Interface modifier as well as preparation method and application thereof
Through the covalent combination of the interface modifier of the multifunctional molecular structure with white carbon black and rubber, it participates in the vulcanization process, the problems of insufficient wear resistance and volatile organic matter emissions in the prior art are solved. Higher wear resistance and lower volatile organic release are achieved.
Patent Information
- Application Number
- CN202411176706.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-12-03
AI Technical Summary
The prior art has shortcomings in improving the wear resistance of white carbon black/rubber composite materials. The coupling efficiency of silane coupling agents is low and volatile organic compounds are generated during use, which affects environmental protection and production costs.
Using an interface modifier with a multifunctional molecular structure, the cycloalkenyl silane is prepared by reacting amino cycloalkenyl olefins and alkoxysilane glycidyl ether under specific conditions. The cycloalkenyl silanes formed are covalently combined with white carbon black and rubber to participate in sulfurization. process to improve the efficiency of silanization reaction.
Significantly improve the dispersion and interface combination of white carbon black in the rubber matrix, reduce the acron wear volume of composite materials, reduce the silane content and volatile organic matter release, and improve wear resistance and mechanical properties.
Smart Images

Figure CN119060085A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of interface modifiers, and specifically relates to an interface modifier and a preparation method and application thereof. Background Art
[0002] As a nanofiller, silica is widely used in the rubber industry. Green tires with silica as the main filler have the advantages of anti-skid, low rolling resistance and high wear resistance. Due to the hydrogen bond interaction of the abundant silanol groups on the surface, silica is very easy to agglomerate in the non-polar rubber matrix. In order to improve the performance of composite materials, silane coupling agents are now widely used in industrial production to chemically modify silica to improve the dispersibility and interfacial bonding of silica in the rubber matrix. At present, there are limitations in the application of silane coupling agents. On the one hand, the amount of silane in the traditional formula is 8wt% to 10wt% of silica, and the degree of silanization is seriously insufficient under the existing conditions. The low coupling efficiency leads to excessive actual silane usage, which increases the manufacturing cost of tires. On the other hand, the ethoxy group of the silane coupling agent will produce alcohols such as methanol or ethanol in the silanization reaction with the silanol groups on the surface of silica. Alcohol, as a volatile organic compound, will increase the porosity of the tire and pollute the environment. Improving the coupling efficiency of silane coupling agents and reducing the emission of volatile organic compounds have become important research directions in the current green tire production.
[0003] At present, the relevant fields start from the molecular structure design and prepare various new interface modifiers in order to improve the performance of rubber composite materials and realize the cleanness and environmental protection of industrial production to the greatest extent. Patent CN113652010A uses end-functionalized liquid rubber and mercaptosilane coupling agent to synergistically modify silica, which significantly improves the mechanical strength and dynamic mechanical properties of rubber composite materials, but the presence of mercapto causes the scorch phenomenon of rubber, which greatly affects the vulcanization processing of rubber tires. Patent CN113980366A synthesizes silane-functionalized polysulfides with adjustable molecular structures through reverse vulcanization. The modified rubber composite material achieves lower volatile organic compound emissions and better silica dispersion. The material shows higher mechanical properties and lower rolling resistance, but the presence of polysulfides also affects rubber vulcanization. Patent CN115368573A develops a silane polymer containing polyether long chain segments to further improve the compatibility of silica with rubber matrix. At the same time, the silane polymer can effectively reduce the volatile organic gas generated during industrial production. Patent CN113321855A uses cardanol polyoxyethylene ether sulfide and / or mercapto-containing cardanol polyoxyethylene ether compounds as functional additives in combination with silane coupling agents. The resulting rubber composite material has better wear resistance and lower compression fatigue temperature rise than the existing silica-filled rubber compound.
[0004] However, the above modification methods either introduce polysulfide groups and / or thiol groups that affect the rubber vulcanization process, or involve a multi-step, more complicated chemical synthesis process. Most importantly, the wear resistance needs to be improved. Therefore, it is necessary to develop an interfacial modifier that can improve the wear resistance of silica / rubber composites. Summary of the invention
[0005] The invention provides an interface modifier and a preparation method and application thereof, which solves the problem in the prior art that the wear resistance of a silane coupling agent-modified white carbon black / rubber composite material urgently needs to be improved.
