Method for synthesizing ethylbenzene through alkylation of benzene and ethylene
By using EWT structure molecular sieve catalysts containing aluminum atoms and heteroatoms, the production process of ethylbenzene is optimized, and the problems of low ethylene conversion and high by-products caused by mesoporous molecular sieve are solved, and efficient ethylation selectivity and low By-product generation.
Patent Information
- Application Number
- CN202310640060.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-31
- Publication Date
- 2024-12-03
AI Technical Summary
In the prior art, due to the limitation of the pore structure of the mesoporous molecular sieve during the production process of ethylbenzene, the ethylene conversion rate is low, the by-product selectivity is high, and the xylene and C9 components are high, which affects product quality and price.
A heteroatomic EWT structure molecular sieve containing aluminum atoms and heteroatoms on the skeleton is used as a catalyst to improve the ethylene conversion and ethylation selectivity by optimizing the acidic center distribution and pore structure, and reduce the selectivity of xylene and C9 components.
It significantly improves the ethylene conversion rate and ethylation selectivity, reduces the generation of by-products such as xylene and isopropyl benzene, reduces the selectivity of C9 components, improves the activity and stability of the catalyst, and optimizes product quality.
Smart Images

Figure CN119059865A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of petrochemical industry, and in particular to a method for synthesizing ethylbenzene by alkylation of benzene and ethylene. Background Art
[0002] Ethylbenzene is an important organic chemical raw material, mainly used to produce styrene, which is an important monomer for synthesizing polymer materials. In recent years, my country's demand for styrene, especially high-quality styrene, has been increasing. At present, the main production route of ethylbenzene is the alkylation reaction of benzene and ethylene. In this reaction process, the target product ethylbenzene will continue to undergo alkylation reaction with ethylene to produce polyethylbenzene components such as diethylbenzene and triethylbenzene. Some polyethylbenzene components can be converted into ethylbenzene through transalkylation reaction, thereby increasing the yield of ethylbenzene products. In industry, ethylbenzene is generally produced by alkylation reaction and transalkylation reaction supporting processes. Among them, the alkylation reaction process is divided into molecular sieve gas phase method and liquid phase method. The molecular sieve gas phase alkylation technology for ethylbenzene is represented by the Mobil / Badger process. This process uses medium-pore ZSM-5 molecular sieve as a catalyst, has the advantages of no corrosion, no pollution, simple process, high ethylene space velocity and high heat recovery rate, and was industrialized in the 1980s.
[0003] US4107224 reported that the reaction temperature was 375-425℃ with HZSM-5 molecular sieve as catalyst, and the xylene content was high, >1500ppm. Since the boiling points of xylene and ethylbenzene are close, separation is difficult, which affects the product quality and price of ethylbenzene. At the same time, the side reactions such as polymerization and cracking of ethylene lead to the production of cumene (C 9 The selectivity of by-products such as ethylbenzene and C-butylene is also high. This is because the pore diameter of the mesoporous molecular sieve is close to the diameter of benzene / alkylbenzene, and the diffusion of reactant and product molecules in the pores is limited, so the reaction needs to be carried out at a higher temperature. Under high reaction temperature conditions, side reactions such as ethylbenzene isomerization to xylene and ethylene to propylene and butene are intensified, resulting in xylene, C-butylene and C-butylene in the product. 9 The component content is high.
[0004] According to the number of pore window rings, molecular sieves can be divided into microporous molecular sieves (8MR), medium pore molecular sieves (10MR), large pore molecular sieves (12MR) and ultra-large pore molecular sieves (>12MR). Ultra-large pore molecular sieves break through the pore limitations of molecular sieves and show advantages in improving the reaction activity of macromolecules, extending the life of molecular sieves and improving product selectivity. Among the 255 molecular sieve structures that have been disclosed on the IZA website, there are only more than 10 ultra-large pore molecular sieves, including phosphorus aluminum / gallium, silicon germanium / gallium and silicon aluminum molecular sieves. However, the number of B acid centers of ultra-large pore silicon aluminum molecular sieves is small, and they still need to be synthesized under high silicon or pure silicon conditions, which makes them difficult to be used in macromolecular acid-catalyzed reactions. The addition of aluminum can adjust the acid center of the molecular sieve, and how to promote aluminum to enter the ultra-large pore molecular sieve framework is a key issue. Inserting a large aluminum-oxygen tetrahedron into a regular silica molecular sieve framework may cause irregular deformation of the framework and extend to the entire molecular sieve crystal, making the coordination of the atoms in the molecular sieve framework complicated. This is from the molecular sieve. 29 Si MAS NMR and 27 Al MAS NMR spectrum can be seen (1. CAFyfe, H. Strobl, GT Kokotailo, CT Pastzto, GE Barlow, S. Bradley, Zeolites, 8 (1988); 2. J. Stelzer, M. Paulus, M. Hunger, J. Weitkamp, Microporous Mesoporous Mater., 22 (1998) 1.; 3. JA van Bokhoven, DC Koningsberger, P. Kunkeler, P. van Bekkum and A. PM Kentgens, J. Am. Chem. Soc., 122 (2000) 12842.). In addition to aluminum, heteroatoms can also be inserted into the molecular sieve framework, such as iron, gallium, boron and titanium. Among them, compared with aluminum, the size of the boron oxygen tetrahedron is smaller and it is easier to enter the molecular sieve framework. Without distorting the silicon oxygen tetrahedron, the coordination of silicon and boron in the silicon-boron molecular sieve is relatively simple. This is from the molecular sieve. 29 Si MAS NMR and 11 B MAS NMR spectra can be seen (4. C. Yang, Q. Xu, C. Hu, Mat. Chem. Phys., 63 (2000) 55; 5. SI Zones, SJ. Hwang, Microporous Mesoporous Mater., 58 (2003) 263.). However, due to the low stability of boron-containing molecular sieves, boron atoms are more likely to fall off from the framework during the thermal / hydrothermal treatment of ion exchange. Summary of the invention
[0005] The purpose of the present invention is to provide a method for synthesizing ethylbenzene by alkylation of benzene and ethylene. The method uses a heteroatom EWT structure molecular sieve containing aluminum atoms and heteroatoms on the skeleton as a catalyst. When catalyzing the alkylation reaction of benzene and ethylene, the ethylene conversion rate and ethylation selectivity can be improved, while the xylene content and C 9 Component selectivity.
