Resin microsphere as well as preparation method and application thereof

By optimizing the seed swelling polymerization method, resin microspheres with particle sizes of 4-9 μm and crosslinking degree of 30%-45% were prepared, and the problem of difficult control of crosslinking degree and particle size uniformity of resin microspheres in the prior art was solved. , improves its pressure resistance and reproducibility, and is suitable for high-efficiency chromatography separation.

CN119060231AActive Publication Date: 2024-12-03NANJING UNIV +1

Patent Information

Application Number
CN202310651871.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-06-02
Publication Date
2024-12-03
Estimated Expiration
2043-06-02

AI Technical Summary

Technical Problem

When preparing micron-scale styrene divinyl benzene resin microspheres, it is difficult to achieve high crosslinking, controllable and uniform particle size at the same time, resulting in poor pressure resistance and poor reproducibility of resin microspheres, which is difficult to Meet the requirements of chromatographic fillers.

Method used

The seed swelling polymerization method is used to optimize the composition and reaction conditions of the raw material phase, including the use of a variety of dispersants, emulsifiers and initiators, and the raw materials are added in batches, controlling the temperature and time, and gradually improving the crosslinking degree and particle size uniformity. Resin microspheres with particle size of 4-9 μm and crosslinking degree of 30%-45% were prepared.

Benefits of technology

It achieves high crosslinking degree and particle size uniformity of resin microspheres, improves its pressure resistance and product reproducibility, is suitable for chromatographic column fillers, and meets the needs of chromatographic separation effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060231A_ABST
    Figure CN119060231A_ABST
Patent Text Reader

Abstract

The invention discloses a resin microsphere as well as a preparation method and application thereof, the method is used for improving a dispersing agent used in a seed microsphere preparation process, and the size uniformity of the obtained seed microsphere can be effectively ensured; and in combination with the improvement in the swelling process of the seed microspheres, the finally prepared resin microspheres have a polydispersity coefficient of 1-1.2 and a particle size of 4-9 [mu] m.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a seed microsphere and a resin microsphere, and also provides a preparation method and application of the seed microsphere and the resin microsphere. Background Art

[0002] Micron-sized styrene divinylbenzene resin microspheres are a new type of functional material with the advantages of good sphericity, large specific surface area, and easy surface modification. They are one of the available fillers for chromatographic columns such as ion chromatography and liquid chromatography. When used as a chromatographic column filler, the cross-linking degree and uniformity of the particle size of the resin microspheres are important factors affecting their chromatographic separation effect, wherein the cross-linking degree is required to be at least not less than 25%. A higher cross-linking degree can ensure that the resin microspheres are not easy to swell and dissolve in organic matter, and can withstand greater pressure; and generally a certain range of particle sizes (usually 4 to 10 microns) need to be selected.

[0003] The seed swelling method is one of the most ideal methods for preparing monodisperse porous polymer microspheres. The seed swelling polymerization system usually consists of seed microspheres (or seed droplets), swelling agents, monomers (or monomer droplets), dispersed phases, initiators and stabilizers. In order to prepare cross-linked porous microspheres, cross-linking agents and porogens are also required. The specific method is to first introduce the swelling agent into the seed microspheres to activate the seed microspheres, then add the monomers to continue swelling, add the stabilizer after the swelling is completed, heat up and polymerize, and finally centrifuge the polymerization system. The obtained particles are extracted with appropriate solvents to obtain porous polymer microspheres.

[0004] However, the existing methods for preparing micron-sized styrene divinylbenzene resin microspheres usually have the following problems:

[0005] First, during the preparation process, if the prepared resin microspheres are expected to have a particle size suitable for use as chromatographic column fillers or have relatively good uniformity, the prepared resin microspheres usually have a problem of too low cross-linking (generally less than 10%). When the cross-linking is too low, the resin microspheres will have more internal channels, which may bring a large specific surface area, but will make the resin microspheres have poor pressure resistance and easy to collapse;

[0006] For example, the patent application document with application number 201110230790.9 discloses a method for preparing monodisperse microspheres of vinylpyrrolidone and divinylbenzene - swelling copolymerization method, in which polystyrene microsphere seeds are prepared by dispersion polymerization method, and comonomers such as N-vinylpyrrolidone and acrylic acid ester are introduced in the swelling copolymerization process to prepare the corresponding copolymer microspheres. The preparation process of this method has the following problems: (1) The solution addition time is relatively long (2-11h), and the solution added in this process may coagulate or react prematurely, and deteriorate. In addition, there are problems such as inconvenience in operation and difficulty in control; (2) The aforementioned problem of difficult control of operability will also affect the stability of product properties under the same conditions in different batches, that is, the reproducibility of the microspheres prepared by this method is not good; (3) The particle size of the microspheres synthesized by this method is concentrated between 20-80μm, and the cross-linking degree is not high enough, which is difficult to meet the requirements of chromatographic fillers.