[0006] The first aspect of the present invention provides an interfacial modifier, the general structural formula of which is as follows:
[0007]
[0008] Wherein, R is one of norbornene ring group, cyclohexenyl group, cyclopentenyl group and cycloheptenyl group; R1 is independently selected from C1-C8 straight chain alkyl group or straight chain alkoxy group; R2 is independently selected from C1-C8 straight chain alkyl group or straight chain alkoxy group; R3 is independently selected from methyl group, ethyl group or C1-C2 alkoxy group; R4 is independently selected from methyl group, ethyl group or C1-C2 alkoxy group; R5 is independently selected from methyl group, ethyl group or C1-C2 alkoxy group; X is hydrogen atom, methyl group, ethyl group, halogen atom, hydroxyl group or C1-C2 alkoxy group.
[0009] Preferably, R is a norbornene ring group; R1 is independently selected from a C1-C6 straight-chain alkyl group or a C1-C6 straight-chain alkoxy group; R2 is independently selected from a C3-C6 straight-chain alkyl group or a C3-C6 straight-chain alkoxy group; R3 is independently selected from a methyl group or a C1-C2 straight-chain alkoxy group; R4 is independently selected from a methyl group or a C1-C2 straight-chain alkoxy group; R5 is independently selected from a methyl group or a C1-C2 straight-chain alkoxy group; and X is a hydrogen atom, an alkyl group, a halogen atom, or a hydroxyl group.
[0010] Preferably, R is 5-norbornene; R1 is methine; R2 is methoxypropyl; R3 is ethoxy; R4 is ethoxy; R5 is methyl; and X is a hydrogen atom.
[0011] The second object of the present invention is to protect the preparation method of the interface modifier, the steps comprising:
[0012] The aminocycloolefin and alkoxysilane glycidyl ether are reacted at 40° C. to 180° C. to obtain the interface modifier.
[0013] Preferably, the reaction time is 5 h to 24 h.
[0014] Preferably, the molar ratio of aminocycloolefin to alkoxysilane glycidyl ether is 1:2.
[0015] Preferably, the general formula of the aminocycloolefin is as follows:
[0016]
[0017] Wherein, R is one of norbornene ring group, cyclohexenyl group, cyclopentenyl group and cycloheptenyl group; R1 is independently selected from C1-C8 straight chain alkyl group or straight chain alkoxy group; X is hydrogen atom, methyl group, ethyl group, halogen atom, hydroxyl group or C1-C2 alkoxy group.
[0018] Preferably, the general formula of the alkoxysilane glycidyl ether is as follows:
[0019]
[0020] Among them, R2 is independently selected from a C1-C8 straight-chain alkyl or straight-chain alkoxy group; R3 is independently selected from a methyl group, an ethyl group or a C1-C2 alkoxy group; R4 is independently selected from a methyl group, an ethyl group or a C1-C2 alkoxy group; R5 is independently selected from a methyl group, an ethyl group or a C1-C2 alkoxy group.
[0021] The third object of the present invention is to protect the application of the interface modifier in silica / rubber composite materials.
[0022] Preferably, the white carbon black / rubber composite material comprises the following raw materials in parts by weight:
[0023] 100 parts of rubber, 2-4 parts of interface modifier, 40-50 parts of white carbon black, 2 parts of antioxidant, 9.5-13.5 parts of vulcanization package.
[0024] Preferably, the white carbon black / rubber composite material comprises the following raw materials in parts by weight:
[0025] 100 parts of rubber, 2-4 parts of interface modifier, 40 parts of white carbon black, 2 parts of antioxidant, and 13.5 parts of vulcanization package.
[0026] Preferably, the rubber is one or more of emulsion-polymerized styrene-butadiene rubber, solution-polymerized styrene-butadiene rubber, natural rubber, isoprene rubber, butadiene rubber, butyl rubber, and silicone rubber.
[0027] Preferably, the antioxidant is one or more of antioxidant RD, antioxidant 4010NA, antioxidant 4010 and antioxidant 4020.
[0028] Preferably, the vulcanization package comprises the following raw materials by weight: 5 parts of zinc oxide, 1 part of stearic acid, 2 to 5 parts of accelerator, and 1.5 to 2.5 parts of sulfur.