[0006] In order to achieve the above object, the present disclosure provides a method for synthesizing ethylbenzene by alkylation of benzene and ethylene, the method comprising: contacting benzene with ethylene under alkylation reaction conditions and in the presence of a catalyst; wherein the catalyst is a heteroatom EWT structure molecular sieve, the framework of the heteroatom EWT structure molecular sieve contains silicon elements, aluminum elements and heteroatom elements, and the heteroatom EWT structure molecular sieve is SiO 2 Silicon and Al 2 O 3 The molar ratio of aluminum element is more than 10, and the heteroatom EWT structure molecular sieve is SiO 2 The molar ratio of silicon element calculated as silicon element to heteroatom element calculated as heteroatom oxide is greater than 10; the heteroatom element includes one or more of boron, iron, titanium, gallium and germanium.
[0007] Optionally, the alkylation reaction conditions include: temperature of 300-360°C, preferably 330-360°C; time of 10-400h, preferably 20-100h; pressure of 0.6-1.2MPa, preferably 0.8-1.0MPa; the feed molar ratio of benzene to ethylene is (4-8):1, preferably (6-7.5):1; preferably, the reaction is carried out in a fixed bed reactor, and the mass space velocity of ethylene is 0.5-10.0h -1 , preferably 5.0~8.0h -1 .
[0008] Optionally, the heteroatom EWT structured molecular sieve is SiO 2 Silicon and Al 2 O 3 The molar ratio of aluminum element is 10 to 60, preferably 15 to 30; the heteroatom EWT structure molecular sieve is SiO 2 The molar ratio of silicon element calculated as silicon and the heteroatom element calculated as heteroatom oxide is 10-250, preferably 120-240.
[0009] Optionally, when the heteroatom element is boron, the heteroatom EWT structure molecular sieve is SiO 2 Silicon and B 2 O 3The molar ratio of boron to the heteroatom element is 120 to 180; when the heteroatom element is one or more of iron, titanium, gallium and germanium, the heteroatom EWT structure molecular sieve is SiO 2 The molar ratio of silicon element calculated as silicon element to heteroatom element calculated as heteroatom oxide is 150-240.
[0010] Optionally, the total specific surface area of the heteroatom EWT structure molecular sieve is 300 to 650 cm 2 / g, preferably 450 to 580 cm 2 / g; total pore volume is 0.25~0.60cm 3 / g, preferably 0.25 to 0.45 cm 3 / g; the volume of mesopores with a pore size of 2.0 to 20.0 nm is 0.05 to 0.35 cm 3 / g, preferably 0.10 to 0.25 cm 3 / g; the percentage of the mesopore volume with a pore size of 2.0-20.0nm to the total pore volume is 30-50%, preferably 35-50%; the average particle size of the heteroatom EWT structure molecular sieve is 0.2-1.5μm, preferably 0.3-1.0μm; the relative crystallinity is 50-100%, preferably 75-95%; the ratio of the B acid amount to the L acid amount of the heteroatom EWT structure molecular sieve measured by pyridine adsorption infrared method at 350°C is 0.3-0.6; preferably, the heteroatom EWT structure molecular sieve is a hydrogen type heteroatom EWT structure molecular sieve.
[0011] Optionally, the method further comprises preparing the catalyst by the following steps:
[0012] (1) mixing a silicon source, a heteroatom element source, a first alkali source, a first organic template and water, and performing a first crystallization on the obtained first material to be crystallized to obtain a molecular sieve raw powder; and calcining the molecular sieve raw powder to obtain a sodium-type molecular sieve;
[0013] (2) performing ion exchange on the sodium molecular sieve using an acid solution, mixing the obtained molecular sieve intermediate with an aluminum source, a second alkali source and a second organic template, and performing a second crystallization on the obtained second material to be crystallized;
[0014] Wherein, the heteroatom element includes one or more of boron, iron, titanium, gallium and germanium, the first organic template and the second organic template are respectively a cyclic diquaternary ammonium base compound and / or a cyclic diquaternary ammonium salt compound; the temperature of the first crystallization is 60-180°C, preferably 100-170°C; the time is 96-168h, preferably 96-144h; the temperature of the second crystallization is 60-180°C, preferably 100-170°C; the time is 96-168h, preferably 96-144h.
[0015] Optionally, the silicon source is selected from one or more of silica sol, water glass, solid silica gel, tetraethyl orthosilicate and white carbon black, preferably solid silica gel; the heteroatom element source is selected from one or more of boron oxide, boric acid, iron oxide, titanium oxide, gallium oxide and germanium oxide, preferably boron oxide and / or boric acid; the first alkali source and the second alkali source are respectively selected from one or more of sodium hydroxide, potassium hydroxide and lithium hydroxide, preferably, the first alkali source and the second alkali source are both sodium hydroxide; the aluminum source is selected from one or more of aluminum chloride, aluminum sulfate, hydrated aluminum oxide, sodium aluminate and aluminum sol, preferably sodium aluminate; the first organic template and the second organic template are respectively selected from at least one of the structures shown in formula (1): Where R 1 , R 2 , R 3 and R 4 are independently selected from alkyl groups having 1 to 4 carbon atoms, preferably, R 1 , R 2 , R 3 and R 4 Each is independently selected from one or more of methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl and tert-butyl, preferably methyl or ethyl; m is 2 or 3; n is any integer from 1 to 10; X - Including hydroxide ions or halogen anions.
[0016] Optionally, the silicon source is SiO 2 The heteroatom element source is calculated as heteroatom oxides. When the heteroatom element is boron, the SiO 2 With B 2 O 3 The molar ratio of SiO in the first material to be crystallized is 10 to 250, preferably 30 to 120; when the heteroatom element is one or more of iron, titanium, gallium and germanium, the molar ratio of SiO in the first material to be crystallized is 10 to 250, preferably 30 to 120; 2 The molar ratio of the heteroatom oxide to the heteroatom oxide is 10-250, preferably 30-150.
[0017] Optionally, in step (1), the silicon source is SiO 2 The heteroatom element source is calculated as heteroatom oxide, and the first organic template is calculated as T 1 It means that when the heteroatom element in the first material to be crystallized is boron, SiO 2 With B 2 O 3 The molar ratio of SiO is 10 to 250, preferably 30 to 120; when the heteroatom element is one or more of iron, titanium, gallium and germanium, SiO 2The molar ratio of OH to heteroatom oxide is 10 to 250, preferably 30 to 150; - The first alkali source and SiO 2 The molar ratio of T is 0.2 to 1.0, preferably 0.2 to 0.5; 1 With SiO 2 The molar ratio of H is 0.02 to 0.5, preferably 0.08 to 0.15; 2 O and SiO 2 The molar ratio of is 5 to 20, preferably 5 to 10; in step (2), the aluminum source is Al 2 O 3 The second organic template is T 2 Indicates that the SiO 2 With Al 2 O 3 The molar ratio of OH is 10 or more, preferably 10 to 60, more preferably 15 to 30; - The second alkali source and SiO 2 The molar ratio of T is 0.2 to 1.0, preferably 0.2 to 0.5; 2 With SiO 2 The molar ratio of H is 0.02 to 0.5, preferably 0.08 to 0.15; 2 O and SiO 2 The molar ratio is 5-20, preferably 5-10.
