Carbon ceramic part and preparation method thereof, carbon ceramic brake disc and vehicle
By using specific contents of zirconium carbide and carbon fiber structures in carbon ceramic brake discs, the problem of silicon carbide reacting with oxygen to form silicon oxide at high temperatures is solved, and the mechanical properties and oxidation resistance of carbon ceramics are improved, ensuring the brake of the brake disc Performance and service life.
Patent Information
- Application Number
- CN202310624238.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-30
- Publication Date
- 2024-12-03
AI Technical Summary
The existing carbon ceramic brake discs react with silicon carbide with oxygen at high temperature to form silicon oxide, resulting in low melting point and poor density, reducing the antioxidant ability.
Carbon ceramics with specific contents of zirconium carbide and carbon fiber structures are used to react zirconium carbide with oxygen to generate zirconium oxide, which improves oxidation resistance, and enhances mechanical properties and wear resistance through the design of the fiber layer.
It improves the mechanical properties and oxidation resistance of carbon ceramics, ensuring the brake performance and service life of the brake disc in high temperature environments.
Abstract
Description
Technical Field
[0001] The invention relates to brake disc technology, and in particular to a carbon-ceramic component and a preparation method thereof, a carbon-ceramic brake disc and a vehicle. Background Art
[0002] At present, carbon ceramic brake discs are mostly made of carbon fiber reinforced silicon carbide materials. However, silicon carbide reacts with oxygen at high temperatures to form silicon oxide, which has a low melting point and poor density, thus reducing the anti-oxidation ability of carbon ceramic brake discs. Therefore, it is necessary to improve the mechanical properties of carbon ceramic brake discs without affecting their anti-oxidation performance. Summary of the invention
[0003] The purpose of the present invention is to overcome at least one of the problems existing in the above-mentioned prior art and provide a carbon ceramic part and a preparation method thereof, a carbon ceramic brake disc, and a vehicle. The carbon ceramic part has excellent mechanical properties, wear resistance and oxidation resistance.
[0004] The first aspect of the present invention is to provide a carbon ceramic component, comprising 25-50 parts by weight of carbon, 40-60 parts by weight of silicon carbide, 2-10 parts by weight of silicon, and less than 15 parts by weight of zirconium carbide.
[0005] Preferably, it comprises 30-40 parts by weight of carbon, 45-55 parts by weight of silicon carbide, 3-7 parts by weight of silicon, and 7-12 parts by weight of zirconium carbide.
[0006] Preferably, the structure of the carbon ceramic component comprises a first long fiber layer, a short fiber layer and a second long fiber layer which are arranged in sequence.
[0007] Preferably, the thickness of the first long fiber layer and the second long fiber layer are independently 0.5-6 mm, and the fiber length is independently greater than 60 mm; the thickness of the short fiber layer is 26-32 mm, and the fiber length is less than 30 mm.
[0008] A second aspect of the present invention is to provide a method for preparing a carbon ceramic part, comprising the following steps: Mixing carbon powder, phenolic resin powder, silicon carbide powder, zirconium oxide powder and short fiber bundles to obtain a short fiber mixture, wherein the carbon powder is 10-20 parts by weight, the phenolic resin powder is 5-25 parts by weight, the silicon carbide powder is 2-30 parts by weight, the zirconium oxide powder is 10-25 parts by weight, and the short fiber bundle is 30-60 parts by weight; Mixing carbon powder, phenolic resin powder, silicon carbide powder, zirconium oxide powder and solvent to obtain a coating slurry, and applying the coating slurry to the surface of the long fiber cloth to obtain a coated long fiber cloth; Placing one or more layers of coated long fiber cloth on the bottom surface of the mold, filling the short fiber mixture, and then placing one or more layers of coated long fiber cloth on the short fiber mixture, and obtaining a green body after curing and carbonizing; The green body is subjected to liquid phase siliconization to obtain a carbon ceramic part.
[0009] Preferably, the carbon powder is 12-16 parts by weight, the phenolic resin powder is 10-20 parts by weight, the silicon carbide powder is 5-25 parts by weight, the zirconium oxide powder is 13-22 parts by weight, and the short fiber bundle is 35-50 parts by weight.
