Recovery method of polyester-based blended fabric

Through the depolymerization liquid system of sulfolane, alcohol and strong alkali, the complex and environmentally friendly problems of separation and purification in the recycling of polyester-based blended textiles are solved, and efficient, selective depolymerization and high purity recycling are achieved, ensuring the non-polyester components Complete recycling, providing economically viable recycling solutions.

CN119059896AInactive Publication Date: 2024-12-03DONGHUA UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411555299.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-04
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The prior art has difficulties in the recycling of polyester-based blended textiles, such as complex separation and purification, low yield of target products, poor quality of recycling monomers, and high waste waste treatment rate, and the co-solvent system is damaged to the cotton and ammonia components. It is difficult to achieve selective degradation and environmentally friendly large-scale recycling.

Method used

Depolymerization of polyester-based blended textiles is performed by using a depolymerization solution composed of sulfolane, alcohol and strong alkali. Through hydrogen bond competition and the action of alkoxide, the ester bonds are selectively broken to form high-purity terephthalic acid or lactic acid, and combined with Acidification treatment enables efficient separation and recycling.

Benefits of technology

The selective depolymerization and full recovery of polyester-based blended textiles are achieved, ensuring complete recycling of non-polyester components, with yields up to 90~99%, purity up to 95~99%, and sulfolane is an environmentally friendly material, reducing treatment Waste products and waste phenomena.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119059896A_ABST
    Figure CN119059896A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of fabric recovery, and relates to a polyester-based blended fabric recovery method which specifically comprises the following steps: adding a polyester-based blended fabric into a depolymerization solution consisting of sulfolane, alcohol and strong alkali for depolymerization, separating liquid and solid after depolymerization, and treating, when polyester in the polyester-based blended fabric is PET (Polyethylene Terephthalate), PBT (Polybutylene Terephthalate) or PBAT (Poly Butylene Terephthalate), the treatment process comprises the following steps: adding deionized water into the solid, filtering again to obtain filtrate, adjusting the pH value of the filtrate with acid until precipitate is separated out, and collecting the precipitate to obtain rPTA; when the polyester in the polyester-based blended fabric is PLA, the treatment process comprises the following steps: carrying out reduced pressure distillation on the liquid, and collecting distillate to obtain lactic acid. According to the method, the environment-friendly sulfolane with stable property is used as the cosolvent, and forms a cosolvent system with the alcohol and the strong base, so that high-selectivity depolymerization separation of the polyester-based blended fabric can be realized, the other component can be completely recovered, and full-amount recovery and reutilization can be realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of fabric recycling, and in particular relates to a method for recycling polyester-based blended fabrics. Background Art

[0002] Recycling waste polyester-based blended fabrics (mainly composed of more than 65wt% polyester components, such as polyester-ammonia, polyester-cotton, etc.) not only saves resources and reduces dependence on fossil fuels such as oil, but also greatly reduces environmental pollution. At the same time, the recycling of waste polyester-based blended fabrics has also brought significant economic benefits to related companies and effectively reduced production costs.

[0003] At present, there are many difficulties in the chemical recycling process of waste polyester-based blended fabrics, such as complex separation and purification, low yield of target products, poor quality of recycled monomers, and high waste treatment and production rate. Based on the dual goals of full recovery and environmental protection, researchers have designed an innovative green co-solvent system. The system is composed of alcohol and polar co-solvents, and aims to efficiently and selectively depolymerize and separate various polyester-based blended fabrics such as polyester-ammonia, polyester-cotton, and polyester-nylon through a one-pot process, thereby obtaining high-purity recycled terephthalic acid (rPTA). The reaction equation of the polyester depolymerization process is as follows: Figure 1 As shown (taking EG and KOH as examples).