[0007] Secondly, during the preparation process, if it is desired that the prepared resin microspheres have a higher degree of crosslinking, the particle size of the resin will gradually increase as the degree of crosslinking increases, and the particle size dispersion of the resin will increase, resulting in poor uniformity.

[0008] Therefore, the preparation of porous resin microspheres with high cross-linking degree, large particle size and uniform particle size has great research value and application prospects. Summary of the invention

[0009] 1. Problem to be solved

[0010] Based on the existing preparation methods of porous polymer microspheres, it is impossible to prepare porous polymer microspheres with high crosslinking degree, controllable and uniform particle size. One of the purposes of the present invention is to provide a preparation method of resin microspheres, which can improve the particle size uniformity and crosslinking degree of the obtained product by adopting a seed swelling polymerization method.

[0011] Based on one of the purposes of the present invention, the present invention also provides resin microspheres and particle groups thereof, as well as chromatographic fillers and chromatographic columns based on the resin microsphere particle groups.

[0012] 2. Technical solution

[0013] In order to solve the above problems, the technical solution adopted by the present invention is as follows:

[0014] [1] According to the purpose of the present invention, the present invention provides a method for preparing resin microspheres.

[0015] The process comprises the following steps:

[0016] A. Seed microsphere synthesis stage

[0017] A1 Prepare the raw materials phase 1:

[0018] The raw material phase 1 includes a solvent; and

[0019] at least two types of dispersants;

[0020] A2 prepares raw materials for phase 2:

[0021] The second raw material phase includes styrene and an initiator;

[0022] A3 seed microsphere synthesis:

[0023] The raw material phase 2 and the raw material phase 1 are added, and after the addition is completed, the reaction is carried out at 60-80° C. for 4 to 24 hours to obtain seed microspheres; preferably, the reaction is carried out at 65-75° C. for 4 to 24 hours to obtain seed microspheres;

[0024] B. Seed microsphere swelling stage

[0025] B1 prepare raw materials for phase 3:

[0026] The raw material phase three includes seed microspheres and an emulsifier;

[0027] B2 prepares raw materials phase 4:

[0028] The prepared raw material phase 4 includes styrene, divinylbenzene, a porogen, an emulsifier, an initiator and a surfactant.

[0029] B3 seed microsphere swelling 1:

[0030] Adding, swelling and reacting the raw material phase 3 and the raw material phase 4;

[0031] The adding is performed in N times, where N is an integer ≥2.

[0032] [1.1] According to the method for preparing resin microspheres of any embodiment of the first aspect of the present invention, in A1, the raw material phase 1 includes two dispersants of type 1 and type 2;

[0033] The type 1 dispersant is selected from any one or two of polyvinyl pyrrolidone and polyvinyl alcohol, wherein the molecular weight of the polyvinyl alcohol is ≥10000;

[0034] The second type of dispersant is selected from any one or more of polyacrylic acid, polyvinyl alcohol, ethyl cellulose, hydroxypropyl methylcellulose, and hydroxy calcium phosphate, wherein the molecular weight of the polyvinyl alcohol is less than 10,000.

[0035] [1.2] According to the method for preparing resin microspheres of any embodiment of the first aspect of the present invention, the mass ratio of the type 1 dispersant to the type 2 dispersant is (10-13): (0.5-1.5).

[0036] [1.3] According to the method for preparing resin microspheres of any embodiment of the first aspect of the present invention, A. in the seed microsphere synthesis stage, the emulsifier includes any one or more of sodium dodecylbenzene sulfonate and sodium dodecyl sulfate;

[0037] The initiator includes any one or more of azobisisobutyronitrile, azobisisoheptanenitrile, dimethyl azobisisobutyrate, benzoyl peroxide, and dibenzoyl peroxide.

[0038] [1.4] According to the method for preparing resin microspheres of any embodiment of the first aspect of the present invention, in the A. seed microsphere synthesis stage, the mass ratio of styrene, initiator, dispersant and solvent is (30-80): (1-3): (5-10): (300-600).