[0010] Preferably, the particle size of the carbon powder is 0.5-50 μm, the particle size of the silicon carbide powder is 0.5-50 μm, and the particle size of the zirconium oxide powder is 5-150 μm.
[0011] Preferably, the curing conditions include: curing by pressurizing at 130-180° C. with a pressure of 5-30 MPa.
[0012] Preferably, the carbonization temperature is 1500-1800° C., and the insulation time is 2-4 hours.
[0013] Preferably, arranging the short fiber mixture on the surface of the coated long fiber cloth comprises: arranging one or more layers of coated long fibers in a mold, then filling the short fiber mixture, and then arranging one or more layers of coated long fibers on the short fiber mixture.
[0014] A third aspect of the present invention is to provide a carbon-ceramic brake disc, comprising the aforementioned carbon-ceramic part or the carbon-ceramic part prepared by the aforementioned preparation method.
[0015] A fourth aspect of the present invention is to provide a vehicle comprising the aforementioned carbon-ceramic brake disc.
[0016] The invention increases the mechanical properties of the carbon ceramic by making the carbon ceramic contain a specific content of zirconium carbide. Under the application environment of the carbon ceramic, the zirconium carbide of the carbon ceramic reacts with oxygen at high temperature to produce zirconium oxide, thereby improving the oxidation resistance of the carbon ceramic. DETAILED DESCRIPTION
[0017] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0018] The present invention provides a carbon ceramic component, comprising 25-50 parts by weight of carbon, 40-60 parts by weight of silicon carbide, 2-10 parts by weight of silicon, and less than 15 parts by weight of zirconium carbide.
[0019] The invention increases the mechanical properties of the carbon ceramic by making the carbon ceramic contain a specific content of zirconium carbide. Under the application environment of the carbon ceramic, the zirconium carbide of the carbon ceramic reacts with oxygen at high temperature to produce zirconium oxide, thereby improving the oxidation resistance of the carbon ceramic.
[0020] In some embodiments, the carbon ceramic component includes 30-40 parts by weight of carbon, 45-55 parts by weight of silicon carbide, 3-7 parts by weight of silicon, and 7-12 parts by weight of zirconium carbide, which can further increase the mechanical properties of the carbon ceramic component.
[0021] In some embodiments, the structure of the carbon ceramic component includes a first long fiber layer, a short fiber layer, and a second long fiber layer arranged in sequence. Since the fiber length in the long fiber layer is greater than the fiber length in the short fiber layer, the first long fiber layer and / or the second long fiber layer on the surface of the carbon ceramic component can further enhance the friction resistance of the carbon ceramic component. Specifically, the fiber length in the short fiber layer is less than or equal to 30 mm, and the fiber length in the first long fiber layer and the second long fiber layer is greater than or equal to 60 mm. By controlling the length of the short fibers and the length of the long fibers within the above range, the mechanical properties of the carbon ceramic component can be ensured.
[0022] In some embodiments, the thickness of the first long fiber layer can be 0.5-6 mm, the thickness of the short fiber layer can be 26-32 mm, and the thickness of the second long fiber layer can be 0.5-6 mm. By controlling the thickness of the aforementioned fiber layers, the strength of the carbon ceramic part can be enhanced, and the difficulty of manufacturing the carbon ceramic part can be reduced, thereby saving costs.
[0023] The present invention also provides a method for preparing a carbon ceramic part, comprising the following steps: S1: mixing carbon powder, phenolic resin powder, silicon carbide powder, zirconium oxide powder and short fiber bundles to obtain a short fiber mixture, wherein the carbon powder is 10-20 parts by weight, the phenolic resin powder is 5-25 parts by weight, the silicon carbide powder is 2-30 parts by weight, the zirconium oxide powder is 10-25 parts by weight, and the short fiber bundle is 30-60 parts by weight; S2: mixing carbon powder, phenolic resin powder, silicon carbide powder, zirconium oxide powder and solvent to obtain a coating slurry, and applying the coating slurry to the surface of the long fiber cloth to obtain a coated long fiber cloth; S3: placing one or more layers of coated long fiber cloth on the bottom surface of the mold, filling the short fiber mixture, and then placing one or more layers of coated long fiber cloth on the short fiber mixture, and obtaining a green body after curing and carbonization; S4: Liquid phase siliconizing the green body to obtain a carbon ceramic part.