[0004] The document (Cosolvent-promoted selective non-aqueous hydrolysis of PET wastes and facile product separation [J]. Green Chemistry, 2022, 24(8): 3284-92.) discloses a THF / EG co-solvent system, but the co-solvent system can only separate polyester-ammonia and polyester-cotton blends, and the co-solvent THF in the co-solvent system is highly toxic and has varying degrees of damage to the cotton and ammonia components in the blends (i.e., no selective degradation). These shortcomings limit its application. Subsequently, the document (Selective depolymerization of PET tomonomers from its waste blends and composites at ambient temperature [J]. Chemical Engineering Journal, 2023, 470. 144032.) discloses a DCM / EtOH co-solvent system for recycling polyester-based blended fabrics. Although the separation of polyester-based blended fabrics can be achieved, due to the low boiling point (39.8°C), instability and environmentally unfriendly characteristics of DCM, it is difficult to adapt to the needs of large-scale waste textile recycling.

[0005] Therefore, it is particularly necessary to propose a recycling method that can selectively degrade the components of waste polyester-based blended fabrics and has environmentally friendly properties. Summary of the invention

[0006] The purpose of the invention is to solve the problems existing in the prior art and provide a method for recycling polyester-based blended fabrics.

[0007] To achieve the above object, the technical solution adopted by the present invention is as follows:

[0008] A method for recovering a polyester-based blended fabric comprises adding the polyester-based blended fabric into a depolymerization liquid composed of cyclopentane, alcohol and a strong base for depolymerization, separating the liquid and the solid after depolymerization, and treating the same. When the polyester in the polyester-based blended fabric is PET, PBT or PBAT, the treatment process comprises: adding deionized water to the solid and filtering it again to obtain a filtrate, adjusting the pH value of the filtrate with an acid until a precipitate is precipitated, collecting the precipitate, and obtaining rPTA; when the polyester in the polyester-based blended fabric is PLA, the treatment process comprises: performing reduced pressure distillation on the liquid, collecting the distillate, and obtaining lactic acid.

[0009] As the preferred technical solution:

[0010] A method for recycling a polyester-based blended fabric as described above, wherein the polyester-based blended fabric is a polyester-spandex blended fabric, a polyester-cotton blended fabric, a polyester-nylon blended fabric, a PBT / cotton blended fabric, a PLA / cotton blended fabric or a PBAT / cotton blended fabric, and the polyester content is above 65wt%.

[0011] In the above-mentioned method for recycling a polyester-based blended fabric, the alcohol is ethylene glycol (EG), propylene glycol, butylene glycol or hexylene glycol; and the strong base is sodium hydroxide or potassium hydroxide.

[0012] In the above-mentioned method for recovering a polyester-based blended fabric, the volume ratio of sulfolane to alcohol is 30:70-70:30; the concentration of the strong alkali in the depolymerization solution is 0.04-0.07 g / mL; and the mass ratio of the polyester-based blended fabric to the depolymerization solution is 1:20-40.

[0013] The method for recovering a polyester-based blended fabric as described above comprises adding the polyester-based blended fabric into a depolymerization solution formed by sulfolane, alcohol and a strong base for depolymerization, wherein the depolymerization solution formed by sulfolane, alcohol and a strong base is heated to 50-90°C at a heating rate of 1-5°C / min, adding the polyester-based blended fabric thereto, and keeping the temperature for 30-90 minutes under magnetic stirring.

[0014] In the above-mentioned method for recovering a polyester-based blended fabric, the purity of rPTA or lactic acid is 95-99%, and the yield of rPTA or lactic acid is 90-99%.

[0015] In the above-mentioned method for recycling a polyester-based blended fabric, the recovery rate of components other than polyester in the polyester-based blended fabric is 97-99%.

[0016] Principle of the invention:

[0017] The depolymerization liquid of the present invention is composed of sulfolane, alcohol and strong base. The depolymerization process is as follows: Figure 3 As shown (taking polyester as PET as an example), first, the sulfur-oxygen double bond of cyclopentane sulfone provides a hydrogen bond acceptor, competing with the hydroxide ion of the strong base and forming a hydrogen bond with the alcohol. At the same time, during the depolymerization process, the alcohol and the strong base form an alcohol salt to attack the carboxyl bond in the polyester ester group, causing it to break the chain to form di(2-hydroxyethyl) terephthalate. Then the strong base acts as a strong nucleophile to directly attack the ester group to generate terephthalate, and finally the monomer terephthalic acid is obtained after acidification.