[0018] Optionally, in step (1), the calcination temperature is 400-650°C, and the time is 1-7h; in step (2), the weight ratio of the acid solution to the sodium molecular sieve is (1-100):1, the concentration of the acid solution is 0.01-0.10 mol / L, the ion exchange temperature is 60-90°C, and the time is 2-24h; the acid solution is selected from one or more of hydrochloric acid solution, nitric acid solution and sulfuric acid solution.
[0019] Through the above technical scheme, the present disclosure provides a method for synthesizing ethylbenzene by alkylation of benzene and ethylene. The method uses a heteroatom EWT structure molecular sieve containing aluminum atoms and heteroatoms on the skeleton as a catalyst. The heteroatom EWT structure molecular sieve has a 3D pore system composed of 21-membered rings and ten-membered rings, has a suitable acid center distribution, and shows advantages in improving the utilization rate of acid centers; in addition, the skeleton aluminum atoms of the molecular sieve can adjust the acid amount of the molecular sieve, and the skeleton heteroatoms can adjust the position and acid type of the skeleton aluminum, so that the acidity of the molecular sieve is more suitable and the intracrystalline mesopores are more abundant. When the heteroatom EWT structure molecular sieve is used for the alkylation reaction of benzene and ethylene, it shows optimized catalytic performance, can improve the ethylene conversion rate and ethylation selectivity, while reducing the xylene content, reducing the generation of by-products such as isopropylbenzene, and reducing C9 The component selectivity has a catalytic effect significantly better than the ten-membered ring ZSM-5 molecular sieve. The present invention adopts a secondary crystallization method of crystallization-decomposition-dissolution-recrystallization, first preparing an EWT structure molecular sieve containing silicon and heteroatoms, and then removing part of the framework heteroatoms to form a silanol nest, providing vacancies to facilitate Al atoms to enter the framework to complete isomorphous substitution, so as to prepare a molecular sieve with a lower silicon-aluminum ratio, while improving the acidity and pore structure of the molecular sieve to meet the needs of acidic catalytic reactions.
[0020] Other features and advantages of the present disclosure will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] The accompanying drawings are used to provide a further understanding of the present disclosure and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present disclosure but do not constitute a limitation of the present disclosure. In the accompanying drawings:
[0022] Figure 1 is the XRD spectrum of the heteroatom EWT structure molecular sieve 1 with a framework containing boron atoms prepared in Example 1 of the present disclosure;
[0023] Figure 2 This is a SEM picture of the heteroatom EWT structure molecular sieve 1 with a framework containing boron atoms prepared in Example 1 of the present disclosure;
[0024] Figure 3 The heteroatom EWT structure molecular sieve 1 with a framework containing boron atoms prepared in Example 1 of the present disclosure is 29 Si MAS NMR spectrum;
[0025] Figure 4 The heteroatom EWT structure molecular sieve 1 with a framework containing boron atoms prepared in Example 1 of the present disclosure is 27 Al MAS NMR spectrum;
[0026] Figure 5 The heteroatom EWT structure molecular sieve 1 with a framework containing boron atoms prepared in Example 1 of the present disclosure is 11 B MAS NMR spectrum;
[0027] Figure 6 is an isotherm curve diagram of the heteroatom EWT structure molecular sieve 1 with a framework containing boron atoms obtained in Example 1 of the present disclosure;
[0028] Figure 7 is the XRD spectrum of the heteroatom EWT structure molecular sieve 2 containing iron atoms in the framework prepared in Example 2 of the present disclosure;
[0029] Figure 8 is the XRD spectrum of the heteroatom EWT structure molecular sieve 3 containing titanium atoms in the framework prepared in Example 3 of the present disclosure;
[0030] Fig. 9 This is the XRD spectrum of the heteroatom EWT structured molecular sieve 4 containing gallium atoms in the framework prepared in Example 4 of the present disclosure. DETAILED DESCRIPTION
[0031] The specific implementation of the present disclosure is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described herein is only used to illustrate and explain the present disclosure, and is not used to limit the present disclosure.
[0032] The first aspect of the present disclosure provides a method for synthesizing ethylbenzene by alkylation of benzene and ethylene, the method comprising: contacting benzene with ethylene under alkylation reaction conditions and in the presence of a catalyst; wherein the catalyst is a heteroatom EWT structure molecular sieve, the framework of the heteroatom EWT structure molecular sieve contains silicon elements, aluminum elements and heteroatom elements, and the heteroatom EWT structure molecular sieve contains SiO 2 Silicon and Al 2 O 3 The molar ratio of aluminum element is more than 10, and the heteroatom EWT structure molecular sieve is SiO 2 The molar ratio of silicon element calculated as silicon element to heteroatom element calculated as heteroatom oxide is greater than 10; the heteroatom element includes one or more of boron, iron, titanium, gallium and germanium.
[0033] The method for synthesizing ethylbenzene by alkylation of benzene and ethylene provided in the present disclosure uses a heteroatom EWT structure molecular sieve containing aluminum atoms and heteroatoms on the skeleton as a catalyst. The heteroatom EWT structure molecular sieve has a 3D pore system composed of a 21-membered ring and a ten-membered ring, has a suitable acid center distribution, and can significantly improve the utilization rate of the acid center of the molecular sieve. In addition, the skeleton aluminum atoms of the molecular sieve can adjust the acid amount of the molecular sieve, and the skeleton heteroatoms can adjust the position and acid distribution of the skeleton aluminum, thereby making its acidity more suitable and the intracrystalline mesopores richer. When the heteroatom EWT structure molecular sieve is used for the alkylation reaction of benzene and ethylene, it exhibits optimized catalytic performance, can improve the ethylene conversion rate and ethylation selectivity, while reducing the xylene content, and can reduce the generation of by-products such as isopropylbenzene, reducing C 9 Component selectivity.
[0034] In one embodiment of the present disclosure, the alkylation reaction conditions include: temperature of 300-360°C, preferably 330-360°C; time of 10-400h, preferably 20-100h; pressure of 0.6-1.2MPa, preferably 0.8-1.0MPa; the feed molar ratio of benzene to ethylene is (4-8):1, preferably (6-7.5):1; preferably, the reaction is carried out in a fixed bed reactor, and the mass space velocity of ethylene is 0.5-10.0h-1 , preferably 5.0~8.0h -1 In the above embodiment, by selecting the preferred alkylation reaction conditions and feed ratio, it is beneficial for benzene and ethylene to fully react, and the ethylation selectivity is further improved.