[0029] Preferably, the accelerator is one or more of accelerator CZ, accelerator DZ, accelerator M, accelerator DM, accelerator NS, accelerator D and accelerator TT.
[0030] The fourth object of the present invention is to protect the preparation method of the white carbon black / rubber composite material, the steps comprising:
[0031] The rubber, interface modifier, white carbon black, antioxidant and vulcanization package in the formulated amount are mixed at 50° C. to 150° C. for 5 to 12 minutes, and hot-pressed vulcanized to obtain the rubber composite material.
[0032] Preferably, the hot pressing vulcanization conditions are 140-170°C, 100-200 kgf / cm 2 , 10 to 40 minutes.
[0033] Preferably, the mixing conditions are: 80-120° C., 8-10 min.
[0034] Compared with the prior art, the present invention has the following beneficial effects:
[0035] 1) The interface modifier provided by the present invention can, based on its multifunctional molecular structure, on the one hand, covalently bond with silica to significantly improve the dispersibility of silica in the rubber matrix; on the other hand, it can bond with the rubber matrix to effectively participate in the vulcanization process of the rubber matrix, and improve the efficiency of the silanization reaction through internal catalysis, thereby improving the wear resistance of the silica / rubber composite material. It can be seen from the test results that compared with the existing interface modifiers, the interface modifier prepared by the present invention can significantly reduce the Akron wear volume of the composite material after being used in the silica / rubber composite material. In addition, compared with traditional silanes, the interface modifier of the present invention has a lower silane content, and the release of volatile organic compounds in the process of modifying silica is less.
[0036] 2) The synthesis process of the interface modifier of the present invention is simple and does not require complicated purification steps. It can be successfully prepared through a simple step of epoxy-amino ring-opening reaction, and can be directly mixed with silica and rubber to improve the dispersion of silica in the rubber matrix and the interface bonding with the matrix, thereby enhancing the performance of the composite material.
[0037] 3) The interface modifier of the present invention is compatible with the processing technology of the tire industry and can be directly applied to a variety of industrial rubber formulations using white carbon black as a filler. It has universal applicability and huge application potential, and is of great significance for the development of high-performance, low-volatile organic compound emission green tires. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 A synthetic route diagram of the interface modifier provided by the present invention;
[0039] Figure 2 This is the infrared spectrum of the interface modifier prepared in Example 7 of the present invention;
[0040] Figure 3 This is the infrared spectrum of the interface modifier prepared in Comparative Example 3 of the present invention. DETAILED DESCRIPTION
[0041] The technical solutions in the embodiments of the present application will be described clearly and completely below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0042] In the following description of this embodiment, the term "and / or" is used to describe the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can represent: A exists alone, B exists alone, and A and B exist at the same time. Among them, A and B can be singular or plural; the single symbol " / " means "or".
[0043] In the following description of this embodiment, the term "at least one" refers to one or more, and "plurality" refers to two or more. "At least one of the following" or similar expressions refer to any combination of these items, including any combination of single items or plural items. For example, "at least one of A, B or C", or "at least one of A, B and C" can represent any one of A, B, C, or A+B, or A+C, or B+C, or A+B+C, where A, B, C can be single or multiple, respectively.
[0044] In the following description of this embodiment, the order of serial numbers does not mean the order of execution. Some or all of the steps can be executed in parallel or sequentially. The execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of this embodiment.
[0045] In the following description of the present embodiment, the numerical range should be understood to also specifically disclose each intermediate value between the upper and lower limits of the range. Any stated value or intermediate value in the stated range and any other stated value or each smaller range between the intermediate values in the stated range are also included in the present embodiment, and the upper and lower limits of the smaller range can be independently included or excluded in the range.
[0046] Unless otherwise stated, the technical / scientific terms used in the present embodiment have the same meanings as those generally understood by those skilled in the art to which the present application belongs. Although the present application only describes preferred methods and materials, any similar or equivalent methods and materials may also be used in the implementation or testing of the present application. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials related to the documents. In the event of any conflict with any incorporated document, the content of this specification shall prevail.