[0039] [1.5] According to the method for preparing resin microspheres of any embodiment of the first aspect of the present invention, in A3, the temperature when the raw material phase is added does not exceed 50 degrees Celsius, and preferably the temperature when the raw material phase is added is 30-50°C; after the addition of raw material phase one or raw material phase two is completed, the temperature is increased to enter the total reaction stage, the temperature of the total reaction stage is 60-80°C, preferably the temperature is 65-75°C, and the total reaction time is 4-24h.

[0040] [1.6] According to the method for preparing resin microspheres of any embodiment of the first aspect of the present invention, the adding in A3 is performed N times, and N is an integer ≥ 2;

[0041] The adding process includes:

[0042] The temperature during the addition does not exceed 50° C., and preferably the temperature during the addition is 30-50° C.; the interval time between the addition of the previous batch and the addition of the next batch is 10-120 minutes.

[0043] [1.7] According to the method for preparing resin microspheres of any embodiment of the first aspect of the present invention,

[0044] Adding the raw material phase 2 to the raw material phase 1 in N times;

[0045] After the addition of the second raw material phase is completed, the temperature is kept warm, and then the temperature is raised to 60-80°C through at least one heating-warming treatment, and the reaction is carried out at 60-80°C for 4-24 hours; preferably at 65-75°C for 4-24 hours;

[0046] Wherein, the heating-insulating treatment is performed by heating (heating rate not exceeding 10° C. / h) and the insulation time each time is 10 to 120 minutes.

[0047] [1.8] According to the method for preparing resin microspheres of any embodiment of the first aspect of the present invention, in the A. seed microsphere synthesis stage, the particle size of the prepared seed microspheres is 0.5-3 μm.

[0048] [1.9] According to the method for preparing resin microspheres of any embodiment of the first aspect of the present invention, in the A. seed microsphere synthesis stage, the particle size of the seed microspheres can be any value taken from any of the following numerical ranges: 0.5-3 μm, 0.5-2.5 μm, 0.5-2 μm, 0.5-1.5 μm, 0.5-1 μm, 1-3 μm, 1-2.5 μm, 1-2 μm, 1-1.5 μm, 1.5-3 μm, 1.5-2.5 μm, 1.5-2 μm, 2-3 μm, 2-2.5 μm, 2.5-3 μm;

[0049] [1.10] According to the method for preparing resin microspheres of any embodiment of the first aspect of the present invention, in the A. seed microsphere synthesis stage, the prepared seed microspheres have a polydispersity index of 1-1.2; preferably a polydispersity index of 1.02-1.1.

[0050] [1.11] According to the method for preparing resin microspheres of any embodiment of the first aspect of the present invention, B. in the seed microsphere swelling stage, the emulsifier comprises any one or more of sodium dodecylbenzene sulfonate and sodium dodecyl sulfate;

[0051] The initiator includes any one or more of azobisisobutyronitrile, azobisisoheptanenitrile, dimethyl azobisisobutyrate, benzoyl peroxide, and dibenzoyl peroxide;

[0052] The porogen includes any one or more of linear polystyrene, dibutyl phthalate, toluene, liquid paraffin, and polyvinyl acetate; preferably, the porogen includes any one or two of dibutyl phthalate and toluene.

[0053] [1.12] According to the method for preparing resin microspheres of any embodiment of the first aspect of the present invention, in B1, the mass percentages of seed microspheres and emulsifier are (0.5-2): (0.5-1.5).

[0054] [1.13] According to the method for preparing resin microspheres of any embodiment of the first aspect of the present invention, in B2, the raw material phase 4 is added to the raw material phase 3 in N times;

[0055] The raw material phase four includes a first raw material phase four and a second raw material phase four.

[0056] [1.14] According to the method for preparing resin microspheres of any embodiment of the first aspect of the present invention, the mass percentages of styrene, divinylbenzene, porogen, emulsifier and initiator in the first raw material phase four are (1.5-3):(1-4):(1-2):(0.5-1.5):(0.5-1.5).

[0057] [1.15] According to the method for preparing resin microspheres of any embodiment of the first aspect of the present invention, the mass percentages of styrene, divinylbenzene, emulsifier and initiator in the second raw material phase four are (1.5-3):(1-4):(0.5-1.5):(0.5-1.5).