[0035] In one embodiment of the present disclosure, the heteroatom EWT structured molecular sieve is composed of SiO 2 Silicon and Al 2 O 3 The molar ratio of aluminum element is 10 to 60, preferably 15 to 30; the heteroatom EWT structure molecular sieve is SiO 2 The molar ratio of silicon element calculated as silicon to heteroatom element calculated as heteroatom oxide is 10 to 250, preferably 120 to 240. In the above embodiment, by selecting the preferred silicon-aluminum ratio and silicon-heteroatom ratio, the acid distribution and acid strength of the molecular sieve can be further adjusted, thereby improving the catalytic activity of the molecular sieve.
[0036] In one embodiment of the present disclosure, when the heteroatom element is boron, the heteroatom EWT structure molecular sieve is SiO 2 Silicon and B 2 O 3 The molar ratio of boron to the heteroatom element is 120 to 180; when the heteroatom element is one or more of iron, titanium, gallium and germanium, the heteroatom EWT structure molecular sieve is SiO 2 The molar ratio of silicon element calculated as silicon element to heteroatom element calculated as heteroatom oxide is 150-240.
[0037] In one embodiment of the present disclosure, the total specific surface area of the heteroatom EWT structure molecular sieve is 300 to 650 cm 2 / g, preferably 450 to 580 cm 2 / g; total pore volume is 0.25~0.60cm 3 / g, preferably 0.25 to 0.45 cm 3 / g; the volume of mesopores with a pore size of 2.0 to 20.0 nm is 0.05 to 0.35 cm 3 / g, preferably 0.10 to 0.25 cm 3 / g; the percentage of the mesopore volume with a pore size of 2.0 to 20.0 nm to the total pore volume is 30 to 50%, preferably 35 to 50%; the average particle size of the heteroatom EWT structure molecular sieve is 0.2 to 1.5 μm, preferably 0.3 to 1.0 μm; the relative crystallinity is 50 to 100%, preferably 75 to 95%; the ratio of the amount of B acid to the amount of L acid measured by the pyridine adsorption infrared method at 350°C of the heteroatom EWT structure molecular sieve is 0.3 to 0.6. In a preferred embodiment, the heteroatom EWT structure molecular sieve is a hydrogen-type heteroatom EWT structure molecular sieve. In the above embodiment, the heteroatom EWT structure molecular sieve has a rich mesoporous structure, which is beneficial to catalyze the alkylation reaction of benzene and ethylene, and improve the ethylene conversion rate and ethylation selectivity; by selecting a molecular sieve with a preferred acid strength, it is beneficial to improve the catalytic activity and selectivity of the molecular sieve.
[0038] In one embodiment of the present disclosure, the method further comprises preparing the catalyst by the following steps:
[0039] (1) mixing a silicon source, a heteroatom element source, a first alkali source, a first organic template and water, and performing a first crystallization on the obtained first material to be crystallized to obtain a molecular sieve raw powder; and calcining the molecular sieve raw powder to obtain a sodium-type molecular sieve;
[0040] (2) performing ion exchange on the sodium molecular sieve using an acid solution, mixing the obtained molecular sieve intermediate with an aluminum source, a second alkali source and a second organic template, and performing a second crystallization on the obtained second material to be crystallized;
[0041] Wherein, the heteroatom element includes one or more of boron, iron, titanium, gallium and germanium; the first organic template and the second organic template are cyclic diquaternary ammonium base compounds and / or cyclic diquaternary ammonium salt compounds respectively; the temperature of the first crystallization is 60-180°C, preferably 100-170°C; the time is 96-168h, preferably 96-144h; the temperature of the second crystallization is 60-180°C, preferably 100-170°C; the time is 96-168h, preferably 96-144h. The cyclic diquaternary ammonium base compound refers to a ring-forming compound containing two quaternary ammonium bases, and the N atoms of the two quaternary ammonium bases are not directly connected; the cyclic diquaternary ammonium salt compound refers to a ring-forming compound containing two quaternary ammonium salts, and the N atoms of the two quaternary ammonium salts are not directly connected.
[0042] In the above embodiment, by adopting the secondary crystallization method of crystallization-decomposition-dissolution-recrystallization, firstly, the EWT structure molecular sieve containing silicon and heteroatoms is prepared, and then some of the framework heteroatoms are removed to form a silanol nest, providing vacancies to facilitate Al atoms to enter the framework to complete isomorphous substitution, so as to prepare a molecular sieve with a lower silicon-aluminum ratio, improve the acidity of the molecular sieve, and meet the needs of acidic catalytic reactions. The method disclosed in the present invention can not only synthesize a super-large pore structure molecular sieve with a 3D pore system composed of 21-membered rings and ten-membered rings, but also generate a large number of mesopores with larger pore sizes, effectively improving the pore structure of the molecular sieve, so that larger aluminum atoms and heteroatom elements can be introduced into the molecular sieve framework, so as to optimize the acid distribution and acid strength of the molecular sieve, and obtain higher ethylene conversion rate and ethylation selectivity.
[0043] In one embodiment of the present disclosure, the silicon source is selected from one or more of silica sol, water glass, solid silica gel, tetraethyl orthosilicate and white carbon black, preferably solid silica gel; the heteroatom element source is selected from one or more of boron oxide, boric acid, iron oxide, titanium oxide, gallium oxide and germanium oxide, preferably boron oxide and / or boric acid; the first alkali source and the second alkali source are respectively selected from one or more of sodium hydroxide, potassium hydroxide and lithium hydroxide, preferably, the first alkali source and the second alkali source are both sodium hydroxide; the aluminum source is selected from one or more of aluminum chloride, aluminum sulfate, hydrated aluminum oxide, sodium aluminate and aluminum sol, preferably sodium aluminate.
[0044] In one embodiment of the present disclosure, the first organic template and the second organic template are respectively selected from at least one of the structures shown in formula (1): Where R 1 , R 2 , R 3 and R 4 are independently selected from alkyl groups having 1 to 4 carbon atoms, preferably, R 1 , R 2 , R 3 and R 4 Each is independently selected from one or more of methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl and tert-butyl, preferably methyl or ethyl; m is 2 or 3; n is any integer from 1 to 10; X - Including hydroxide ions or halogen anions.
[0045] In one embodiment of the present disclosure, the silicon source is SiO 2 The heteroatom element source is calculated as heteroatom oxides. When the heteroatom element is boron, the SiO 2 With B 2 O 3The molar ratio of SiO in the first material to be crystallized is 10 to 250, preferably 30 to 120; when the heteroatom element is one or more of iron, titanium, gallium and germanium, the molar ratio of SiO in the first material to be crystallized is 10 to 250, preferably 30 to 120; 2 The molar ratio of the heteroatom oxide to the heteroatom oxide is 10-250, preferably 30-150.
