.

[0005] To achieve the above object, the present invention adopts the following technical solution: a rare earth tantalate ceramic material with high toughness, the chemical formula of the rare earth tantalate material is (MO2 ) x -(RETa 3 O 9 ) 1-x ; Wherein, M is a mixture of at least two metal cations of Ti, Zr, Hf; RE is Y or Gd; 0<X<0.15; The ceramic material is TaCl 5 Powder, Y 2 O 3 Powder, Gd 2 O 3 Powder, TiCl 4 Powder, ZrCl 4 Powder and HfO 2 The powder is prepared by a hydrothermal method followed by spark plasma sintering.

[0006] Preferably, as a modification, the metal cations are mixed in an equimolar ratio.

[0007] Preferably, as an improvement, M is a mixture of three metal cations of Ti, Zr and Hf in an equimolar ratio; RE is Y.

[0008] Preferably, as an improvement, TaCl 5 Powder, Y 2 O 3 Powder, Gd 2 O 3 Powder, TiCl 4 Powder, ZrCl 4 Powder and HfO 2 The purity of the powder is ≥99.9%.

[0009] Preferably, as an improvement, a method for preparing a high-toughness rare earth tantalate ceramic material comprises the following steps:

[0010] Step (1): Weigh TaCl 5 Powder, Y 2 O 3 Powder, Gd 2 O 3 Powder, TiCl 4 Powder, ZrCl 4 Powder and HfO 2 Powder, add solvent respectively for the first stirring to obtain a uniform solution A;

[0011] Step (2): mixing the solution A obtained in step (1) and stirring for a second time, while adding ammonia water (NH3·H2O) to adjust the pH value, to obtain solution B;

[0012] Step (3): placing the solution B obtained in step (2) in a reaction vessel and performing a hydrothermal reaction to obtain a solution C;

[0013] Step (4): washing and drying the solution C in step (3) to obtain powder D;

[0014] Step (5): Place the powder D in step (4) in a mold and sinter it using spark plasma to form a block E.

[0015] Preferably, as an improvement, in step (1), the solvent is deionized water; the rotation speed of the first stirring is 100 to 300 r / min, and the stirring time is 2 to 4 h.

[0016] Preferably, as an improvement, in step (2), the rotation speed of the second stirring is 400-800 r / min, the stirring time is 3-5 h; and the pH value is 9-11.

[0017] Preferably, as an improvement, in step (3), the temperature of the hydrothermal reaction is 200-250° C., and the reaction time is 36-48 h.

[0018] Preferably, as an improvement, in step (4), the solvent used for washing is ethanol or deionized water; the drying temperature is 60 to 80° C., and the drying time is 24 to 48 hours.

[0019] Preferably, as an improvement, in step (5), the sintering temperature is 1530-1680° C., the sintering time is 10-20 min, and the pressure is 70-100 MPa.

[0020] The principle and advantages of this solution are: in practical application, in this technical solution, in view of the unsatisfactory hardness and fracture toughness of rare earth tantalum ceramic materials in the prior art, a new method is proposed to improve the hardness of rare earth tantalum ceramic materials in RETa. 3 O 9 Ti, Hf, and Zr are co-doped in ceramics, with at least two metal cations in the ceramics, to improve toughness by solid solution strengthening mechanism; 2 ) x -(RETa 3 O 9 ) 1-x Ceramics, using spark plasma sintering to reduce grain size, improve fracture toughness and hardness through fine grain strengthening mechanism. The range of X can avoid the formation of second phases at the grain boundaries, thereby avoiding embrittlement of rare earth tantalate ceramics.