[0058] [1.16] According to the method for preparing resin microspheres of any embodiment of the first aspect of the present invention, the ratio of the first raw material phase 4 to the raw material phase 3 is (1-2): (1-2); and / or,

[0059] The usage ratio of the first raw material phase four to the second raw material phase four is (1-2): (1-2).

[0060] [1.17] According to the method for preparing resin microspheres of any embodiment of the first aspect of the present invention, in B3, the first raw material phase 4 is first added, and the addition is performed N times, wherein N is an integer ≥ 2; preferably, N is an integer of 2 to 5;

[0061] Then, the second raw material phase four is added, and the addition is performed in N times, where N is an integer ≥ 2; preferably, N is an integer of 2 to 5.

[0062] [1.18] According to the method for preparing resin microspheres of any embodiment of the first aspect of the present invention, the process of adding the first raw material phase 4 comprises:

[0063] The temperature during addition does not exceed 50°C, preferably the temperature during addition is 30-50°C; the interval time between the addition of the previous batch and the addition of the next batch is 10-120 minutes;

[0064] and / or,

[0065] In the above B3, after the addition of the first raw material phase 4 is completed, swelling is carried out, and then the reaction is carried out at 60-80° C. for 4-24 hours; preferably, the reaction is carried out at a temperature of 65-75° C. for 4-24 hours.

[0066] [1.19] According to the method for preparing resin microspheres of any embodiment of the first aspect of the present invention, the process of adding the second raw material phase 4 comprises:

[0067] The temperature of each batch of the second raw material phase 4 when added does not exceed 50°C, preferably the temperature when added is 30-50°C; the interval time between the addition of the previous batch and the addition of the next batch is 10-120min;

[0068] and / or,

[0069] After the previous batch is added, the temperature is raised to 60-80°C (preferably 65-75°C), reacted for 10-120 minutes, and then cooled to no more than 50°C, preferably 30-50°C before the next batch is added;

[0070] After the addition of the second raw material phase 4 is completed, swelling is carried out, and then the reaction is carried out at 60-80° C. for 4-24 hours; preferably at a temperature of 65-75° C. for 4-24 hours.

[0071] [1.20] According to the method for preparing resin microspheres of any embodiment of the first aspect of the present invention, the mass ratio of the first raw material phase 4 added in each batch to the total mass of the first raw material phase 4 is 20 to 50 wt % calculated based on the mass of the first raw material phase 4;

[0072] and / or,

[0073] Calculated according to the mass of the second raw material phase four, the mass ratio of the amount of the second raw material phase four in each added batch to the total amount of the second raw material phase four is 20-50wt%.

[0074] [1.21] According to the method for preparing resin microspheres of any embodiment of the first aspect of the present invention, the particle size of the seed microspheres is 0.5-3 μm, and the polydispersity coefficient is 1-1.2; preferably, the polydispersity coefficient is 1.02-1.1.

[0075] The seed microspheres are prepared by [a seed microsphere and a preparation method thereof].

[0076] [2] Based on the first aspect of the purpose of the present invention, the second aspect of the present invention provides [a resin microsphere], wherein the resin microsphere is prepared by any of the above methods.

[0077] [2.1] According to any embodiment of the second aspect of the present invention, the resin microspheres have a particle size of 4-9 μm.

[0078] [2.2] According to the resin microspheres of any embodiment of the second aspect of the present invention, the particle size of the resin microspheres can be any value taken from any of the following numerical ranges: 4-9 microns, 4-8 microns, 4-7 microns, 4-6 microns, 4-5 microns, 5-9 microns, 5-8 microns, 5-7 microns, 5-6 microns, 6-9 microns, 6-8 microns, 6-7 microns, 7-9 microns, 7-8 microns, 8-9 microns.

[0079] [2.3] According to any embodiment of the second aspect of the present invention, the resin microsphere particles have a crosslinking degree of 30%-45%.

[0080] [2.4] According to the resin microspheres of any embodiment of the second aspect of the present invention, the degree of crosslinking of the resin microspheres can be any value within any of the following numerical ranges: 30-45%, 30-40%, 30-35%, 35-45%, 35-40%, 40-45%.

[0081] [2.5] According to any embodiment of the second aspect of the present invention, the resin microspheres have a polydispersity index of 1 to 1.2, preferably a polydispersity index of 1.02-1.1.