[0047] The present application provides an interfacial modifier, the general structural formula of which is as follows:
[0048]
[0049] Wherein, R is one of norbornene ring group, cyclohexenyl group, cyclopentenyl group and cycloheptenyl group; R1 is independently selected from C1-C8 straight chain alkyl group or straight chain alkoxy group; R2 is independently selected from C1-C8 straight chain alkyl group or straight chain alkoxy group; R3 is independently selected from methyl group, ethyl group or C1-C2 alkoxy group; R4 is independently selected from methyl group, ethyl group or C1-C2 alkoxy group; R5 is independently selected from methyl group, ethyl group or C1-C2 alkoxy group; X is hydrogen atom, methyl group, ethyl group, halogen atom, hydroxyl group or C1-C2 alkoxy group.
[0050] Table 1 Sources of raw materials used in the examples and comparative examples of the present invention
[0051]
[0052]
[0053] The synthesis route of the interface modifier in the embodiment of the present invention is shown in Figure 1 .
[0054] Example 1
[0055] An interfacial modifier has the following structural formula:
[0056]
[0057] 9.8 g of 5-norbornene-2-methylamine and 39.5 g of 3-glycidyloxypropylmethyldiethoxysilane were added to a single-necked flask, and heated and stirred at 40° C. After reacting for 24 hours, cycloalkenylsilane, i.e., the interface modifier, was obtained with a yield of 97%.
[0058] A rubber composite material comprises the following raw materials in parts by weight:
[0059] 100g of emulsion polybutadiene styrene rubber, 2g of cycloalkenyl silane, 40g of white carbon black, 40202g of antioxidant, and 9.5g of vulcanization package.
[0060] Curing package: zinc oxide 5g, stearic acid 1g, accelerator CZ 1.6g, accelerator D 2g, sulfur 1.5g.
[0061] A method for preparing a rubber composite material comprises the following steps:
[0062] The rubber, cycloalkenyl silane, white carbon black, antioxidant 4020 and vulcanization package in the formula were mixed at 50°C for 12 minutes and hot-pressed to obtain the rubber composite material. The hot-pressed vulcanization conditions were 140°C, 100 kgf / cm 2 , 40min.
[0063] Example 2
[0064] An interfacial modifier has the following structural formula:
[0065]
[0066] 9.8 g of 5-norbornene-2-methylamine and 39.5 g of 3-glycidyloxypropylmethyldiethoxysilane were added to a single-necked flask, and heated and stirred at 80° C. After reacting for 10 hours, cycloalkenylsilane, i.e., the interface modifier, was obtained with a yield of 97%.
[0067] A rubber composite material comprises the following raw materials in parts by weight:
[0068] 100g of emulsion polybutadiene styrene rubber, 2g of cycloalkenyl silane, 40g of white carbon black, 40202g of antioxidant, and 10.5g of vulcanization package.
[0069] Curing package: zinc oxide 5g, stearic acid 1g, accelerator CZ 1.6g, accelerator D 2g, sulfur 2g.
[0070] A method for preparing a rubber composite material comprises the following steps:
[0071] The rubber, cycloalkenyl silane, white carbon black, antioxidant 4020 and vulcanization package in the formula were mixed at 80°C for 8 minutes and hot-pressed to obtain the rubber composite material. The hot-pressed vulcanization conditions were 150°C, 130 kgf / cm 2 , 30min.
[0072] Example 3
[0073] An interfacial modifier has the following structural formula:
[0074]
[0075] 9.8 g of 5-norbornene-2-methylamine and 39.5 g of 3-glycidyloxypropylmethyldiethoxysilane were added to a single-necked flask, nitrogen was introduced, and the mixture was heated and stirred at 120° C. After reacting for 8 hours, cycloalkenylsilane, i.e., the interface modifier, was obtained with a yield of 97%.
[0076] A rubber composite material comprises the following raw materials in parts by weight:
[0077] Emulsion polybutadiene styrene rubber 100g, cycloalkenyl silane 2g, white carbon black 40g, antioxidant 40202g, vulcanization package 11.5g. Vulcanization package: zinc oxide 5g, stearic acid 1g, accelerator CZ 1.6g, accelerator D 2g, sulfur 2.5g.
[0078] A method for preparing a rubber composite material comprises the following steps:
[0079] The rubber, cycloalkenyl silane, white carbon black, antioxidant and vulcanization package in the formula are mixed at 120°C for 10 minutes and hot-pressed to obtain the rubber composite material. The hot-pressed vulcanization conditions are 160°C, 160kgf / cm 2 , 20min.