[0021] In the technical research and development stage, in terms of the material formula composition, this solution first adopted the co-doping of Ti, Hf, and Zr, using the solid solution strengthening mechanism to improve toughness, and using higher purity powders to reduce the content of introduced impurity elements, avoid impurity elements promoting grain growth at high temperatures, and avoid impurities from segregating at grain boundaries and affecting its fracture toughness. In terms of the optimization of the preparation process, this technical solution uses a hydrothermal method to prepare (MO 2 ) x -(RETa 3 O 9 ) 1-x Ceramics, using spark plasma sintering to reduce grain size, and improving fracture toughness and hardness through fine grain strengthening mechanism. By optimizing the hydrothermal reaction thermometer time, it can promote dissolution and diffusion of reactants, increase the reaction rate, and help the full growth and crystallization of crystals to obtain higher quality products. And by limiting the pH to optimize the hydrothermal reaction conditions, promote powder dissolution, improve the selectivity, yield and quality of the reaction. After the hydrothermal reaction is completed, the unreacted raw materials and impurities can be removed by solvent washing to improve the purity of the product; by optimizing the sintering conditions, the excessive growth of grains can be controlled, and the rare earth tantalate ceramics obtained have clear grain boundaries, good bonding and high density.

[0022] In summary, this technical solution optimizes the overall material formula composition and preparation process, so that the prepared rare earth tantalate material has fine grains and has the performance advantages of low thermal conductivity, high fracture toughness and high hardness. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 XRD diagrams of the rare earth tantalate materials prepared in Examples 1 to 4 of the present invention;

[0024] Figure 2 This is a SEM image of the rare earth tantalate material prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0025] The following is further described in detail through specific implementations, but the implementation of the present invention is not limited thereto. Unless otherwise specified, the technical means used in the following implementations are conventional means well known to those skilled in the art; the experimental methods used are all conventional methods; the materials, reagents, etc. used can all be obtained from commercial channels.

[0026] Program Overview:

[0027] A rare earth tantalate ceramic material with high toughness. The chemical formula of the rare earth tantalate material is (MO 2 ) x -(RETa 3 O 9 ) 1-x; Wherein, M is a mixture of at least two metal cations of Ti, Zr, and Hf (the metal cations are mixed in an equal molar ratio); RE is Y or Gd; 0<X<0.15; The ceramic material is TaCl 5 Powder, Y 2 O 3 Powder, Gd 2 O 3 Powder, TiCl 4 Powder, ZrCl 4 Powder and HfO 2 The powder is made by hydrothermal method and then spark plasma sintering; TaCl 5 Powder, Y 2 O 3 Powder, Gd 2 O 3 Powder, TiCl 4 Powder, ZrCl 4 Powder and HfO 2 The purity of the powder is ≥99.9%.

[0028] A method for preparing a high-toughness rare earth tantalate ceramic material comprises the following steps:

[0029] Step (1): Weigh TaCl according to the ratio 5 Powder, Y 2 O 3 Powder, Gd 2 O 3 Powder, TiCl 4 Powder, ZrCl 4 Powder and HfO 2 powder, and added solvents for the first stirring to obtain a uniform solution A; wherein TaCl 5 Powder, Y 2 O 3 Powder, Gd 2 O 3 Powder, TiCl 4 Powder, ZrCl 4 Powder and HfO 2 The purity of the powder is ≥99.9%, and the solvent is deionized water; the speed of the first stirring is 100-300 r / min, and the stirring time is 2-4 h;

[0030] Step (2): mixing the solution A obtained in step (1) and stirring for a second time, adding ammonia water (NH3·H2O) to adjust the pH value to 9-11, to obtain a solution B; the speed of the second stirring is 400-800 r / min, and the stirring time is 3-5 h;

[0031] Step (3): placing the solution B obtained in step (2) in a reaction kettle, and performing a hydrothermal reaction in an electric heated blast drying oven to obtain a solution C; the temperature of the hydrothermal reaction is 200 to 250° C., and the reaction time is 36 to 48 hours;

[0032] Step (4): washing and drying the solution C in step (3) to obtain powder D; the washing solvent is ethanol or deionized water; the drying temperature is 60 to 80° C., and the drying time is 24 to 48 hours;

[0033] Step (5): placing the powder D in step (4) in a mold and sintering it by spark plasma to form a block E; the sintering temperature is 1530-1680° C., the sintering time is 10-20 min, and the pressure is 70-100 MPa.