[0018] The sulfur-oxygen double bond of sulfolane competes with the hydroxide ion of the strong base and forms hydrogen bonds with the alcohol. On the one hand, it can weaken the solvation degree of the strong base (the strong base is a strong hydrogen bond acceptor, and its solvation strength in the hydrogen bond donor solvent is stronger. As the solvation degree increases, its reaction activity decreases, which is not conducive to depolymerization). On the other hand, it forms hydrogen bonds with alcohol to activate the alcohol and make it easier to attack the ester group of the polyester. The hydrogen bond formed by the sulfur-oxygen double bond and the alcohol is stronger than the hydrogen bond formed by the strong base and the alcohol, and the reaction potential energy is lower, which can make the depolymerization reaction easier.

[0019] In addition, the sulfur-oxygen double bond of sulfolane acts on the surface of polyester, breaking some chemical bonds (ester groups) on the surface of polyester, and breaking long chains into short chains or small molecular products, such as Figure 4 As shown in the figure, the polyester (taking PET as an example) treated with cyclopentane becomes rough on the surface, forming notches or grooves, thereby increasing the contact area between the polyester and the solvent, promoting interfacial mass transfer, being more conducive to the reaction, and accelerating the depolymerization reaction rate to a certain extent.

[0020] More importantly, the sulfolane used in the present invention can selectively depolymerize the ester bonds (i.e., only the ester bonds in the polymer are broken without affecting other types of chemical bonds), on the one hand because the electron cloud density of sulfolane is relatively high, and on the other hand because the ring structure of sulfolane has a steric effect, which enables sulfolane to form a stable compound with the carboxylic acid ester bond structure in the polyester through hydrogen bonds without affecting the non-polyester components, such as Figure 2 As shown, taking spandex as an example, after being treated with the depolymerization solution of the present invention, the spandex not only maintains a complete macroscopic morphology, but also has no damage to its microstructure.

[0021] Beneficial effects:

[0022] The sulfolane / alcohol-alkali co-solvent system used in the present invention can not only selectively depolymerize polyester to recover its monomers when depolymerizing polyester-based blended fabrics, but also ensure the complete recovery of non-polyester components, achieving full recovery (all components with a content of ≥5wt% in the blended fabric are recovered), effectively avoiding the phenomenon of "waste treatment and waste production". In addition, the sulfolane in the system is an environmentally friendly and biosafe reagent, which has little harm to the human body and the environment. In addition, it is low in cost and economically feasible, which provides the possibility for the industrialization of the recovery of polyester-based blended fabrics. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 is the reaction equation for depolymerization of PET to PTA in the co-solvent system;

[0024] Figure 2 This is a comparison diagram of the apparent morphology of spandex before and after being treated with the depolymerization solution of the present invention;

[0025] Figure 3 It is a schematic diagram of the depolymerization principle of the polyester-based blended fabric of the present invention;

[0026] Figure 4 This is the electron microscopic comparison of PET before and after sulfolane treatment;

[0027] Figure 5 This is the NMR image of hydrogen bonding between sulfolane and ethylene glycol, where the right image is an enlarged image of the left image with the chemical shift on the abscissa at 4.3-4.7 ppm. DETAILED DESCRIPTION

[0028] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0029] Detection methods of relevant indicators:

[0030] The purity of rPTA was directly measured by the HPLC standard curve method. The specific measurement conditions were as follows: a Venusil MP C18 column (size 4.6 mm × 250 mm) was used, the mobile phase was a mixture of methanol and water (volume ratio 60:40), and the pH was adjusted to 3.0 by glacial acetic acid; the flow rate was set to 0.5 mL / min; the detection wavelength of the UV detector was set to 240 nm; the temperature of the column was maintained at 25 °C;

[0031] Yield of rPTA: Use the formula Calculate, where m rPTAis the mass of rPTA monomer actually recovered, M rPTA is the molar mass of the monomer; m PET is the mass of the original polyester in the textile, M PET is the molar mass of the repeating unit of PET (192 g / mol);

[0032] Recovery rate of components other than polyester in polyester-based blended fabrics: Use the formula Calculation, where m0 is the original mass of non-polyester fibers in the fabric, and m1 is the mass of non-polyester fibers actually recovered after treatment;