[0080] Example 4
[0081] An interfacial modifier has the following structural formula:
[0082]
[0083] 9.8 g of 5-norbornene-2-methylamine and 39.5 g of 3-glycidyloxypropylmethyldiethoxysilane were added to a single-necked flask, nitrogen was introduced, and the mixture was heated and stirred at 180° C. After reacting for 5 hours, cycloalkenylsilane, i.e., the interface modifier, was obtained with a yield of 97%.
[0084] A rubber composite material comprises the following raw materials in parts by weight:
[0085] 100g of emulsion polybutadiene styrene rubber, 2g of cycloalkenyl silane, 40g of white carbon black, 40202g of antioxidant, and 13.5g of vulcanization package.
[0086] Curing package: zinc oxide 5g, stearic acid 1g, accelerator CZ 1.6g, accelerator D 2g, sulfur 2.5g.
[0087] A method for preparing a rubber composite material comprises the following steps:
[0088] The rubber, cycloalkenyl silane, white carbon black, antioxidant and vulcanization package in the formula are mixed at 150°C for 5 minutes and hot-pressed to obtain the rubber composite material. The hot-pressed vulcanization conditions are 170°C, 200kgf / cm2 , 10min.
[0089] Example 5
[0090] An interfacial modifier has the following structural formula:
[0091]
[0092] 9.8 g of 5-norbornene-2-methylamine and 39.5 g of 3-glycidyloxypropylmethyldiethoxysilane were added to a single-necked flask, nitrogen was introduced, and the mixture was heated and stirred at 80° C. After reacting for 10 hours, cycloalkenylsilane, i.e., the interface modifier, was obtained with a yield of 97%.
[0093] A rubber composite material comprises the following raw materials in parts by weight:
[0094] 100g of emulsion polybutadiene styrene rubber, 3g of cycloalkenyl silane, 40g of white carbon black, 40202g of antioxidant, and 13.5g of vulcanization package.
[0095] Curing package: zinc oxide 5g, stearic acid 1g, accelerator CZ 1.6g, accelerator D 2g, sulfur 2.5g.
[0096] A method for preparing a rubber composite material comprises the following steps:
[0097] The rubber, cycloalkenyl silane, white carbon black, antioxidant and vulcanization package in the formula are mixed at 150°C for 5 minutes and hot-pressed to obtain the rubber composite material. The hot-pressed vulcanization conditions are 170°C, 200kgf / cm 2 , 10min.
[0098] Example 6
[0099] An interfacial modifier has the following structural formula:
[0100]
[0101] 9.8 g of 5-norbornene-2-methylamine and 39.5 g of 3-glycidyloxypropylmethyldiethoxysilane were added to a single-necked flask, nitrogen was introduced, and the mixture was heated and stirred at 80° C. After reacting for 10 hours, cycloalkenylsilane, i.e., the interface modifier, was obtained with a yield of 97%.
[0102] A rubber composite material comprises the following raw materials in parts by weight:
[0103] 100g of emulsion polybutadiene styrene rubber, 4g of cycloalkenyl silane, 40g of white carbon black, 40202g of antioxidant, and 13.5g of vulcanization package.
[0104] Curing package: zinc oxide 5g, stearic acid 1g, accelerator CZ 1.6g, accelerator D 2g, sulfur 2.5g.
[0105] A method for preparing a rubber composite material comprises the following steps:
[0106] The rubber, cycloalkenyl silane, white carbon black, antioxidant and vulcanization package in the formula are mixed at 150°C for 5 minutes and hot-pressed to obtain the rubber composite material. The hot-pressed vulcanization conditions are 170°C, 200kgf / cm 2 , 10min.
[0107] Example 7
[0108] An interfacial modifier has the following structural formula:
[0109]
[0110] 9.8 g of 5-norbornene-2-methylamine and 39.5 g of 3-glycidyloxypropylmethyldiethoxysilane were added to a single-necked flask, nitrogen was introduced, and the mixture was heated and stirred at 80° C. After reacting for 10 hours, cycloalkenylsilane, i.e., the interface modifier, was obtained with a yield of 97%.
[0111] A rubber composite material comprises the following raw materials in parts by weight:
[0112] 100g natural rubber, 2g cycloalkenylsilane, 50g white carbon black, 40202g antioxidant, 13.5g vulcanization package.