[0034] Example 1

[0035] A method for preparing a high-toughness rare earth tantalate ceramic material comprises the following steps:

[0036] Step (1): Weigh 0.02 mol of TiCl 4 Powder, ZrCl 4 Powder, HfO 2 Powder, 2.82molTaCl 5 Powder and 0.47 molY 2 O 3 Powder, deionized water was added according to the molar ratio of powder to solvent (1:5) and stirred at a speed of 100 r / min for 4 h to obtain a uniform solution;

[0037] Step (2): the solution obtained in step (1) was mixed and stirred at a speed of 400 r / min for 5 h, and ammonia water (NH3·H2O) was added to adjust the pH value to 9 to obtain a mixed uniform solution;

[0038] Step (3): placing the solution obtained in step (2) in a reaction kettle, and subjecting it to a hydrothermal reaction at 200° C. in an electric air drying oven for 42 hours to obtain a post-reaction solution;

[0039] Step (4): The reaction solution in step (3) was washed three times with ethanol and dried at 60° C. for 48 h to obtain a precursor powder.

[0040] Step (5): placing the powder in step (4) in a mold and sintering by spark plasma to obtain rare earth tantalate ceramics, wherein the sintering temperature is 1600° C., the sintering time is 15 min, and the pressure is 80 MPa.

[0041] Example 2

[0042] A method for preparing a high-toughness rare earth tantalate ceramic material comprises the following steps:

[0043] Step (1): Weigh 0.04 mol of TiCl 4 Powder, ZrCl 4 Powder, HfO 2 Powder, 2.64molTaCl 5 Powder and 0.44molY 2 O 3 Powder, deionized water was added according to the molar ratio of powder to solvent (1:7) and stirred at 200 r / min for 3 h to obtain a uniform solution;

[0044] Step (2): the solution obtained in step (1) was mixed and stirred at a speed of 700 r / min for 3.5 h, and ammonia water (NH3·H2O) was added to adjust the pH value to 11 to obtain a mixed uniform solution;

[0045] Step (3): placing the solution obtained in step (2) in a reaction kettle, and subjecting it to a hydrothermal reaction at 220° C. in an electric heated blast drying oven for 40 h to obtain a post-reaction solution;

[0046] Step (4): The reaction solution in step (3) was washed three times with ethanol and dried at 65° C. for 36 h to obtain a precursor powder.

[0047] Step (5): placing the powder in step (4) in a mold and sintering by spark plasma to obtain rare earth tantalate ceramics, wherein the sintering temperature is 1680° C., the sintering time is 10 min, and the pressure is 100 MPa.

[0048] Example 3

[0049] A method for preparing a high-toughness rare earth tantalate ceramic material comprises the following steps:

[0050] Step (1): Weigh 0.02 mol of TiCl 4 Powder, ZrCl 4 Powder, HfO 2 Powder, 2.82molTaCl 5 Powder and 0.47 molGd 2 O 3 Powder, deionized water was added according to the molar ratio of powder to solvent (1:7) and stirred at 200 r / min for 3 h to obtain a uniform solution;

[0051] Step (2): the solution obtained in step (1) was mixed and stirred at a speed of 700 r / min for 3.5 h, and ammonia water (NH3·H2O) was added to adjust the pH value to 11 to obtain a mixed uniform solution;

[0052] Step (3): placing the solution obtained in step (2) in a reaction kettle, and subjecting it to a hydrothermal reaction at 220° C. in an electric heated blast drying oven for 40 h to obtain a post-reaction solution;

[0053] Step (4): The reaction solution in step (3) was washed three times with ethanol and dried at 65° C. for 36 h to obtain a precursor powder.

[0054] Step (5): placing the powder in step (4) in a mold and sintering by spark plasma to obtain rare earth tantalate ceramics, wherein the sintering temperature is 1680° C., the sintering time is 10 min, and the pressure is 100 MPa.

[0055] Example 4

[0056] A method for preparing a high-toughness rare earth tantalate ceramic material comprises the following steps:

[0057] Step (1): Weigh 0.04 mol of TiCl 4 Powder, ZrCl 4 Powder, HfO 2 Powder, 2.64molTaCl 5 Powder and 0.44molGd 2 O 3 Powder, according to the molar ratio of powder to solvent (1:6), deionized water was added and stirred at a speed of 250 r / min for 3.5 h to obtain a uniform solution;

[0058] Step (2): the solution obtained in step (1) was mixed and stirred at a speed of 500 r / min for 3 h, and ammonia water (NH3·H2O) was added to adjust the pH value to 10 to obtain a mixed uniform solution;

[0059] Step (3): placing the solution obtained in step (2) in a reaction kettle, and subjecting it to a hydrothermal reaction at 240° C. in an electric heated blast drying oven for 45 hours to obtain a post-reaction solution;

[0060] Step (4): The reaction solution in step (3) was washed three times with ethanol and dried at 75° C. for 48 h to obtain a precursor powder.