[0024] The present invention adds a specific amount of zirconium oxide, and after carbonization treatment, the carbon contained in the raw material reacts with zirconium oxide to produce zirconium carbide, and the final carbon ceramic part contains zirconium carbide, which increases the mechanical properties of the carbon ceramic part. Under the application environment, the zirconium carbide of the carbon ceramic part reacts with oxygen to produce zirconium oxide at high temperatures, thereby improving the oxidation resistance of the carbon ceramic part. For example, the carbon ceramic part is made into a carbon ceramic brake disc and installed in a vehicle. The temperature of the vehicle can reach up to 1100°C during rapid braking. At this time, the zirconium carbide reacts with oxygen to produce zirconium oxide, thereby improving the oxidation resistance of the brake disc.
[0025] In some embodiments, by controlling the particle size of zirconium oxide powder, carbon is allowed to exist in gaseous form during the reduction of zirconium oxide, and a certain amount of zirconium carbide whiskers are precipitated on the pore surface of the green body, further enhancing the strength of the carbon ceramic component. Preferably, the particle size of the zirconium oxide powder is 0.5-100 μm.
[0026] In some embodiments, the particle size of the carbon powder may be 0.5-50 μm, and the particle size of the silicon carbide powder may be 0.5-50 μm, which helps to improve the fluidity of the sizing material on the fiber surface during the hot pressing process to obtain a dense hot pressed green body.
[0027] In some embodiments, the comprehensive performance of carbon ceramics can be further improved by controlling the carbon powder to 12-16 parts by weight, the phenolic resin powder to 10-20 parts by weight, the silicon carbide powder to 5-25 parts by weight, the zirconium oxide powder to 13-22 parts by weight, and the short fiber bundle content to 35-50 parts by weight.
[0028] In some embodiments, in step S1, the carbon powder, phenolic resin powder, silicon carbide powder, zirconium oxide powder and short fiber bundles can be placed in a solvent first so that they can be fully dispersed. The solvent used can include but is not limited to ethanol, methanol, purified water, etc. For example, the carbon powder, phenolic resin powder, silicon carbide powder, zirconium oxide powder and short fiber bundles can be placed in ethanol and mixed, and stirred for 1-3 hours. After stirring, the mixed solution is heated until the ethanol evaporates to obtain a dry mixture.
[0029] In some embodiments, the short fiber bundles bonded in the dried mixture can be separated to obtain a short fiber mixture.
[0030] In some embodiments, in step S2, carbon powder, phenolic resin powder, silicon carbide powder, and zirconium oxide powder can be first placed in a solvent so that they can be fully dispersed. The solvent used may include, but is not limited to, ethanol, methanol, pure water, etc. For example, carbon powder, phenolic resin powder, silicon carbide powder, and zirconium oxide powder can be placed in ethanol and mixed to obtain a brushing slurry, and the brushing slurry is applied to the surface of the long fiber cloth to obtain a brushed long fiber cloth. Specifically, the content of carbon powder can be 10-30 parts by weight, the content of phenolic resin powder can be 15-40 parts by weight, the content of silicon carbide powder can be 0.1-25 parts by weight, and the content of zirconium oxide powder can be 15-40 parts by weight. Controlling the solid content of the brushing slurry at 60%-80% can better apply the brushing slurry to the surface of the long fiber cloth.
[0031] In some embodiments, in step S2, after the coating slurry is applied to the surface of the long-fiber cloth, the solvent in the coating slurry is dried to obtain the coated long-fiber cloth. The drying temperature may be 60-70°C.
[0032] In some embodiments, in step S3, one or more layers of coated long fibers are arranged in a mold, and then the short fiber mixture is filled in, and then one or more layers of coated long fibers are arranged on the short fiber mixture, and then pressurized and cured at 130-180°C with a pressure of 5-30MPa.
[0033] In some embodiments, the carbonization temperature may be 1500-1800°C, within which zirconium oxide and carbon react to form zirconium carbide, and the holding time is 2-4 hours to obtain a green body. Preferably, the carbonization temperature may be 1600-1650°C.