[0033] Purity of lactic acid: directly measured by high performance liquid chromatography standard curve method, the specific measurement conditions are as follows: using Venusil MP C18 chromatographic column (specification: 4.6mm×250mm), the mobile phase is a mixture of methanol and ammonium dihydrogen phosphate aqueous solution with a volume ratio of 95:5 (methanol is analytical grade, and the concentration of ammonium dihydrogen phosphate aqueous solution is 0.0025M), the pH of the mixed solution is adjusted to 2.5 with phosphoric acid, the flow rate is set to 1mL / min; the detection wavelength of the ultraviolet detector is set to 210nm; the temperature of the chromatographic column is maintained at 25°C;

[0034] Lactic acid yield: Use the formula Calculate, where m rLA is the mass of lactic acid (rLA) monomer actually recovered, M rLA is the molar mass of the monomer (90 g / mol); m PLA is the mass of the original polylactic acid in the textile, M PLA is the molar mass of the repeating unit of PLA (72 g / mol).

[0035] Example 1

[0036] A method for recycling polyester-based blended fabrics, the specific steps are as follows:

[0037] (1) Raw material preparation:

[0038] Sulfolane;

[0039] Alcohol: ethylene glycol;

[0040] Strong base: sodium hydroxide;

[0041] Acid: hydrochloric acid;

[0042] Polyester-based blended fabric: polyester-spandex blended fabric, polyester content is 95wt%;

[0043] (2) Preparation of depolymerization solution:

[0044] The sulfolane, alcohol and strong base are mixed evenly to form a depolymerization solution; in the depolymerization solution, the volume ratio of sulfolane to alcohol is 70:30, and the concentration of the strong base is 0.04 g / mL;

[0045] In this process, the sulfur-oxygen double bond of sulfolane provides a hydrogen bond acceptor, competing with the hydroxide ion of the strong base to form a hydrogen bond with the alcohol; Figure 5 The NMR image of hydrogen bonding between sulfolane and alcohol shown in the figure shows that after the introduction of sulfolane, the hydrogen atom on the alcohol hydroxyl group undergoes a chemical shift from 4.48ppm to 4.45ppm and forms a triplet. This change clearly indicates that hydrogen bonding is formed between sulfolane and alcohol.

[0046] (3) Depolymerization of polyester-based blended fabrics:

[0047] After the depolymerization liquid was heated to 50°C at a heating rate of 1°C / min, the polyester-based blended fabric was added thereto and kept warm for 90 minutes under magnetic stirring;

[0048] Among them, the mass ratio of the polyester-based blended fabric to the depolymerization liquid is 1:40;

[0049] (4) Separation and filtration:

[0050] After completing step (3), firstly, filtering is used to separate solids and liquids from the depolymerized system, wherein the solids are spandex and terephthalate;

[0051] Deionized water is then added to the solid and filtered again to obtain a filtrate, which is an aqueous solution of terephthalate. The pH value of the filtrate is adjusted to 3 with an acid, and the precipitate is separated to obtain rPTA.

[0052] After testing, the purity of rPTA was 96%, the yield of rPTA was 90%, and the recovery rate of spandex was 99%.

[0053] Comparative Example 1

[0054] A method for recycling polyester-based blended fabrics is basically the same as that in Example 1, except that DMSO is used in this comparative example instead of sulfolane in Example 1.

[0055] After testing, the purity of rPTA obtained in this comparative example was 90%, and the recovery rate of spandex was 0%.

[0056] Compared with Example 1, Comparative Example 1 has no selectivity for the recovery of polyester-based blended fabrics, cannot selectively depolymerize polyester and retain non-polyester components, the product is complex and difficult to separate, and the impurity content is high, resulting in low purity of the recovered monomers. This is because DMSO is a highly polar aprotic solvent, and while depolymerizing polyester, it is easy to form a large number of hydrogen bonds with the surface of spandex, thereby causing the breakage of the spandex molecular chain. Moreover, the spandex after the breakage is not easy to be collected and recovered, and the purpose of selective separation and recovery of blended fabrics in Example 1 cannot be achieved.