[0082] [2.6] According to the resin microspheres of any embodiment of the second aspect of the present invention, the polydispersity coefficient of the resin microspheres can be any value within any of the following numerical ranges: 1-1.2, 1.01-1.1, 1.02-1.09, 1.02-1.07, 1.02-1.05, 1.023-1.035, 1.035-1.045, 1.035-1.055, 1.035-1.065, 1.035-1.075, 1.035-1.085, 1.035-1.097.

[0083] [3] Based on the first or second aspect of the present invention, the third aspect of the present invention provides [a resin microsphere particle group], wherein the resin microsphere particle group is prepared by any of the above methods.

[0084] [3.1] According to any embodiment of the third aspect of the present invention, the resin microsphere particle group comprises resin microsphere particles with a particle size of 4-9 μm, accounting for 92.6-97.3 wt%.

[0085] [3.2] According to the resin microsphere particle group of any embodiment of the third aspect of the present invention, the particle size of the resin microsphere can be any value taken from any of the following numerical ranges: 4-9 microns, 4-8 microns, 4-7 microns, 4-6 microns, 4-5 microns, 5-9 microns, 5-8 microns, 5-7 microns, 5-6 microns, 6-9 microns, 6-8 microns, 6-7 microns, 7-9 microns, 7-8 microns, 8-9 microns.

[0086] [3.3] According to any embodiment of the third aspect of the present invention, the resin microsphere particle group comprises resin microsphere particles having a crosslinking degree of 30%-45%.

[0087] [3.4] According to the resin microsphere particle group of any embodiment of the third aspect of the present invention, the crosslinking degree of the resin microsphere can be any value within any of the following numerical ranges: 30-45%, 30-40%, 30-35%, 35-45%, 35-40%, 40-45%.

[0088] [3.5] According to any embodiment of the third aspect of the present invention, the resin microsphere particle group has a polydispersity index of 1 to 1.2, preferably a polydispersity index of 1.02-1.1.

[0089] [3.6] According to the resin microsphere particle group of any embodiment of the third aspect of the present invention, the polydispersity coefficient of the resin microsphere particles contained in the resin microsphere particle group can be any value taken from any of the following numerical ranges: 1-1.2, 1.01-1.1, 1.02-1.09, 1.02-1.07, 1.02-1.05, 1.023-1.035, 1.035-1.045, 1.035-1.055, 1.035-1.065, 1.035-1.075, 1.035-1.085, 1.035-1.097.

[0090] [4] Based on any one of the first to third aspects of the present invention, the fourth aspect of the present invention provides [a chromatographic filler], wherein the chromatographic filler comprises resin microspheres prepared by any of the above methods; and / or any one of the above resin microsphere particle groups.

[0091] [5] Based on any one of the first to fourth aspects of the present invention, the fifth aspect of the present invention provides [a chromatographic column], which comprises resin microspheres prepared by any of the above methods; and / or any one of the above resin microsphere particle groups; and / or, chromatographic filler. BRIEF DESCRIPTION OF THE DRAWINGS

[0092] Figure 1These are the resin microspheres prepared in Example 6A. DETAILED DESCRIPTION

[0093] The present disclosure may be more easily understood by reference to the following description in conjunction with the accompanying drawings and examples, all of which constitute a part of the present disclosure. It should be understood that the present disclosure is not limited to the specific products, methods, conditions or parameters described and / or shown herein. Further, the terms used herein are only used for the purpose of describing specific embodiments by way of example and are not intended to be limiting unless otherwise stated.

[0094] It should also be understood that, for the sake of clarity, certain features of the present disclosure may be described herein in the context of separate embodiments, but may also be provided in combination with each other in a single embodiment. That is, unless clearly incompatible or specifically not included, each separate embodiment is considered to be combinable with any other embodiment, and the combination is considered to represent another different embodiment. Conversely, for the sake of simplicity, the various features of the present disclosure described in the context of a single embodiment may also be provided individually or in any sub-combination. Finally, although a particular embodiment may be described as part of a series of steps or part of a more general structure, each step or substructure itself may also be considered to be an independent embodiment.

[0095] Unless otherwise indicated, it should be understood that each individual element in a list and each combination of individual elements in the list will be interpreted as a different embodiment. For example, a list of embodiments represented as "A, B, or C" should be interpreted to include embodiments "A", "B", "C", "A or B", "A or C", "B or C", or "A, B, or C".