[0113] Curing package: zinc oxide 5g, stearic acid 1g, accelerator CZ 1.6g, accelerator D 2g, sulfur 2.5g.
[0114] A method for preparing a rubber composite material comprises the following steps:
[0115] The natural rubber, cycloalkenyl silane, white carbon black, antioxidant and vulcanization package in the formula are mixed at 150°C for 5 minutes and hot-pressed to obtain the rubber composite material. The hot-pressed vulcanization conditions are 170°C, 200kgf / cm 2 , 10min.
[0116] Since the interface modifiers prepared in Examples 1 to 6 have the same structure as the interface modifier prepared in Example 7, only the spectrum of the interface modifier prepared in Example 7 is used for description below. Figure 2 The infrared spectrum of the interface modifier prepared in Example 7 of the present invention, wherein 3443 cm -1 The absorption peak attributable to the stretching vibration of hydroxyl group is 2850-2950cm -1 is the stretching vibration peak of methylene, 1660cm-1 The stretching vibration absorption peaks attributable to unsaturated carbon-carbon double bonds are 1085-1300 cm -1 It is the asymmetric stretching vibration band of aliphatic ether, 1000-1200cm -1 is the stretching vibration band of Si-O, 1071cm -1 The above infrared absorption bands prove that the interface modifier prepared in Example 1 of the present invention is successfully synthesized.
[0117] Comparative Example 1
[0118] A rubber composite material comprises the following raw materials in parts by weight:
[0119] Emulsion polybutadiene styrene rubber 100g, white carbon black 40g, antioxidant 40202g; vulcanization bag 9.5g.
[0120] Zinc oxide 5g, stearic acid 1g, accelerator CZ 1.6g, accelerator D 2g, sulfur 1.5g.
[0121] A method for preparing a rubber composite material comprises the following steps:
[0122] The rubber, white carbon black, antioxidant and vulcanization package in the formula are mixed at 50°C for 12 minutes, and hot-pressed vulcanized to obtain the rubber composite material. The hot-pressed vulcanization conditions are 140°C, 100kgf / cm 2 , 10min.
[0123] Comparative Example 2
[0124] A rubber composite material comprises the following raw materials in parts by weight:
[0125] 100g natural rubber, 50g white carbon black, 40202g antioxidant, 13.5g vulcanization package.
[0126] Curing package: zinc oxide 5g, stearic acid 1g, accelerator CZ 1.6g, accelerator D 2g, sulfur 2.5g.
[0127] A method for preparing a rubber composite material comprises the following steps:
[0128] The natural rubber, white carbon black, antioxidant and vulcanization package in the formula are mixed at 150°C for 5 minutes and hot-pressed to obtain the rubber composite material. The hot-pressed vulcanization conditions are 170°C, 200kgf / cm 2 , 10min.
[0129] Comparative Example 3
[0130] An interface modifier, the interface modifier in this comparative example is acyclic alkenyl silane H, and its structural formula is as follows:
[0131]
[0132] 7.7 g of 5-hexen-1-amine and 38.6 g of 3-glycidyloxypropylmethyldiethoxysilane were added to a single-necked flask, nitrogen was introduced, and the mixture was heated and stirred at 80° C. After reacting for 10 hours, acyclic alkenylsilane H was obtained with a yield of 96%.
[0133] Figure 3 This is the infrared spectrum of the interface modifier prepared in this comparative example. -1 The absorption peaks are attributable to the stretching vibration of hydroxyl groups, 2858-2965 cm -1 is the stretching vibration peak of methylene, 1684 cm -1 The stretching vibration absorption peaks attributable to unsaturated carbon-carbon double bonds are 1019-1262 cm -1 It is the asymmetric stretching vibration band of aliphatic ether, 1012-1105cm -1 is the stretching vibration band of Si-O, 1074cm -1 The above infrared absorption bands prove that the non-cyclic olefin interface modifier prepared in this comparative example is successfully synthesized.
[0134] A rubber composite material comprises the following raw materials in parts by weight:
[0135] Emulsion polybutadiene styrene rubber 100g, non-cycloalkenyl silane H 2g, white carbon black 40g, antioxidant 40202g, vulcanization package 13.5g.
[0136] Curing package: zinc oxide 5g, stearic acid 1g, accelerator CZ 1.6g, accelerator D 2g, sulfur 2.5g.