[0034] In some implementations, the blank may be deburred and heat dissipation holes may be processed, and then liquid phase siliconization may be performed to obtain a carbon ceramic part.
[0035] The present invention also provides a carbon-ceramic brake disc, comprising the aforementioned carbon-ceramic part or the carbon-ceramic part prepared by the aforementioned preparation method.
[0036] The carbon ceramic parts are machined to obtain the required carbon ceramic brake disc. The carbon ceramic brake disc has good mechanical strength. During the operation of the carbon ceramic brake disc, at high temperature, the zirconium carbide of the carbon ceramic brake disc will react with oxygen in the air to produce zirconium oxide, which can improve the anti-oxidation performance of the carbon ceramic brake disc.
[0037] The present invention also provides a vehicle, comprising the aforementioned carbon-ceramic brake disc. The vehicle using the carbon-ceramic brake disc not only has excellent braking performance, but also has good mechanical properties and a long service life.
[0038] The present invention will be described in detail below by way of examples, but the present invention is not limited to the following examples. Example 1
[0039] (1) Mix carbon powder, phenolic resin powder, silicon carbide powder, zirconium oxide powder, short fiber bundles and ethanol, and stir for 2 hours; wherein the carbon powder (particle size between 1-20 μm) content is 14 parts by weight, the phenolic resin powder is 16 parts by weight, the silicon carbide powder (particle size between 1-20 μm) content is 8 parts by weight, the zirconium oxide powder (particle size between 0.5-50 μm) content is 15 parts by weight, and the short fiber content is 47 parts by weight; heat the stirred mixture until the alcohol is completely evaporated to obtain a dry mixture; (2) separating the bonded short fiber bundles in the dry mixture to obtain a short fiber mixture; (3) mixing carbon powder, phenolic resin powder, silicon carbide powder, zirconium oxide powder and ethanol, wherein the content of carbon powder is 26 parts by weight, the content of phenolic resin powder is 30 parts by weight, the content of silicon carbide powder is 16 parts by weight, the content of zirconium oxide powder is 29 parts by weight, and the solid content is 70%, to obtain a coating slurry; applying the coating slurry on the surface of the long fiber cloth, and placing the cloth in an oven to completely dry the alcohol, to obtain a coated long fiber cloth; (4) arranging the short fiber mixture on the surface of the coated long fiber cloth includes: arranging one or more layers of coated long fibers in a mold, then filling the short fiber mixture, and then arranging one or more layers of coated long fibers on the short fiber mixture; pressurizing and curing at 150° C. and a pressure of 15 MPa; (5) The solidified green body is placed in a carbonization furnace for carbonization at a temperature of 1600°C for 3 hours; (6) Deburring the carbonized blank and processing heat dissipation holes; (7) The processed carbide body is subjected to liquid phase siliconization to obtain a carbon ceramic body; the surface and side surfaces are mechanically processed to obtain the desired carbon ceramic brake disc.
[0040] The carbon-ceramic brake disc of Example 1 has a mass composition of 32 wt % carbon, 54 wt % silicon carbide, 6 wt % silicon, and 8 wt % zirconium carbide. Example 2
[0041] (1) Mix carbon powder, phenolic resin powder, silicon carbide powder, zirconium oxide powder, short fiber bundles and ethanol, and stir for 2 hours; wherein the carbon powder (particle size between 1-20 μm) content is 14 parts by weight, the phenolic resin powder is 11 parts by weight, the silicon carbide powder (particle size between 1-20 μm) content is 15 parts by weight, the zirconium oxide powder (particle size between 10-80 μm) content is 22 parts by weight, and the short fiber content is 38 parts by weight; heat the stirred mixture until the alcohol is completely evaporated to obtain a dry mixture; (2) separating the bonded short fiber bundles in the dry mixture to obtain a short fiber mixture; (3) mixing carbon powder, phenolic resin powder, silicon carbide powder, zirconium oxide powder and ethanol, wherein the content of carbon powder is 23 parts by weight, the content of phenolic resin powder is 18 parts by weight, the content of silicon carbide powder is 24 parts by weight, the content of zirconium oxide powder is 35 parts by weight, and the solid content is 70%, to obtain a coating slurry; applying the coating slurry on the surface of the long fiber cloth, and placing the cloth in an oven to completely dry the alcohol, to obtain a coated long fiber cloth; (4) arranging the short fiber mixture on the surface of the coated long fiber cloth includes: arranging one or more layers of coated long fibers in a mold, then filling the short fiber mixture, and then arranging one or more layers of coated long fibers on the short fiber mixture; pressurizing and curing at 150° C. and a pressure of 15 MPa; (5) The solidified green body is placed in a carbonization furnace for carbonization at a temperature of 1600°C for 3 hours; (6) Deburring the carbonized blank and processing heat dissipation holes; (7) The processed carbide body is subjected to liquid phase siliconization to obtain a carbon ceramic body; the surface and side surfaces are mechanically processed to obtain the desired carbon ceramic brake disc.