[0057] Comparative Example 2

[0058] A method for recovering a polyester-based blended fabric is basically the same as that in Example 1, except that: in this comparative example, there is no sulfolane, that is, the depolymerization liquid is formed by uniformly mixing an alcohol (ethylene glycol) and a strong base (sodium hydroxide), and the concentration of the strong base is the same as that in Example 1; and the process of depolymerizing the polyester-based blended fabric in step (3) is as follows: at a pressure of 5 atm, the depolymerization liquid is heated to 200° C. at a heating rate of 2° C. / min, the polyester-based blended fabric is added thereto, and the mixture is kept warm for 3 h under magnetic stirring; wherein the mass ratio of the polyester-based blended fabric to the depolymerization liquid is 1:40;

[0059] After testing, the product obtained in this comparative example is rPTA, the purity of rPTA is 90%, the yield of rPTA is 85%, and the recovery rate of spandex is 0%.

[0060] Compared with Example 1, Comparative Example 2 not only needs to be carried out under high temperature, high pressure and long time conditions, but also has low efficiency and high energy consumption, and is not economically feasible; and the non-polyester components cannot be recycled, and the quality of the non-polyester components in the blended fabric will be greatly damaged under high temperature and high pressure conditions, and has no recycling value.

[0061] Example 2

[0062] A method for recycling polyester-based blended fabrics, the specific steps are as follows:

[0063] (1) Raw material preparation:

[0064] Sulfolane;

[0065] Alcohol: Propylene glycol;

[0066] Strong base: potassium hydroxide;

[0067] Acid: hydrochloric acid;

[0068] Polyester-based blended fabric: polyester-nylon blended fabric, polyester content is 90wt%;

[0069] (2) Preparation of depolymerization solution:

[0070] The sulfolane, alcohol and strong base are mixed evenly to form a depolymerization solution; in the depolymerization solution, the volume ratio of sulfolane to alcohol is 60:40, and the concentration of the strong base is 0.06 g / mL;

[0071] (3) Depolymerization of polyester-based blended fabrics:

[0072] After the depolymerization solution was heated to 60°C at a heating rate of 2°C / min, the polyester-based blended fabric was added thereto and kept warm for 80 minutes under magnetic stirring;

[0073] Among them, the mass ratio of the polyester-based blended fabric to the depolymerization liquid is 1:30;

[0074] (4) Separation and filtration:

[0075] After completing step (3), firstly separate the solid and the liquid from the depolymerized system by filtering, wherein the solid is nylon and terephthalate;

[0076] Deionized water is then added to the solid and filtered again to obtain a filtrate, which is an aqueous solution of terephthalate. The pH value of the filtrate is adjusted to 3 with an acid, and the precipitate is separated to obtain rPTA.

[0077] After testing, the purity of rPTA was 97%, the yield of rPTA was 95%, and the recovery rate of nylon was 98%.

[0078] Example 3

[0079] A method for recycling polyester-based blended fabrics, the specific steps are as follows:

[0080] (1) Raw material preparation:

[0081] Sulfolane;

[0082] Alcohol: Butanediol;

[0083] Strong base: potassium hydroxide;

[0084] Acid: sulfuric acid;

[0085] Polyester-based blended fabric: polyester-cotton blended fabric, polyester content is 85wt%;

[0086] (2) Preparation of depolymerization solution:

[0087] The sulfolane, alcohol and strong base are mixed evenly to form a depolymerization solution; in the depolymerization solution, the volume ratio of sulfolane to alcohol is 50:50, and the concentration of the strong base is 0.05 g / mL;

[0088] (3) Depolymerization of polyester-based blended fabrics:

[0089] After the depolymerization solution was heated to 70°C at a heating rate of 3°C / min, the polyester-based blended fabric was added thereto and kept warm for 60 min under magnetic stirring;

[0090] Among them, the mass ratio of the polyester-based blended fabric to the depolymerization liquid is 1:30;

[0091] (4) Separation and filtration:

[0092] After completing step (3), firstly separate the solid and liquid from the depolymerized system by filtering, wherein the solid is cotton and terephthalate;

[0093] Deionized water is then added to the solid and filtered again to obtain a filtrate, which is an aqueous solution of terephthalate. The pH value of the filtrate is adjusted to 3 with an acid, and the precipitate is separated to obtain rPTA.