[0137] A method for preparing a rubber composite material comprises the following steps:
[0138] The rubber, non-cycloalkenyl silane H, white carbon black, antioxidant and vulcanization package in the formula are mixed at 150°C for 5 minutes and hot-pressed to obtain the rubber composite material. The hot-pressed vulcanization conditions are 170°C, 200kgf / cm 2 , 10min.
[0139] Comparative Example 4
[0140] A rubber composite material comprises the following raw materials in parts by weight:
[0141] Emulsion polybutadiene styrene rubber 100g, Si692g, white carbon black 40g, antioxidant 40202g, vulcanization package 13.5g.
[0142] Curing package: zinc oxide 5g, stearic acid 1g, accelerator CZ 1.6g, accelerator D 2g, sulfur 1.5g.
[0143] A method for preparing a rubber composite material comprises the following steps:
[0144] The rubber, Si69, white carbon black, antioxidant and vulcanization package in the formula are mixed at 150°C for 5 minutes and hot-pressed to obtain the rubber composite material. The hot-pressed vulcanization conditions are 170°C, 200kgf / cm 2 , 10min.
[0145] The rubber composite materials prepared in Examples 1-7 and the rubber composite materials prepared in Comparative Examples 1-4 were subjected to mechanical tests, respectively, and the test results are shown in Table 2; wherein, the tensile strength, elongation at break and 300% elongation stress were measured in accordance with ISO37-2005, the test temperature was room temperature, and the stretching rate was 500 mm / min; the fatigue heat generation standard was measured in accordance with ISO 4666-3:2006; the rolling resistance was measured using a rubber processing analyzer, and the tanδ value of 7% strain measured at a frequency of 10 Hz represented the rolling resistance; the anti-wet skid performance was measured using a dynamic thermal mechanical analyzer, and the tanδ value of 0°C measured at a frequency of 10 Hz represented the anti-wet skid performance, the temperature change rate was 3°C / min, and the strain was 0.1%; the wear volume was measured using an Akron abrasion tester, and the measurement standard was GB / T 1689-2014.
[0146] Table 2 Performance test results of rubber composites prepared in different groups
[0147]
[0148]
[0149] Comparison of Comparative Example 1 in Table 2 and Examples 1-7 respectively shows that in the mixing process of silica / rubber composite materials, after adding cycloalkenyl interfacial modifiers of different structures, the 300% tensile stress and wet skid resistance (Tanδ(0°C)) are significantly improved, the rolling resistance (Tanδ(60°C)) is reduced, and the fatigue temperature rise and wear volume are significantly reduced. Comparison of Comparative Example 1 in Table 2 with Example 1 shows that when cycloalkenyl silane is added, the elongation at break can be reduced, the 300% tensile stress can be increased, the fatigue temperature rise can be reduced, the rolling resistance can be reduced, the wet skid resistance can be improved, and the Akron wear volume can be reduced. Increasing the amount of interfacial modifier can improve the tensile modulus and wear volume of the rubber composite material (see Examples 4 to 6). When the amount of cycloalkenyl silane is 5% of silica, the rubber composite material has the best comprehensive performance, including higher mechanical properties and lower fatigue temperature rise, rolling resistance and Akron wear volume.
[0150] By comparing Comparative Example 2 with Example 7, it can be found that Example 7 has higher tensile strength and 300% modulus of tensile stress, lower fatigue temperature rise and rolling resistance (Tanδ@60°C), and lower Akron wear volume, which indicates that cycloalkenylsilane can still play a coupling role in the silica / natural rubber mixing process, and the mechanical properties of the prepared rubber composite material are improved while also achieving improved dynamic properties.
[0151] By comparing Comparative Example 3 with Example 1, Example 2, Example 3, Example 6, and Example 7, it was found that compared with non-cycloalkenyl silane, the rubber composite material prepared after adding cycloalkenyl silane obtained better comprehensive performance, and the rubber composite material prepared by norbornene silane had the best comprehensive performance. This is because the ring tension of the norbornene structure makes its unsaturated double bond have high reactivity with sulfur, which can participate in the vulcanization process of the rubber and build a good interface bonding.