[0061] Step (5): placing the powder in step (4) in a mold and sintering by spark plasma to obtain rare earth tantalate ceramics, wherein the sintering temperature is 1530° C., the sintering time is 20 min, and the pressure is 100 MPa.

[0062] Example 5

[0063] A method for preparing a high-toughness rare earth tantalate ceramic material comprises the following steps:

[0064] Step (1): Weigh 0.03 mol of TiCl 4 Powder and ZrCl 4 Powder, 2.82molTaCl 5 Powder and 0.47 molY 2 O 3 Powder, deionized water was added according to the molar ratio of powder to solvent (1:9) and stirred at a speed of 150 r / min for 4 h to obtain a uniform solution;

[0065] Step (2): the solution obtained in step (1) was mixed and stirred at a speed of 500 r / min for 4.5 h, and ammonia water (NH3·H2O) was added to adjust the pH value to 11 to obtain a mixed uniform solution;

[0066] Step (3): placing the solution obtained in step (2) in a reaction kettle, and subjecting it to a hydrothermal reaction at 240° C. in an electric heated blast drying oven for 38 hours to obtain a post-reaction solution;

[0067] Step (4): The reaction solution in step (3) was washed three times with ethanol and dried at 80° C. for 32 h to obtain a precursor powder.

[0068] Step (5): placing the powder in step (4) in a mold and sintering by spark plasma to obtain rare earth tantalate ceramics, wherein the sintering temperature is 1650° C., the sintering time is 15 min, and the pressure is 85 MPa.

[0069] Example 6

[0070] A method for preparing a high-toughness rare earth tantalate ceramic material comprises the following steps:

[0071] Step (1): Weigh 0.03 mol of TiCl 4 Powder and HfO 2 Powder, 2.82molTaCl 5 Powder and 0.47 molGd 2 O 3 Powder, deionized water was added according to the molar ratio of powder to solvent (1:10) and stirred at a speed of 250 r / min for 2 h to obtain a uniform solution;

[0072] Step (2): the solution obtained in step (1) was mixed and stirred at a speed of 750 r / min for 3 h, and ammonia water (NH3·H2O) was added to adjust the pH value to 9 to obtain a mixed uniform solution;

[0073] Step (3): placing the solution obtained in step (2) in a reaction kettle, and subjecting it to a hydrothermal reaction at 250° C. in an electric heated air drying oven for 38 hours to obtain a post-reaction solution;

[0074] Step (4): The reaction solution in step (3) was washed three times with ethanol and dried at 80° C. for 44 h to obtain a precursor powder.

[0075] Step (5): placing the powder in step (4) in a mold and sintering by spark plasma to obtain rare earth tantalate ceramics, wherein the sintering temperature is 1600° C., the sintering time is 15 min, and the pressure is 100 MPa.

[0076] Comparative Example 1

[0077] This comparative example uses a solid phase method to prepare rare earth tantalate ceramics, including the following steps:

[0078] Step (1): Weigh 0.02 mol of TiCl 4 Powder, ZrCl 4 Powder, HfO 2 Powder, 2.82molTaCl 5 Powder and 0.47 molY 2 O 3 Powder, add ethanol according to the molar ratio of powder to solvent (1:5), put into a ball mill and stir at a speed of 300 r / min for 24 h to obtain a uniform solution;

[0079] Step (2): drying the solution obtained in step (1) at 80° C. for 48 h to obtain a precursor powder;

[0080] Step (3): the precursor powder in step (2) is passed through a 300-mesh sieve, and then the pressure is maintained at 100 MPa for 3 minutes to obtain a block;

[0081] Step (4): Sinter the block in step (3) in a muffle furnace to obtain rare earth tantalate ceramics, wherein the sintering temperature is 1700° C. and the sintering time is 5 hours.