[0042] The carbon-ceramic brake disc of Example 2 has a mass composition of 35 wt % carbon, 48 wt % silicon carbide, 5 wt % silicon, and 12 wt % zirconium carbide. Example 3
[0043] (1) Mix carbon powder, phenolic resin powder, silicon carbide powder, zirconium oxide powder, short fiber bundles and ethanol, and stir for 2 hours; wherein the carbon powder (particle size between 1-20 μm) content is 13 parts by weight, the phenolic resin powder is 15 parts by weight, the silicon carbide powder (particle size between 1-20 μm) content is 23 parts by weight, the zirconium oxide powder (particle size between 10-80 μm) content is 14 parts by weight, and the short fiber content is 35 parts by weight; heat the stirred mixture until the alcohol is completely evaporated to obtain a dry mixture; (2) separating the bonded short fiber bundles in the dry mixture to obtain a short fiber mixture; (3) mixing carbon powder, phenolic resin powder, silicon carbide powder, zirconium oxide powder and ethanol, wherein the content of carbon powder is 20 parts by weight, the content of phenolic resin powder is 22 parts by weight, the content of silicon carbide powder is 36 parts by weight, the content of zirconium oxide powder is 22 parts by weight, and the solid content is 70%, to obtain a coating slurry; applying the coating slurry on the surface of the long fiber cloth, and placing the cloth in an oven to completely dry the alcohol, to obtain a coated long fiber cloth; (4) arranging the short fiber mixture on the surface of the coated long fiber cloth includes: arranging one or more layers of coated long fibers in a mold, then filling the short fiber mixture, and then arranging one or more layers of coated long fibers on the short fiber mixture; pressurizing and curing at 150° C. and a pressure of 15 MPa; (5) The solidified green body is placed in a carbonization furnace for carbonization at a temperature of 1600°C for 3 hours; (6) Deburring the carbonized blank and processing heat dissipation holes; (7) The processed carbide body is subjected to liquid phase siliconization to obtain a carbon ceramic body; the surface and side surfaces are mechanically processed to obtain the desired carbon ceramic brake disc.
[0044] The carbon-ceramic brake disc of Example 3 has a mass composition of 30 wt % carbon, 53 wt % silicon carbide, 6 wt % silicon, and 7 wt % zirconium carbide. Example 4
[0045] (1) Mix carbon powder, phenolic resin powder, silicon carbide powder, zirconium oxide powder, short fiber bundles and ethanol, and stir for 2 hours; wherein the carbon powder (particle size between 1-20 μm) content is 14 parts by weight, the phenolic resin powder is 18 parts by weight, the silicon carbide powder (particle size between 1-20 μm) content is 16 parts by weight, the zirconium oxide powder (particle size between 10-80 μm) content is 15 parts by weight, and the short fiber content is 37 parts by weight; heat the stirred mixture until the alcohol is completely evaporated to obtain a dry mixture; (2) separating the bonded short fiber bundles in the dry mixture to obtain a short fiber mixture; (3) mixing carbon powder, phenolic resin powder, silicon carbide powder, zirconium oxide powder and ethanol, wherein the content of carbon powder is 22 parts by weight, the content of phenolic resin powder is 29 parts by weight, the content of silicon carbide powder is 26 parts by weight, the content of zirconium oxide powder is 23 parts by weight, and the solid content is 70%, to obtain a coating slurry; applying the coating slurry on the surface of the long fiber cloth, and placing the cloth in an oven to completely dry the alcohol, to obtain a coated long fiber cloth; (4) arranging the short fiber mixture on the surface of the coated long fiber cloth includes: arranging one or more layers of coated long fibers in a mold, then filling the short fiber mixture, and then arranging one or more layers of coated long fibers on the short fiber mixture; pressurizing and curing at 150° C. and a pressure of 15 MPa; (5) The solidified green body is placed in a carbonization furnace for carbonization at a temperature of 1600°C for 3 hours; (6) Deburring the carbonized blank and processing heat dissipation holes; (7) The processed carbide body is subjected to liquid phase siliconization to obtain a carbon ceramic body; the surface and side surfaces are mechanically processed to obtain the desired carbon ceramic brake disc.