[0152] Comparing Comparative Example 4 with Example 1, Example 2, Example 3, Example 6, and Example 7, it is found that compared with the traditional sulfur-containing group silane coupling agent, the comprehensive performance of the rubber composite material prepared after the addition of cycloalkenyl silane is significantly improved. This is because the interface modifier prepared by the present invention can improve the dispersibility of silica in the rubber matrix by covalently bonding with silica; on the other hand, the interface modifier can be combined with the rubber matrix and effectively participate in the vulcanization process of the rubber matrix, thereby improving the silanization reaction efficiency through internal catalysis, thereby improving the wear resistance of the silica / rubber composite material.
[0153] In summary, the multifunctional interfacial modifier of the present invention can improve the dispersibility of silica in rubber, greatly reduce the fatigue temperature rise of the rubber composite material under dynamic load, and at the same time, the anti-slip performance and wear resistance of the material are significantly improved, and finally a rubber composite material with low heat generation, anti-slip and high wear resistance can be obtained.
[0154] Although the preferred embodiments of the present invention have been described, those skilled in the art may make other changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.
[0155] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.
Claims
1. An interfacial modifier, characterized in that: Its general structural formula is as follows: Wherein, R is one of norbornene ring group, cyclohexenyl group, cyclopentenyl group and cycloheptenyl group; R1 is independently selected from C1-C8 straight chain alkyl group or straight chain alkoxy group; R2 is independently selected from C1-C8 straight chain alkyl group or straight chain alkoxy group; R3 is independently selected from methyl group, ethyl group or C1-C2 alkoxy group; R4 is independently selected from methyl group, ethyl group or C1-C2 alkoxy group; R5 is independently selected from methyl group, ethyl group or C1-C2 alkoxy group; X is hydrogen atom, methyl group, ethyl group, halogen atom, hydroxyl group or C1-C2 alkoxy group.
2. A method for preparing the interface modifier according to claim 1, characterized in that the steps include: The aminocycloolefin and alkoxysilane glycidyl ether are reacted at 40° C. to 180° C. to obtain the interface modifier.
3. Use of the interfacial modifier according to claim 1 in a silica / rubber composite material.
4. A white carbon black / rubber composite material, characterized in that: Its weight Including the following ingredients: 100 parts of rubber, 2-4 parts of interface modifier, 40-50 parts of white carbon black, 2 parts of antioxidant, 9.5-13.5 parts of vulcanization package.
5. The white carbon black / rubber composite material according to claim 4, characterized in that: The rubber is one or more of emulsion-polymerized styrene-butadiene rubber, solution-polymerized styrene-butadiene rubber, natural rubber, isoprene rubber, butadiene rubber, butyl rubber, and silicone rubber.
6. The white carbon black / rubber composite material according to claim 5, characterized in that: The antioxidant is one or more of antioxidant RD, antioxidant 4010NA, antioxidant 4010 and antioxidant 4020.
7. The white carbon black / rubber composite material according to claim 6, characterized in that: The vulcanization package comprises the following raw materials by weight: 5 parts of zinc oxide, 1 part of stearic acid, 2 to 5 parts of accelerator, and 1.5 to 2.5 parts of sulfur.
8. The white carbon black / rubber composite material according to claim 7, characterized in that: The accelerator is one or more of accelerator CZ, accelerator DZ, accelerator M, accelerator DM, accelerator NS, accelerator D and accelerator TT.
9. A method for preparing the white carbon black / rubber composite material according to claim 4, characterized in that the steps include: The rubber, interface modifier, white carbon black, antioxidant and vulcanization package in the formulated amount are mixed at 50° C. to 150° C. for 5 to 12 minutes, and hot-pressed vulcanized to obtain the rubber composite material.
10. A method for preparing the white carbon black / rubber composite material according to claim 9, characterized in that: The mixing conditions are: 80-120° C., 8-10 min.
Citation Information
Patent Citations
White carbon black / rubber composite material with low heat generation and high wear resistance as well as preparation method and application of white carbon black / rubber composite material
CN113321855A
Rubber composite material filled with white carbon black synergistically modified by end group functionalized liquid rubber and sulfydryl silane coupling agent and preparation method of rubber composite material
CN113652010A
Preparation method of sulfur-containing silane copolymer modified white carbon black-rubber composite material
CN113980366A
Silane polymer containing polyether chain segment, rubber composite material containing silane polymer and preparation method of rubber composite material