[0082] Comparative Example 2

[0083] The difference from Comparative Example 1 is that the raw material powder is 0.02 mol TiCl 4 Powder, ZrCl 4 Powder, HfO 2 Powder, 2.82molTaCl 5 Powder and 0.47 molGd 2 O 3 powder.

[0084] Comparative Example 3

[0085] The difference from Example 1 is that the raw material powder is 3 mol TaCl 5 Powder and 0.5 molY 2 O 3 powder.

[0086] Comparative Example 4

[0087] The difference from Example 1 is that the raw material powder is 3 mol TaCl 5 Powder and 0.5 molGd 2 O 3 powder.

[0088] Comparative Example 5

[0089] The difference between this comparative example and Example 1 is that in this comparative example, 0.01 mol TiO 2 、0.02molZrO 2 、0.03molHfO 2 .

[0090] Comparative Example 6

[0091] The difference between this comparative example and Example 1 is that: in this comparative example, 0.01 mol Ni 2 O 3 、0.02molCr 2 O 3 、0.03molAl 2 O 3

[0092] Experimental Example 1 XRD Characterization

[0093] The ceramic blocks obtained in Examples 1 to 6 and Comparative Examples 1 to 6 were tested using an X-ray diffractometer. Taking the rare earth tantalate material obtained in Examples 1 to 4 as an example, its XRD spectrum is as follows: Figure 1 As shown, the diffraction peaks of the XRD test results of Examples 1 to 4 correspond to the standard peaks of their standard PDF card #52-0566, and there is no second phase diffraction peak, indicating that the prepared sample is a single-phase rare earth tantalate material. This shows that Ti, Zr, and Hf ions are doped into YTa 3 O 9 or GdTa 3 O 9 The lattice leads to the lattice, and the corresponding solid solution is obtained.

[0094] Experimental Example 2 SEM Characterization

[0095] The ceramic blocks obtained in Examples 1 to 6 and Comparative Examples 1 to 6 were tested using a scanning electron microscope. Taking the rare earth tantalate material obtained in Example 1 as an example, its SEM spectrum is as follows: Figure 2 As shown, according to Figure 2It is observed that there are no pores in the crystal structure of rare earth tantalate materials, the grains are evenly distributed and the grain boundaries are clear, the grains are well bonded, and the grain size is 1 to 3 microns, which is smaller than the grain size obtained by the solid phase method. Rare earth tantalate materials prepared by hydrothermal method can reduce the grain size, refine the grains and strengthen them, thereby improving the fracture toughness.

[0096] Experimental Example 3 Hardness Test

[0097] The ceramic blocks obtained in Examples 1 to 6 and Comparative Examples 1 to 6 were polished and pressed with a load of 9.8 N using a micro Vickers hardness tester to obtain the hardness. Each sample was measured 10 times, the maximum and minimum values ​​were removed, and the average of the remaining values ​​was the final hardness value. The results are shown in Table 1: The hardness of Examples 1 to 6 is higher than that of Comparative Examples 1 to 6, indicating that the hardness of rare earth tantalate can be improved by using the method provided by the invention.

[0098] Table 1 Average hardness of Examples 1 to 6 and Comparative Examples 1 to 6 (n=3)

[0099]

[0100]

[0101] Experimental Example 4 Fracture toughness test

[0102] The ceramic blocks obtained in Examples 1 to 6 and Comparative Examples 1 to 4 were polished, and the fracture toughness of the tantalate ceramics was calculated using the indentation method. Taking the ceramic blocks obtained in Examples 1 to 6 and Comparative Examples 1 to 4 as examples, the specific method is as follows: the polished ceramic blocks are indented with a Vickers hardness tester at a certain load (F) to obtain the hardness (H), and each sample is performed 10 times; then the indentation diagonal length (a) and the crack length (c) of the crack extending along the diagonal are obtained in the scanning electron microscope image; using the formula,

[0103]