[0046] In one embodiment of the present disclosure, in step (1), the silicon source is SiO 2 The heteroatom element source is calculated as heteroatom oxide, and the first organic template is calculated as T 1 It means that when the heteroatom element in the first material to be crystallized is boron, SiO 2 With B 2 O 3 The molar ratio of SiO is 10 to 250, preferably 30 to 120; when the heteroatom element is one or more of iron, titanium, gallium and germanium, SiO 2 The molar ratio of OH to heteroatom oxide is 10 to 250, preferably 30 to 150; - The first alkali source and SiO 2 The molar ratio of T is 0.2 to 1.0, preferably 0.2 to 0.5; 1 With SiO 2 The molar ratio of H is 0.02 to 0.5, preferably 0.08 to 0.15; 2 O and SiO 2 The molar ratio of is 5 to 20, preferably 5 to 10; in step (2), the aluminum source is Al 2 O 3 The second organic template is T 2 Indicates that the SiO 2 With Al 2 O 3 The molar ratio of OH is 10 or more, preferably 10 to 60, more preferably 15 to 30; - The second alkali source and SiO 2 The molar ratio of T is 0.2 to 1.0, preferably 0.2 to 0.5; 2 With SiO 2 The molar ratio of H is 0.02 to 0.5, preferably 0.08 to 0.15; 2 O and SiO 2 The molar ratio is 5-20, preferably 5-10.
[0047] In one embodiment of the present disclosure, in step (1), the calcination temperature is 400-650°C, and the time is 1-7h; in step (2), the weight ratio of the acid solution to the sodium molecular sieve is (1-100):1, the concentration of the acid solution is 0.01-0.10 mol / L, the ion exchange temperature is 60-90°C, and the time is 2-24h; the acid solution is selected from one or more of hydrochloric acid solution, nitric acid solution and sulfuric acid solution.
[0048] The present disclosure is further illustrated below by way of examples, but the present disclosure is not limited thereby.
[0049] Example 1
[0050] (1) Add an aqueous solution containing 0.01425 mol of a first organic template into the polytetrafluoroethylene liner (the first organic template is denoted as T 1 , the structure is Where m = 2, n = 3, R 1 , R 2 , R 3 and R 4 All are methyl, T 1 The molar mass is 248 g / mol, the mass fraction is 25.74%, and X - Br - ) and 0.0032 mol of boric acid; then add 0.02 mol of sodium hydroxide (first alkali source) and 0.051 mol of water, and finally add 0.095 mol of coarse block solid silica gel (silicon source), stir evenly, and obtain a first material to be crystallized, wherein SiO 2 With B 2 O 3 The molar ratio is 30, with OH - The first alkali source and SiO 2 The molar ratio is 0.21, T 1 With SiO 2 The molar ratio of H 2 O and SiO 2 The molar ratio is 6.5; the polytetrafluoroethylene lined gland is sealed, placed in a stainless steel crystallization kettle, placed in a rotary oven, the crystallization temperature program is set, and the first crystallization is started at a temperature of 160°C and a time of 144h. After the first crystallization is completed, the crystallization kettle is cooled to room temperature, the crystallization kettle is opened, the product is washed and filtered with deionized water, and finally dried in an oven at 80°C for 12h. The obtained molecular sieve raw powder is placed in a muffle furnace at 550°C for 5h to remove the first organic template, and a sodium molecular sieve with a boron skeleton is obtained.
[0051] (2) Using hydrochloric acid solution to carry out ion exchange on sodium molecular sieve, specifically: mixing hydrochloric acid solution and sodium molecular sieve at a weight ratio of 40:1, heating to 80°C under stirring and reflux conditions, maintaining for 12 hours (i.e., the ion exchange temperature is 80°C and the time is 12 hours), washing, filtering and drying to obtain a molecular sieve intermediate; wherein the concentration of the hydrochloric acid solution is 0.03 mol / L. Adding an aqueous solution containing 0.01425 mol of a second organic template (the second organic template is denoted as T 2 , T 2 Structure and T 1 Same, T 2 The molar mass is 248 g / mol, the mass fraction is 25.74%), 3.41 mL sodium aluminate (aluminum source, which contains 101.5 g / L of aluminum oxide, 194 g / L of sodium hydroxide, 150.35 g / L of sodium oxide, a specific gravity of 1.227 g / mL, and a mass fraction of 20.50% aqueous solution), 0.02 mol of sodium hydroxide (a second alkali source) and 0.198 mol of water, and then the molecular sieve intermediate is added, and the obtained second material to be crystallized is stirred uniformly, wherein SiO 2 With Al 2 O 3 The molar ratio of sodium aluminate is 28, and the molar ratio of OH is 28. - The second alkali source and SiO 2 The molar ratio is 0.384, T 2 With SiO 2 The molar ratio of H 2 O and SiO 2 The molar ratio is 10; finally, the polytetrafluoroethylene lined pressure cover is sealed, placed in a stainless steel crystallization kettle, and placed in a rotary oven for a second crystallization. The temperature of the second crystallization is 160°C and the time is 144h to obtain a heteroatom EWT structure molecular sieve 1 containing aluminum atoms and boron atoms in the framework, that is, catalyst 1, recorded as C1.
[0052] The XRD spectrum of the prepared catalyst C1 is shown in Figure 1 As shown in the SEM images Figure 2 As shown, 29 Si MAS NMR spectrum is shown in Figure 3 As shown, 27 Al MAS NMR spectrum is shown in Figure 4 As shown, 11 B MAS NMR spectrum Figure 5 As shown, the isotherm curve is Figure 6 shown.
[0053] Among them, from Figure 1It can be seen that the XRD spectrum of C1 has peaks near 2q=5.1, 8.2, and 8.9°, indicating that catalyst C1 is an EWT structure molecular sieve with a relative crystallinity of 79%. Figure 2 It can be seen that the average particle size of C1 is 0.4-0.8 μm; Figure 3 It can be seen that the silicon element in C1 appears in the form of Si-Al or Si-B coordination, indicating that the boron element enters the molecular sieve framework; Figure 4 It can be seen that the aluminum element in C1 exists in a four-coordinated form; Figure 5 It can be seen that part of the boron element in C1 exists in a tetracoordinate form; Figure 6 It can be seen that C1 has a super-large pore structure.