[0094] After testing, the purity of rPTA was 95%, the yield of rPTA was 97%, and the recovery rate of cotton was 98%.

[0095] Example 4

[0096] A method for recycling polyester-based blended fabrics, the specific steps are as follows:

[0097] (1) Raw material preparation:

[0098] Sulfolane;

[0099] Alcohol: ethylene glycol;

[0100] Strong base: sodium hydroxide;

[0101] Acid: sulfuric acid;

[0102] Polyester-based blended fabric: polyester-nylon blended fabric, polyester content is 65wt%;

[0103] (2) Preparation of depolymerization solution:

[0104] The sulfolane, alcohol and strong base are mixed evenly to form a depolymerization solution; in the depolymerization solution, the volume ratio of sulfolane to alcohol is 40:60, and the concentration of the strong base is 0.05 g / mL;

[0105] (3) Depolymerization of polyester-based blended fabrics:

[0106] After the depolymerization solution was heated to 85°C at a heating rate of 4°C / min, the polyester-based blended fabric was added thereto and kept warm for 50 min under magnetic stirring;

[0107] Among them, the mass ratio of the polyester-based blended fabric to the depolymerization liquid is 1:20;

[0108] (4) Separation and filtration:

[0109] After completing step (3), firstly separate the solid and the liquid from the depolymerized system by filtering, wherein the solid is nylon and terephthalate;

[0110] Deionized water is then added to the solid and filtered again to obtain a filtrate, which is an aqueous solution of terephthalate. The pH value of the filtrate is adjusted to 3 with an acid, and the precipitate is separated to obtain rPTA.

[0111] After testing, the purity of rPTA was 96%, the yield of rPTA was 95%, and the recovery rate of nylon was 97%.

[0112] Example 5

[0113] A method for recycling polyester-based blended fabrics, the specific steps are as follows:

[0114] (1) Raw material preparation:

[0115] Sulfolane;

[0116] Alcohol: ethylene glycol;

[0117] Strong base: potassium hydroxide;

[0118] Acid: hydrochloric acid;

[0119] Polyester-based blended fabric: polyester-spandex blended fabric, polyester content is 98wt%;

[0120] (2) Preparation of depolymerization solution:

[0121] The sulfolane, alcohol and strong base are mixed evenly to form a depolymerization solution; in the depolymerization solution, the volume ratio of sulfolane to alcohol is 30:70, and the concentration of the strong base is 0.07 g / mL;

[0122] (3) Depolymerization of polyester-based blended fabrics:

[0123] After the depolymerization liquid was heated to 90°C at a heating rate of 5°C / min, the polyester-based blended fabric was added thereto and kept warm for 30 minutes under magnetic stirring;

[0124] Among them, the mass ratio of the polyester-based blended fabric to the depolymerization liquid is 1:40;

[0125] (4) Separation and filtration:

[0126] After completing step (3), firstly, filtering is used to separate solids and liquids from the depolymerized system, wherein the solids are spandex and terephthalate;

[0127] Deionized water is then added to the solid and filtered again to obtain a filtrate, which is an aqueous solution of terephthalate. The pH value of the filtrate is adjusted to 3 with an acid, and the precipitate is separated to obtain rPTA.

[0128] After testing, the purity of rPTA was 98%, the yield of rPTA was 94%, and the recovery rate of spandex was 97%.

[0129] Example 6

[0130] A method for recycling polyester-based blended fabrics, the specific steps are as follows:

[0131] (1) Raw material preparation:

[0132] Sulfolane;

[0133] Alcohol: ethylene glycol;

[0134] Strong base: potassium hydroxide;

[0135] Acid: hydrochloric acid;

[0136] Polyester-based blended fabric: polyester-cotton blended fabric, polyester content is 85wt%;

[0137] (2) Preparation of depolymerization solution:

[0138] The sulfolane, alcohol and strong base are mixed evenly to form a depolymerization solution; in the depolymerization solution, the volume ratio of sulfolane to alcohol is 60:40, and the concentration of the strong base is 0.06 g / mL;

[0139] (3) Depolymerization of polyester-based blended fabrics:

[0140] After the depolymerization solution was heated to 80°C at a heating rate of 3°C / min, the polyester-based blended fabric was added thereto and kept warm for 80 min under magnetic stirring;

[0141] Among them, the mass ratio of the polyester-based blended fabric to the depolymerization liquid is 1:30;

[0142] (4) Separation and filtration:

[0143] After completing step (3), firstly separate the solid and liquid from the depolymerized system by filtering, wherein the solid is cotton and terephthalate;

[0144] Deionized water is then added to the solid and filtered again to obtain a filtrate, which is an aqueous solution of terephthalate. The pH value of the filtrate is adjusted to 3 with an acid, and the precipitate is separated to obtain rPTA.

[0145] After testing, the purity of rPTA was 99%, the yield of rPTA was 99%, and the recovery rate of cotton was 97%.

[0146] Example 7

[0147] A method for recycling polyester-based blended fabrics, the specific steps are as follows:

[0148] (1) Raw material preparation:

[0149] Sulfolane;

[0150] Alcohol: Butanediol;

[0151] Strong base: potassium hydroxide;

[0152] Acid: hydrochloric acid;

[0153] Polyester-based blended fabric: PBT / cotton blended fabric, PBT content is 65wt%;

[0154] (2) Preparation of depolymerization solution:

[0155] The sulfolane, alcohol and strong base are mixed evenly to form a depolymerization solution; in the depolymerization solution, the volume ratio of sulfolane to alcohol is 60:40, and the concentration of the strong base is 0.06 g / mL;

[0156] (3) Depolymerization of polyester-based blended fabrics:

[0157] After the depolymerization solution was heated to 80°C at a heating rate of 3°C / min, the polyester-based blended fabric was added thereto and kept warm for 80 min under magnetic stirring;

[0158] Among them, the mass ratio of the polyester-based blended fabric to the depolymerization liquid is 1:30;

[0159] (4) Separation and filtration:

[0160] After completing step (3), firstly separate the solid and liquid from the depolymerized system by filtering, wherein the solid is cotton and terephthalate;

[0161] Deionized water is then added to the solid and filtered again to obtain a filtrate, which is an aqueous solution of terephthalate. The pH value of the filtrate is adjusted to 3 with an acid, and the precipitate is separated to obtain rPTA.

[0162] After testing, the purity of rPTA was 99%, the yield of rPTA was 98%, and the recovery rate of cotton was 97%.

[0163] Example 8

[0164] A method for recycling polyester-based blended fabrics, the specific steps are as follows:

[0165] (1) Raw material preparation:

[0166] Sulfolane;

[0167] Alcohol: hexanediol;

[0168] Strong base: potassium hydroxide;

[0169] Acid: hydrochloric acid;

[0170] Polyester-based blended fabric: PLA / cotton blended fabric, PLA content is 80wt%;

[0171] (2) Preparation of depolymerization solution:

[0172] The sulfolane, alcohol and strong base are mixed evenly to form a depolymerization solution; in the depolymerization solution, the volume ratio of sulfolane to alcohol is 60:40, and the concentration of the strong base is 0.06 g / mL;

[0173] (3) Depolymerization of polyester-based blended fabrics:

[0174] After the depolymerization solution was heated to 80°C at a heating rate of 3°C / min, the polyester-based blended fabric was added thereto and kept warm for 80 min under magnetic stirring;

[0175] Among them, the mass ratio of the polyester-based blended fabric to the depolymerization liquid is 1:30;

[0176] (4) Separation and filtration:

[0177] After completing step (3), firstly separate the solid and the liquid from the depolymerized system by filtering, wherein the solid is cotton, and then separate the product lactic acid from the liquid by vacuum distillation;

[0178] After testing, the purity of lactic acid was 98%, the yield of lactic acid was 99%, and the recovery rate of cotton was 97%.