[0046] The carbon-ceramic brake disc of Example 4 has a mass composition of 36 wt % carbon, 49 wt % silicon carbide, 6 wt % silicon, and 9 wt % zirconium carbide.
[0047] Comparative Example 1 (1) Mix carbon powder, phenolic resin powder, silicon carbide powder, short fiber bundles and ethanol, and stir for 2 hours; wherein the carbon powder (particle size between 1-20 μm) content is 21 parts by weight, the phenolic resin powder is 18 parts by weight, the silicon carbide powder (particle size between 1-20 μm) content is 9 parts by weight, and the short fiber content is 52 parts by weight; heat the stirred mixture until the alcohol is completely evaporated to obtain a dry mixture; (2) separating the bonded short fiber bundles in the dry mixture to obtain a short fiber mixture; (3) mixing carbon powder, phenolic resin powder, silicon carbide powder and ethanol, wherein the content of carbon powder is 44 parts by weight, the content of phenolic resin powder is 37 parts by weight, the content of silicon carbide powder is 19 parts by weight, and the solid content is 70%, to obtain a coating slurry; applying the coating slurry on the surface of the long-fiber cloth, and placing the cloth in an oven to completely dry the alcohol, to obtain a coated long-fiber cloth; (4) Fill the short fiber mixture into the mold, and then place one or more layers of coated long fiber cloth on the short fiber mixture; pressurize and cure at 150°C and a pressure of 15MPa; (5) The solidified green body is placed in a carbonization furnace for carbonization at a temperature of 1600°C for 3 hours; (6) Deburring the carbonized blank and processing heat dissipation holes; (7) The processed carbide body is subjected to liquid phase siliconization to obtain a carbon ceramic body; the surface and side surfaces are mechanically processed to obtain the desired carbon ceramic brake disc.
[0048] The carbon-ceramic brake disc of Comparative Example 1 has a mass composition of 35 wt % carbon, 60 wt % silicon carbide, and 5 wt % silicon.
[0049] Bending strength: The WDW-100 electronic universal testing machine is used for bending strength test. The bending performance test of the material is mainly to determine the size of the plastic deformation or the load size when the material is deformed under a certain load.
[0050] XRD analysis: D / max-rB X-ray diffractometer was used to measure the crystal phase composition and graphitization degree of the test samples.
[0051] Testing method for graphitization degree: Analyze the (002) crystal plane d value (the spacing between the crystal planes) of carbon in the sample based on XRD, and then calculate the graphitization degree of the sample based on the formula G=(0.344-d) / (0.344-0.3354).
[0052] Wear: The dynamic friction coefficient and wear rate of the carbon ceramic brake disc sample were tested using the MM-100 friction tester. The effective friction surface of the test ring has an outer diameter of D75mm / inner diameter of D55mm×10mm, and a specific pressure of 98N / cm 2 , inertia is 3kgf·cm·s 2 , the linear speed is 25m / s. Silicon carbide reacts with oxygen at high temperature to generate silicon oxide, which causes the material to peel off and irregular small pits to appear on the friction surface. The oxidation resistance of the sample is evaluated according to the amount of wear. The smaller the wear, the better the oxidation resistance of the sample.
[0053] Table 1 Bending strength MPa Wear loss μm / surface·times Graphitization degree Example 1 129 0.72 27% Example 2 157 0.48 48.% Example 3 149 0.65 35% Example 4 134 0.69 39% Comparative Example 1 91 1.22 15% It can be seen from the test results of Examples 1-4 and Comparative Example 1 in Table 1 that the carbon ceramic parts provided in the present application have excellent bending strength and wear resistance, small wear amount and corresponding good oxidation resistance.