[0054] Example 2
[0055] The same as Example 1, the only difference is that iron oxide is used instead of boric acid, and SiO 2 with Fe 2 O 3 The molar ratio of SiO in the second crystallization material is 50, the temperature of the first crystallization is 160°C, and the time is 96h; 2 With Al 2 O 3 The molar ratio of sodium aluminate is 25, the temperature of the second crystallization is 165°C, and the time is 120 h, to obtain a heteroatom EWT structure molecular sieve 2 containing aluminum atoms and iron atoms in the framework, namely catalyst 2, recorded as C2.
[0056] The XRD spectrum of the prepared catalyst C2 is as follows: Figure 7 As shown, the XRD spectrum of C2 has peaks near 2q=5.20, 9.00, and 10.39°, indicating that catalyst C2 is an EWT structure molecular sieve with a relative crystallinity of 70%.
[0057] Example 3
[0058] The same as Example 1, the only difference is that titanium oxide is used instead of boric acid, and SiO 2 With TiO 2 The molar ratio of SiO in the second crystallization material is 60, the temperature of the first crystallization is 140°C, and the time is 144h; 2 With Al 2 O 3 The molar ratio of sodium aluminate is 20, the temperature of the second crystallization is 170°C, and the time is 96 hours, to obtain a heteroatom EWT structure molecular sieve 3 containing aluminum atoms and titanium atoms in the framework, namely catalyst 3, recorded as C3.
[0059] The XRD spectrum of the prepared catalyst C3 is as follows: Figure 8As shown, the XRD spectrum of C3 has peaks near 2q=5.20, 9.00, and 10.39°, indicating that catalyst C3 is an EWT structure molecular sieve with a relative crystallinity of 64%.
[0060] Example 4
[0061] The same as Example 1, the only difference is that gallium oxide is used instead of boric acid, and SiO 2 with Ga 2 O 3 The molar ratio of SiO in the second crystallization material is 80, the temperature of the first crystallization is 140°C, and the time is 140h; 2 With Al 2 O 3 The molar ratio of sodium aluminate is 20, the temperature of the second crystallization is 165°C, and the time is 96 hours, to obtain a heteroatom EWT structure molecular sieve 4 containing aluminum atoms and gallium atoms in the framework, namely catalyst 4, recorded as C4.
[0062] The XRD spectrum of the prepared catalyst C4 is as follows: Fig. 9 As shown, the XRD spectrum of C4 has peaks near 2q=5.20, 9.00, and 10.39°, indicating that catalyst C4 is an EWT structure molecular sieve with a relative crystallinity of 72%.
[0063] Example 5
[0064] The same as Example 1, the only difference is that germanium oxide is used instead of boric acid, and SiO 2 With GeO 2 The molar ratio of SiO2 in the second crystallization material is 100, the temperature of the first crystallization is 140°C, and the time is 100h; 2 With Al 2 O 3 The molar ratio of sodium aluminate was 15, the temperature of the second crystallization was 165°C, and the time was 96 hours, to obtain a heteroatom EWT structure molecular sieve 5 containing aluminum atoms and germanium atoms in the framework, namely catalyst 5, recorded as C5.
[0065] Example 6
[0066] The same as Example 1, except that: the SiO 2 With B 2 O 3 The molar ratio of SiO in the second material to be crystallized is 60. 2 With Al 2 O 3 The molar ratio of sodium aluminate is 30, and a heteroatom EWT structure molecular sieve 6 with a framework containing aluminum atoms and boron atoms is obtained, namely catalyst 6, which is recorded as C6.
[0067] Example 7
[0068] The same as Example 1, the only difference is that: in step (1), the temperature of the first crystallization is 150°C and the time is 148h. After the first crystallization is completed, wait for the crystallization kettle to cool to room temperature, open the crystallization kettle, wash and filter the product with deionized water, and finally dry it in an oven at 120°C for 24h. The obtained molecular sieve raw powder is placed in a muffle furnace and calcined at 580°C for 10h to remove the template agent to obtain a sodium type molecular sieve; in step (2), the temperature of the second crystallization is 170°C and the time is 96h, and a heteroatom EWT structure molecular sieve 7 with a framework containing aluminum atoms and boron atoms is obtained, that is, catalyst 7, recorded as C7.
[0069] Comparative Example 1
[0070] (1) Sodium hydroxide (alkali source), sodium aluminate (aluminum source), and a structure as shown in formula (1) ( m=2,n=4,R 1 , R 2 , R 3 and R 4 All are methyl, X - Br - ) is dissolved in water and mixed evenly to form a solution; solid silica gel (silicon source) is added to the solution and mixed evenly to form a gel-like crystallization material. The molar ratio of each material in the crystallization material is: n(SiO 2 ) / n(Al 2 O 3 )=90、n(T) / n(SiO 2 )=0.15、n(OH - ) / n(SiO 2 )=0.38、n(H 2 O) / n(SiO 2 )=7.3, wherein T is an organic template;
[0071] (2) The gel-like material to be crystallized is subjected to a first stage crystallization reaction under autogenous pressure, the temperature of the first stage crystallization is 120°C, the time is 24 hours, and then the temperature is raised to 160°C, and the second stage crystallization reaction is carried out under autogenous pressure for 120 hours. The material after the second stage crystallization is filtered, washed and dried, and then ammonium exchange is carried out with an ammonium salt solution. The exchanged material is filtered, dried, and calcined at 550°C for 4 hours to obtain a hydrogen-type EWT structure molecular sieve, which is comparative catalyst 1, denoted as D1.
[0072] Comparative Example 2
[0073] Take n(SiO 2 ) / n(Al 2 O3 )=40 ZSM-5 molecular sieve (purchased from Sinopec Changling Catalyst Plant) was exchanged with ammonium salt. The exchanged material was filtered and dried, and then calcined at 550°C for 4h to obtain hydrogen-type ZSM-5 molecular sieve, which is comparative catalyst 2, denoted as D2.
[0074] Reaction Example 1
[0075] 2 g of C1 was loaded as a catalyst in a continuous flow pressurized fixed bed reactor, and benzene and ethylene were added as reaction raw materials. The reaction conditions were: temperature 360 °C, pressure 0.8 MPa, mass space velocity of ethylene 7.0 h -1 The reaction operation time was 24h, the feed molar ratio of benzene to ethylene was 7.5:1, and the evaluation results are shown in Table 3.
[0076] Reaction Examples 2 to 9
[0077] The same as reaction example 1, the only difference is: C2~C7, D1~D2 are used instead of C1 respectively. The evaluation results are shown in Table 3.
[0078] Test Case
[0079] In the embodiments and comparative examples of the present disclosure, a Quanta 200F scanning electron microscope (SEM) produced by FEI Company was used for microscopic morphology analysis, and the operating voltage of the SEM was 20 kV; a Japan Hitachi S-4800 type instrument was used to test the average particle size of the catalyst.