[0179] Example 9

[0180] A method for recycling polyester-based blended fabrics, the specific steps are as follows:

[0181] (1) Raw material preparation:

[0182] Sulfolane;

[0183] Alcohol: Butanediol;

[0184] Strong base: potassium hydroxide;

[0185] Acid: hydrochloric acid;

[0186] Polyester-based blended fabric: PBAT / cotton blended fabric, PBAT content is 85wt%;

[0187] (2) Preparation of depolymerization solution:

[0188] The sulfolane, alcohol and strong base are mixed evenly to form a depolymerization solution; in the depolymerization solution, the volume ratio of sulfolane to alcohol is 60:40, and the concentration of the strong base is 0.06 g / mL;

[0189] (3) Depolymerization of polyester-based blended fabrics:

[0190] After the depolymerization solution was heated to 80°C at a heating rate of 3°C / min, the polyester-based blended fabric was added thereto and kept warm for 80 min under magnetic stirring;

[0191] Among them, the mass ratio of the polyester-based blended fabric to the depolymerization liquid is 1:30;

[0192] (4) Separation and filtration:

[0193] After completing step (3), firstly separate the solid and liquid from the depolymerized system by filtering, wherein the solid is cotton and terephthalate;

[0194] Deionized water is then added to the solid and filtered again to obtain a filtrate, which is an aqueous solution of terephthalate. The pH value of the filtrate is adjusted to 3 with an acid, and the precipitate is separated to obtain rPTA.

[0195] After testing, the purity of rPTA was 99%, the yield of rPTA was 99%, and the recovery rate of cotton was 97%.

Claims

1. A method for recycling polyester-based blended fabrics, characterized in that: A polyester-based blended fabric is added to a depolymerization liquid composed of cyclopentane sulfone, alcohol and a strong base for depolymerization. After depolymerization, the liquid and the solid are separated and treated. When the polyester in the polyester-based blended fabric is PET, PBT or PBAT, the treatment process is: deionized water is added to the solid and then filtered again to obtain a filtrate, the pH value of the filtrate is adjusted with an acid until a precipitate is precipitated, and the precipitate is collected to obtain rPTA; when the polyester in the polyester-based blended fabric is PLA, the treatment process is: the liquid is subjected to reduced pressure distillation, and the distillate is collected to obtain lactic acid.

2. The method for recycling polyester-based blended fabric according to claim 1, characterized in that: The polyester-based blended fabric is a polyester-spandex blended fabric, a polyester-cotton blended fabric, a polyester-nylon blended fabric, a PBT / cotton blended fabric, a PLA / cotton blended fabric or a PBAT / cotton blended fabric, and the polyester content is more than 65wt%.

3. The method for recycling polyester-based blended fabric according to claim 1, characterized in that: The alcohol is ethylene glycol, propylene glycol, butylene glycol or hexylene glycol; the strong base is sodium hydroxide or potassium hydroxide.

4. The method for recycling polyester-based blended fabric according to claim 1, characterized in that: The volume ratio of sulfolane to alcohol is 30:70-70:30; the concentration of the strong base in the depolymerization solution is 0.04-0.07 g / mL; and the mass ratio of the polyester-based blended fabric to the depolymerization solution is 1:20-40.

5. The method for recycling polyester-based blended fabric according to claim 1, characterized in that: The process of adding the polyester-based blended fabric into a depolymerization solution formed by cyclopentane sulfone, alcohol and strong base for depolymerization is as follows: after the depolymerization solution formed by cyclopentane sulfone, alcohol and strong base is heated to 50-90°C at a heating rate of 1-5°C / min, the polyester-based blended fabric is added thereto, and the solution is kept warm for 30-90 minutes under magnetic stirring.

6. The method for recycling polyester-based blended fabric according to claim 1, characterized in that: The purity of rPTA or lactic acid is 95-99%, and the yield of rPTA or lactic acid is 90-99%.

7. The method for recycling polyester-based blended fabric according to claim 1, characterized in that: The recovery rate of components other than polyester in polyester-based blended fabrics is 97~99%.

Citation Information

Patent Citations

  • Method for separating and recycling waste polyester-cotton blended fabric

    CN112409635A

  • High-shrinkage polyester sea-island fiber as well as preparation method and application thereof

    CN116288804A

  • Recycling method for depolymerization of waste terylene and mild selective depolymerization of blended textiles of waste terylene

    CN116425621A

  • Polyester-based recycling method for mild, efficient and selective hydrolysis of waste high polymer material

    CN116769231A

  • Efficient alcoholysis method of waste polyester

    CN116891410A