[0096] In the present disclosure, the singular forms of the articles "a," "an," and "the" also include the corresponding plural references, and a reference to a specific value includes at least that specific value unless the context clearly indicates otherwise. Thus, for example, a reference to "a substance" is a reference to at least one of that substance and equivalents thereof.

[0097] The terms including ordinal numbers such as "first" and "second" can be used to explain various components or fluids, but these components and fluids are not limited by these terms. Therefore, without departing from the teachings of the present disclosure, these terms are only used to distinguish the component / fluid from another component / fluid.

[0098] When items are described by using the conjunction terms "... and / or...," etc., the description should be understood to include any one of the associated listed items and all combinations of one or more thereof.

[0099] In general, the use of the term "about" indicates an approximate value that may vary depending on the desired properties obtained by the disclosed subject matter, and will be interpreted in a context-dependent manner based on function. Therefore, one of ordinary skill in the art will be able to interpret a certain degree of difference on a case-by-case basis. In some cases, the number of significant figures used when expressing a particular value can be a representative technique for determining the difference allowed by the term "about". In other cases, a gradient in a range of values ​​can be used to determine the range of differences allowed by the term "about". Further, all ranges in this disclosure are inclusive and combinable, and reference to the values ​​stated in the range includes each value within the range.

[0100] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the invention belongs; the terms used herein and / or include any and all combinations of one or more of the associated listed items.

[0101] In order to demonstrate the technical solutions and advantages of the present invention, the technical solutions in the embodiments of the present invention will be fully described below.

[0102] A. Seed microsphere synthesis stage, the preparation method of the seed microsphere of the present invention comprises the following steps:

[0103] A1 Prepare the raw materials phase 1:

[0104] The raw material phase 1 includes a solvent; and

[0105] at least two types of dispersants;

[0106] A2 prepares raw materials for phase 2:

[0107] The second raw material phase includes styrene and an initiator;

[0108] A3 seed microsphere synthesis:

[0109] The second raw material phase is added to the first raw material phase and reacted to obtain seed microspheres.

[0110] The reactive monomers styrene and divinylbenzene (80 wt%) in the raw material phase are preferably subjected to a deblocking treatment before use to remove the polymerization inhibitors that may exist in the reactive monomers. Generally, styrene and divinylbenzene can be washed with sodium hydroxide solution to remove the polymerization inhibitors, and then the lower aqueous solution is separated with a separatory funnel until the pH of the aqueous solution is neutral.

[0111] The type of solvent in the raw material phase is not particularly limited. For example, any one of water, ethanol, ethylene glycol methyl ether, or any combination thereof can be used as the solvent.

[0112] The type of initiator in the raw material phase is not particularly limited. For example, any one of azobisisobutyronitrile, azobisisoheptanenitrile, dimethyl azobisisobutyrate, benzoyl peroxide, dibenzoyl peroxide, etc., or any combination thereof can be used;

[0113] As the dispersant in the raw material phase, the type of dispersant and the way of use will affect the uniformity of the particle size of the prepared resin microspheres. Therefore, the present invention requires that the dispersant in the raw material phase retains two different types, one selected from one of the following types 1, and the other selected from one of the following types 2:

[0114] The type 1 dispersant is selected from any one of polyvinyl pyrrolidone and polyvinyl alcohol (molecular weight ≥ 10000); for example, the molecular weight of polyvinyl alcohol available on the market can be 47000, 57000, 66000, 89000, 98000, 130000, 145000, 205000;

[0115] The type II dispersant is selected from any one of polyacrylic acid, polyvinyl alcohol (molecular weight <10,000), ethyl cellulose, hydroxypropyl methylcellulose, and calcium hydroxyphosphate; for example, the molecular weight of polyvinyl alcohol available on the market can be 3,200, 5,000, 7,000, 9,000, or 9,900.

[0116] Furthermore, it should be further explained that, in fact, the complexity of the dispersant composition will affect the difficulty of controlling the subsequent reaction. Therefore, in order to meet the requirements of uniformity of the particle size of the prepared resin microspheres and easy control of the subsequent reaction, it is recommended that the dispersant combination type is composed of two different types, one from the above-mentioned type 1 and the other from the above-mentioned type 2. For example:

[0117] Dispersant Combination Type Type 1 Type 2 Ratio (mass ratio) 1 Polyvinylpyrrolidone Polyvinyl alcohol 15:1 2 Polyvinylpyrrolidone acrylic acid 15:2 3 Polyvinyl alcohol Ethyl cellulose 7:1 4 Polyvinylpyrrolidone Hydroxypropyl methylcellulose 8:1 5 Polyvinyl alcohol Hydroxypropyl methylcellulose 7.5:1

[0118] Furthermore, the added amounts of the styrene, initiator, dispersant and solvent are calculated according to the mass ratio of (30-80):(1-3):(5-10):(300-600); the preferred ratio is (50-70):(1.5-2.5):(6.5-8.5):(400-550).