[0054] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0055] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0056] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A carbon ceramic part, characterized in that: The composite material comprises 25-50 parts by weight of carbon, 40-60 parts by weight of silicon carbide, 2-10 parts by weight of silicon, and less than 15 parts by weight of zirconium carbide.
2. The carbon ceramic part according to claim 1, characterized in that: The invention comprises 30-40 parts by weight of carbon, 45-55 parts by weight of silicon carbide, 3-7 parts by weight of silicon, and 7-12 parts by weight of zirconium carbide.
3. The carbon ceramic part according to claim 1, characterized in that: The structure of the carbon ceramic component comprises a first long fiber layer, a short fiber layer and a second long fiber layer which are arranged in sequence.
4. The carbon ceramic part according to claim 3, characterized in that: The thickness of the first long fiber layer and the second long fiber layer are independently 0.5-6 mm, and the fiber length is independently greater than 60 mm; the thickness of the short fiber layer is 26-32 mm, and the fiber length is less than 30 mm.
5. A method for preparing a carbon ceramic part, characterized in that: The following steps are involved: Mixing carbon powder, phenolic resin powder, silicon carbide powder, zirconium oxide powder and short fiber bundles to obtain a short fiber mixture, wherein the carbon powder is 10-20 parts by weight, the phenolic resin powder is 5-25 parts by weight, the silicon carbide powder is 2-30 parts by weight, the zirconium oxide powder is 10-25 parts by weight, and the short fiber bundle is 30-60 parts by weight; Mixing carbon powder, phenolic resin powder, silicon carbide powder, zirconium oxide powder and solvent to obtain a coating slurry, and applying the coating slurry to the surface of the long fiber cloth to obtain a coated long fiber cloth; Placing one or more layers of coated long fiber cloth on the bottom surface of the mold, filling the short fiber mixture, and then placing one or more layers of coated long fiber cloth on the short fiber mixture, and obtaining a green body after curing and carbonizing; The green body is subjected to liquid phase siliconization to obtain a carbon ceramic part.
6. The preparation method according to claim 5, characterized in that: The carbon powder is 12-16 parts by weight, the phenolic resin powder is 10-20 parts by weight, the silicon carbide powder is 5-25 parts by weight, the zirconium oxide powder is 13-22 parts by weight, and the short fiber bundle is 35-50 parts by weight.
7. The preparation method according to claim 5, characterized in that: The particle size of the carbon powder is 0.5-50 μm, the particle size of the silicon carbide powder is 0.5-50 μm, and the particle size of the zirconium oxide powder is 5-150 μm.
8. The preparation method according to claim 5, characterized in that The curing conditions include: curing by pressurizing at 130-180° C. and a pressure of 5-30 MPa.
9. The preparation method according to claim 5, characterized in that: The carbonization temperature is 1500-1800° C., and the insulation time is 2-4 hours.
10. The preparation method according to claim 5, characterized in that: Arranging the short fiber mixture on the surface of the coated long fiber cloth includes: arranging one or more layers of coated long fibers in a mold, then filling the short fiber mixture, and then arranging one or more layers of coated long fibers on the short fiber mixture.
11. A carbon ceramic brake disc, characterized in that: The invention comprises the carbon ceramic part according to any one of claims 1 to 4 or the carbon ceramic part prepared by the preparation method according to any one of claims 5 to 10.
12. A vehicle, characterized in that: Including the carbon-ceramic brake disc as claimed in claim 11.
Citation Information
Patent Citations
Carbon-ceramic composite brake disc and preparation method thereof
CN103553695A
Carbon fiber reinforced carbon-silicon carbide-zirconium carbide composite material and preparation method thereof
CN111099911A
Preparation method of wear-resistant carbon / ceramic brake material
CN112409008A
Carbon / ceramic brake disc with sandwich structure
CN115823151A
Carbon fiber reinforced ceramic brake disc and method for manufacturing the same
KR1020160133580A
Cited By
Carbon-ceramic composite material and preparation method therefor, carbon-ceramic product, carbon-ceramic brake disc, and transportation vehicle
WO2026124309A1