[0080] The crystallinity of the molecular sieve is determined by the RIPP 146-90 standard method. The RIPP standard method mentioned here can be found in "Petrochemical Analysis Methods", edited by Yang Cuiding et al., 1990 edition.
[0081] The chemical composition of the molecular sieve was determined by using a 3013 X-ray fluorescence spectrometer produced by Rigaku Corporation of Japan, and the silicon-aluminum ratio and silicon-heteroatom ratio of the molecular sieve were calculated. The target was tungsten, the excitation voltage was 40 kV, and the excitation current was 50 mA.
[0082] The total specific surface area and total pore volume were measured by nitrogen adsorption BET specific surface area method using AS-3 and AS-6 static nitrogen adsorption instruments produced by Quantachrome Instruments. The specific method is as follows: the sample is placed in a sample treatment system and vacuumed to 1.33×10 -2 Pa, keep the temperature and pressure for 4 hours, purify the sample; test the purified sample at different pressure ratios P / P at a liquid nitrogen temperature of -196°C 0 The adsorption and desorption of nitrogen under the conditions were obtained. 2Adsorption-desorption isotherm curve, and then use the two-parameter BET formula to calculate the total specific surface area, taking the specific pressure P / P 0 = 0.98 or less is the total pore volume of the sample.
[0083] The total acid content is NH 3 The measurement was carried out by the AutochemⅡ2920 programmed temperature desorption instrument of Micromeritics, USA. The specific method was as follows: 0.2 g of the sample to be tested was weighed and loaded into a sample tube, which was placed in a thermal conductivity cell heating furnace. He gas was used as the carrier gas (50 mL / min), and the temperature was raised to 600°C at a rate of 20°C / min. The impurities adsorbed on the catalyst surface were purged for 60 min, and then the temperature was lowered to 100°C, kept constant for 30 min, and switched to NH 3 -He mixed gas (10.02% NH 3 +89.98% He) adsorption for 30 minutes, and then continue to purge with He gas for 90 minutes until the baseline is stable to desorb the physically adsorbed ammonia; the temperature is increased to 600°C at a heating rate of 10°C / min for desorption, and maintained for 30 minutes, and the desorption is completed; a TCD detector is used to detect the change of gas components, and the instrument automatically integrates the total acid content.
[0084] The acid content of B acid and L acid was measured by 2,6-di-tert-butylpyridine adsorption infrared acid method using a Vertex 70 instrument produced by Bruker Instruments. The specific method is as follows: the catalyst is pressed into a 10 mg / cm 2 The slice was placed in a CaF 2 In the infrared cell of the window, first evacuate at 400°C, then reduce to 150°C to adsorb 2,6-di-tert-butylpyridine for 15 minutes, then evacuate for 1 hour, reduce to room temperature to collect spectra, and calculate the acid amount of B acid and the acid amount of L acid. See Applied Catalysis A: General, 294, 2005: 92.
[0085] The ethylene conversion rate, xylene content, and C 9 / C 10 The test method for component selectivity and ethylation selectivity is as follows: the carrier gas is nitrogen, the detector is FID, the column temperature is 80°C, the injector temperature is 260°C, and the detector temperature is 250°C. The initial temperature of the program temperature rise is 0°C, the holding time is 0min, and the heating rate is 3°C / min; the final temperature is 50°C, and the holding time is 20min. The injection volume is 0.2μL.
[0086] In each reaction example:
[0087]
[0088]
[0089]
[0090]
[0091]
[0092]
[0093] Ethylation selectivity = ethylbenzene selectivity + diethylbenzene selectivity
[0094] Table 1
[0095]
[0096] Table 2
[0097]
[0098] Table 3
[0099]
[0100] From the results in Tables 1 to 3 above, it can be seen that the framework of the heteroatom EWT structured molecular sieve provided by the present disclosure contains aluminum atoms and heteroatom elements, which makes the molecular sieve have suitable acidity and acid strength, and the 3D pore system composed of the 21-membered ring and the ten-membered ring of the heteroatom EWT structured molecular sieve can improve the utilization rate of the acid center, improve the activity and stability of the catalyst, and enable it to be used as a catalyst for the alkylation reaction of benzene and ethylene, It can maintain a high ethylation selectivity, a low xylene content and C 9 The component selectivity was high and the continuous operation was 300h. When the comparative example 1 used the EWT structure molecular sieve without heteroatoms in the skeleton as the catalyst for the alkylation reaction of benzene and ethylene, the ethylation selectivity was low and the xylene content was high, which made it difficult to separate ethylbenzene from xylene, and the product quality of ethylbenzene was affected. When the comparative example 2 used the ten-membered ring ZSM-5 molecular sieve as the catalyst, the ethylation selectivity was low and there were more side reactions. The xylene content and C 9 The component selectivity is high. Therefore, the heteroatom EWT structure molecular sieves provided in Examples 1 to 7 of the present disclosure have better performance than the molecular sieves provided in Comparative Examples 1 to 2.
[0101] The preferred embodiments of the present disclosure are described in detail above in conjunction with the accompanying drawings; however, the present disclosure is not limited to the specific details in the above embodiments. Within the technical concept of the present disclosure, a variety of simple modifications can be made to the technical solution of the present disclosure, and these simple modifications all fall within the protection scope of the present disclosure.
[0102] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present disclosure will not further describe various possible combinations.
[0103] In addition, various embodiments of the present disclosure may be arbitrarily combined, and as long as they do not violate the concept of the present disclosure, they should also be regarded as the contents disclosed by the present disclosure.
Claims
1. A method for synthesizing ethylbenzene by alkylation of benzene and ethylene, characterized in that: The method comprises: contacting benzene with ethylene under alkylation reaction conditions and in the presence of a catalyst; wherein the catalyst is a heteroatom EWT structure molecular sieve, the skeleton of the heteroatom EWT structure molecular sieve comprises silicon element, aluminum element and heteroatom element, the molar ratio of silicon element calculated as SiO2 to aluminum element calculated as Al2O3 in the heteroatom EWT structure molecular sieve is greater than 10, the molar ratio of silicon element calculated as SiO2 to heteroatom element calculated as heteroatom oxide in the heteroatom EWT structure molecular sieve is greater than 10; the heteroatom element comprises one or more of boron, iron, titanium, gallium and germanium.