[0119] The reference process for preparing the raw material phase A1 is as follows: dissolve the dispersant in the solvent, introduce nitrogen to drive out oxygen, stir (speed controlled at 200-350r / min) and maintain the temperature (30-50 degrees Celsius) stable, so that the solvent and the dispersant are fully mixed;

[0120] The reference process for preparing the second raw material phase A2 is as follows: weigh a certain amount of deblocked styrene, add the initiator to the styrene monomer, stir to dissolve, and disperse evenly; in order to make the initiator easier to dissolve in the styrene monomer, you can choose to put the styrene monomer into a beaker and heat it in a water bath.

[0121] The reference process for synthesizing A3 seed microspheres is as follows: add the raw material phase 2 prepared in step A2 to the raw material phase 1 prepared in step A1 (the temperature needs to be maintained at 30-50°C during this process), heat up (heating rate not exceeding 10°C / h) to 60-80°C, stir during the reaction, and react at 60-80°C for 4-24h; after the reaction, use ethanol and acetone to ultrasonically wash the obtained seed microspheres, centrifuge and dry.

[0122] In order to further pursue the uniformity of the particle size and the degree of cross-linking of the final seed microspheres, without considering the difficulty of controlling the accuracy of the reaction process, another reference process for synthesizing A3 seed microspheres is as follows:

[0123] Add the raw material phase 2 prepared in step A2 into the raw material phase 1 prepared in step A1 in N batches. During the addition of each batch of raw material phase 2 to raw material phase 1, the temperature should be maintained at 30-50°C with stirring;

[0124] Calculated according to the mass of the raw material phase 2, the mass ratio of each batch of the raw material phase 2 to the total amount of the raw material phase 2 is 20-50wt%; the interval time between the addition of the previous batch and the addition of the next batch is 10-120min.

[0125] After all batches of raw material phase II are added, the mixture is kept at the addition temperature for 10-120 minutes, and then the temperature is raised and kept, and finally the temperature is raised to 60-80 degrees Celsius, and the reaction is carried out at 60-80 degrees Celsius for 4-24 hours, and the reaction is completed. After the reaction is completed, the porogen is removed by ultrasonic washing, centrifugation, and Soxhlet extraction to obtain the final seed microspheres.

[0126] For the heating-keeping treatment, the heating rate generally used for reference is no more than 10°C / h, for example, the heating rate is 2°C / h, 3°C / h, 4°C / h, 5°C / h, 6°C / h, 7°C / h, 8°C / h, 9°C / h;

[0127] The insulation treatment temperatures described therein for reference are 50°C, 53°C, 55°C, 57°C, 60°C, 62°C, 65°C, 67°C, 70°C, 73°C, etc.;

[0128] The insulation treatment time described for reference is 5min, 8min, 10min, 15min, 20min, 25min, 30min, 35min, 40min, 45min, 50min, 55min, 60min, 65min, 70min, 75min, 80min, 85min, 90min, 95min, 100min, 105min, 110min, 115min, 120min, etc.;

[0129] For example, after all batches of raw materials are added to phase II at 40°C and the mixture is kept at 40°C for half an hour, the following heating-keeping process is performed for reference: the temperature is gradually increased to 50°C at a rate of 10°C / h, and the mixture is kept at 50°C for half an hour. The temperature is then gradually increased to 60°C at a rate of 10°C / h, and the mixture is kept at 60°C for half an hour.

[0130] After the heating-insulation treatment process as provided for reference above is completed, the subsequent treatment can be continued in the following exemplified manner to prepare the final seed microspheres: continue to increase the temperature to 75°C at a rate of 10°C / h, react at 75°C for 20h, and after the reaction is completed, ultrasonic washing, centrifugation, and Soxhlet extraction are performed to remove the porogen to obtain the final seed microspheres.

[0131] Finally, based on the preparation method provided by the present invention, the present invention can also provide seed microspheres, and the particle size of the prepared seed microspheres is 0.5-3 μm.