[0104] E is Young's modulus, and the fracture toughness is calculated (the average value of 10 times is taken for each sample). The calculation results are shown in Table 2. Compared with Comparative Examples 1 and 2, Examples 1 and 3 use the hydrothermal method to prepare fine grains, and the fracture toughness is improved by fine grain strengthening; Compared with Comparative Examples 3 and 4, Examples 1 to 6 use the same method to improve the fracture toughness through solid solution strengthening of Ti, Zr and Hf. Compared with Examples 5 and 6, Examples 1 to 4 illustrate that the fracture toughness of Ti, Zr and Hf co-doped is better than that of Ti, Zr and Hf doped with two of them. Compared with Comparative Examples 5 and 6, Examples 1 to 4 illustrate that the effect of doping Ti, Zr and Hf in the same proportion is better than that of doping in different proportions.

[0105] Table 1 Average fracture toughness of Examples 1 to 6 and Comparative Examples 1 to 6 (n=3)

[0106]

[0107]

[0108] The above is only an embodiment of the present invention, and the common knowledge such as the known specific technical solutions and / or characteristics in the solution is not described in detail here. It should be pointed out that for those skilled in the art, without departing from the technical solution of the present invention, several modifications and improvements can be made, which should also be regarded as the protection scope of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to interpret the content of the claims.

Claims

1. A high-toughness rare earth tantalate ceramic material, characterized by: The chemical formula of rare earth tantalate material is (MO2) x -(RETa3O9) 1-x ; Wherein, M is a mixture of at least two metal cations of Ti, Zr, and Hf; RE is Y or Gd; 0<X<0.15; the ceramic material is made of TaCl5 powder, Y2O3 powder, Gd2O3 powder, TiCl4 powder, ZrCl4 powder, and HfO2 powder by a hydrothermal method followed by spark plasma sintering.

2. The high-toughness rare earth tantalate ceramic material according to claim 1, characterized in that: The metal cations are mixed in an equimolar ratio.

3. The high-toughness rare earth tantalate ceramic material according to claim 2, characterized in that: M is a mixture of three metal cations of Ti, Zr and Hf in an equal molar ratio; RE is Y.

4. The high-toughness rare earth tantalate ceramic material according to claim 3, characterized in that: The purity of TaCl5 powder, Y2O3 powder, Gd2O3 powder, TiCl4 powder, ZrCl4 powder and HfO2 powder is ≥99.9%.

5. The method for preparing a high-toughness rare earth tantalate ceramic material according to any one of claims 1 to 4, characterized in that: The steps include: Step (1): weighing TaCl5 powder, Y2O3 powder, Gd2O3 powder, TiCl4 powder, ZrCl4 powder and HfO2 powder, adding solvent respectively and stirring for the first time to obtain a uniform solution A; Step (2): mixing the solution A obtained in step (1) and stirring for a second time, while adding ammonia water (NH3·H2O) to adjust the pH value to obtain solution B; Step (3): placing the solution B obtained in step (2) in a reactor and performing a hydrothermal reaction to obtain a solution C; Step (4): washing and drying the solution C in step (3) to obtain powder D; Step (5): Powder D in step (4) is placed in a mold and sintered using spark plasma to form a block E.

6. The method for preparing a high-toughness rare earth tantalate ceramic material according to claim 5, characterized in that: In step (1), the solvent is deionized water; the rotation speed of the first stirring is 100 to 300 r / min, and the stirring time is 2 to 4 hours.

7. The method for preparing a high-toughness rare earth tantalate ceramic material according to claim 6, characterized in that: In step (2), the second stirring speed is 400-800 r / min, the stirring time is 3-5 h, and the pH value is 9-11.

8. The method for preparing a high-toughness rare earth tantalate ceramic material according to claim 7, characterized in that: In step (3), the temperature of the hydrothermal reaction is 200-250° C., and the reaction time is 36-48 h.

9. The method for preparing a high-toughness rare earth tantalate ceramic material according to claim 8, characterized in that: In step (4), the solvent used for washing is ethanol or deionized water; the drying temperature is 60 to 80° C., and the drying time is 24 to 48 hours.

10. The method for preparing a high-toughness rare earth tantalate ceramic material according to claim 9, characterized in that: In step (5), the sintering temperature is 1530-1680° C., the sintering time is 10-20 min, and the pressure is 70-100 MPa.