2. The method according to claim 1, characterized in that The alkylation reaction conditions include: temperature of 300-360° C., preferably 330-360° C.; time of 10-400 h, preferably 20-100 h; pressure of 0.6-1.2 MPa, preferably 0.8-1.0 MPa; the feed molar ratio of benzene to ethylene is (4-8):1, preferably (6-7.5):1; Preferably, the reaction is carried out in a fixed bed reactor, and the mass space velocity of ethylene is 0.5 to 10.0 h -1 , preferably 5.0~8.0h -1 .
3. The method according to claim 1, characterized in that The molar ratio of silicon element calculated as SiO2 to aluminum element calculated as Al2O3 in the heteroatom EWT structured molecular sieve is 10 to 60, preferably 15 to 30; the molar ratio of silicon element calculated as SiO2 to heteroatom elements calculated as heteroatom oxides in the heteroatom EWT structured molecular sieve is 10 to 250, preferably 120 to 240.
4. The method according to claim 1, characterized in that: When the heteroatom element is boron, the molar ratio of silicon element calculated as SiO2 to boron element calculated as B2O3 in the heteroatom EWT structured molecular sieve is 120 to 180; When the heteroatom element is one or more of iron, titanium, gallium and germanium, the molar ratio of silicon element calculated as SiO2 to the heteroatom element calculated as heteroatom oxide in the heteroatom EWT structure molecular sieve is 150-240.
5. The method according to claim 1, characterized in that The total specific surface area of the heteroatom EWT structure molecular sieve is 300 to 650 cm 2 / g, preferably 450 to 580 cm 2 / g; total pore volume is 0.25~0.60cm 3 / g, preferably 0.25 to 0.45 cm 3 / g; the volume of mesopores with a pore size of 2.0 to 20.0 nm is 0.05 to 0.35 cm 3 / g, preferably 0.10 to 0.25 cm 3 / g; the percentage of the mesopore volume with a pore size of 2.0 to 20.0 nm to the total pore volume is 30 to 50%, preferably 35 to 50%; the average particle size of the heteroatom EWT structure molecular sieve is 0.2 to 1.5 μm, preferably 0.3 to 1.0 μm; the relative crystallinity is 50 to 100%, preferably 75 to 95%; the ratio of the B acid amount to the L acid amount of the heteroatom EWT structure molecular sieve measured by pyridine adsorption infrared method at 350°C is 0.3 to 0.6; Preferably, the heteroatom EWT structure molecular sieve is a hydrogen-type heteroatom EWT structure molecular sieve.
6. The method according to claim 1, characterized in that The method further comprises preparing the catalyst by the following steps: (1) mixing a silicon source, a heteroatom element source, a first alkali source, a first organic template and water, and performing a first crystallization on the obtained first material to be crystallized to obtain a molecular sieve raw powder; and calcining the molecular sieve raw powder to obtain a sodium-type molecular sieve; (2) performing ion exchange on the sodium molecular sieve using an acid solution, mixing the obtained molecular sieve intermediate with an aluminum source, a second alkali source and a second organic template, and performing a second crystallization on the obtained second material to be crystallized; Wherein, the heteroatom element includes one or more of boron, iron, titanium, gallium and germanium, the first organic template and the second organic template are respectively a cyclic diquaternary ammonium base compound and / or a cyclic diquaternary ammonium salt compound; the temperature of the first crystallization is 60-180°C, preferably 100-170°C; the time is 96-168h, preferably 96-144h; the temperature of the second crystallization is 60-180°C, preferably 100-170°C; the time is 96-168h, preferably 96-144h.
7. The method according to claim 6, characterized in that The silicon source is selected from one or more of silica sol, water glass, solid silica gel, ethyl orthosilicate and white carbon black, preferably solid silica gel; The heteroatom element source is selected from one or more of boron oxide, boric acid, iron oxide, titanium oxide, gallium oxide and germanium oxide, preferably boron oxide and / or boric acid; The first alkali source and the second alkali source are respectively selected from one or more of sodium hydroxide, potassium hydroxide and lithium hydroxide. Preferably, the first alkali source and the second alkali source are both sodium hydroxide; The aluminum source is selected from one or more of aluminum chloride, aluminum sulfate, hydrated aluminum oxide, sodium aluminate and aluminum sol, preferably sodium aluminate; The first organic template and the second organic template are respectively selected from at least one of the structures shown in formula (1): wherein R1, R2, R3 and R4 are each independently selected from an alkyl group having 1 to 4 carbon atoms, preferably, R1, R2, R3 and R4 are each independently selected from one or more of methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl and tert-butyl, preferably methyl or ethyl; m is 2 or 3; n is any integer from 1 to 10; X - Including hydroxide ions or halogen anions.
8. The method according to claim 6, characterized in that The silicon source is calculated as SiO2, the heteroatom element source is calculated as heteroatom oxide, and when the heteroatom element is boron, the molar ratio of SiO2 to B2O3 in the first material to be crystallized is 10 to 250, preferably 30 to 120; When the heteroatom element is one or more of iron, titanium, gallium and germanium, the molar ratio of SiO2 to the heteroatom oxide in the first material to be crystallized is 10-250, preferably 30-150.
9. The method according to claim 6, characterized in that In step (1), the silicon source is represented by SiO2, the heteroatom element source is represented by heteroatom oxide, the first organic template is represented by T1, when the heteroatom element in the first material to be crystallized is boron, the molar ratio of SiO2 to B2O3 is 10 to 250, preferably 30 to 120; when the heteroatom element is one or more of iron, titanium, gallium and germanium, the molar ratio of SiO2 to heteroatom oxide is 10 to 250, preferably 30 to 150; when OH is used as - The molar ratio of the first alkali source to SiO2 is 0.2 to 1.0, preferably 0.2 to 0.5; the molar ratio of T1 to SiO2 is 0.02 to 0.5, preferably 0.08 to 0.15; the molar ratio of H2O to SiO2 is 5 to 20, preferably 5 to 10; In step (2), the aluminum source is represented by Al2O3, the second organic template is represented by T2, the molar ratio of SiO2 to Al2O3 in the second material to be crystallized is greater than 10, preferably 10 to 60, more preferably 15 to 30; - The molar ratio of the second alkali source to SiO2 is 0.2-1.0, preferably 0.2-0.5; the molar ratio of T2 to SiO2 is 0.02-0.5, preferably 0.08-0.15; the molar ratio of H2O to SiO2 is 5-20, preferably 5-10.
10. The method according to claim 6, characterized in that In step (1), the calcination temperature is 400-650° C. and the calcination time is 1-7 hours; In step (2), the weight ratio of the acid solution to the sodium molecular sieve is (1-100):1, the concentration of the acid solution is 0.01-0.10 mol / L, the temperature of the ion exchange is 60-90°C, and the time is 2-24h; the acid solution is selected from one or more of hydrochloric acid solution, nitric acid solution and sulfuric acid solution.