[0132] B. Synthesis of resin microspheres. The method for preparing resin microspheres of the present invention comprises the following steps:

[0133] B1 prepare raw materials for phase 3:

[0134] The raw material phase three includes seed microspheres and an emulsifier;

[0135] B2 prepares raw materials phase 4:

[0136] The prepared raw material phase 4 includes styrene, divinylbenzene, a porogen, an emulsifier, and an initiator.

[0137] B3 seed microsphere swelling:

[0138] Allowing the raw material phase 3 and the raw material phase 4 to undergo an addition and swelling total reaction;

[0139] The adding is performed in N times, where N is an integer ≥2.

[0140] The type of emulsifier in the raw material phase is not particularly limited. For example, any one of sodium dodecylbenzene sulfonate, sodium dodecyl sulfate, etc., or any combination thereof can be used as an emulsifier;

[0141] The type of porogen in the raw material phase is not particularly limited. For example, any one of linear polystyrene, dibutyl phthalate, toluene, liquid paraffin, polyvinyl acetate, etc., or any combination thereof can be used as the porogen; and from the perspective of improving the system stability during the reaction, the porogen preferably includes dibutyl phthalate and toluene, but does not include linear polystyrene, liquid paraffin, and polyvinyl acetate.

[0142] Furthermore, in B1, the mass percentages of seed microspheres and emulsifier are calculated as (0.5-2):(0.5-1.5); a more preferred ratio is (0.8-1.6):(0.8-1.2).

[0143] In B2, the mass percentages of seed microspheres, styrene, divinylbenzene, porogen, emulsifier and initiator are (0.5-2):(1.5-3):(1-4):(1-2):(0.5-1.5):(0.5-1.5); the more preferred ratios are (0.8-1.6):(2-2.5):(1.5-3):(1.2-1.8):(0.8-1.2):(0.6-1.2).

[0144] The reference process for preparing the raw material phase 3 in step B1 is as follows: weigh a certain amount of prepared seed microspheres, add them to an aqueous solution containing an emulsifier, disperse them by ultrasonication, and then stir them evenly.

[0145] The reference process for preparing raw material phase 4 of B2 is as follows: add styrene, divinylbenzene, porogen and initiator to an aqueous solution containing an emulsifier, and fully ultrasonically emulsify the solution. The ultrasonic time is 30-60 minutes and the temperature is controlled at 20-40 degrees Celsius.

[0146] The reference process for swelling B3 seed microspheres is as follows: Add the raw material phase 4 prepared in step B2 into the raw material phase 3 prepared in step B1 in N batches. During the addition of each batch of raw material phase 4 to raw material phase 3, the temperature must be maintained at 30-50°C, accompanied by stirring;

[0147] Calculated according to the mass of the raw material phase 4, the mass ratio of each batch of the raw material phase 4 to the total amount of the raw material phase 4 is 20-50wt%; the interval time between the addition of the previous batch and the addition of the next batch is 10-120min.

[0148] After all batches of raw materials in phase 4 are added, the temperature is raised (the heating rate does not exceed 10°C / h) to 60-80 degrees Celsius, and the reaction is carried out at 60-80 degrees Celsius for 4-24 hours. After the reaction, the porogen is removed by ultrasonic washing, centrifugation, and Soxhlet extraction to obtain the final resin microspheres.

[0149] While simultaneously considering the pursuit of uniformity of particle size and degree of crosslinking of the final resin microspheres, the reference process for preparing the raw material phase 4 in step B2 is as follows:

[0150] dividing the raw material phase 4 into a first raw material phase 4 and a second raw material phase 4; and,

[0151] The usage ratio of the first raw material phase 4 to the raw material phase 3 is (1-2): (1-2);

[0152] The usage ratio of the first raw material phase 4 to the second raw material phase 4 is (1-2): (1-2).

[0153] As the first raw material phase 4, it includes styrene, divinylbenzene, a porogen, an emulsifier, and an initiator, and the mass percentages of the styrene, divinylbenzene, a porogen, an emulsifier, and an initiator are (1.5-3):(1-4):(1-2):(0.5-1.5):(0.5-1.5);

[0154] The second raw material phase four includes styrene, divinylbenzene, an emulsifier and an initiator, and the mass percentages of the styrene, divinylbenzene, emulsifier and initiator are (1.5-3):(1-4):(0.5-1.5):(0.5-1.5).

[0155] In addition, based on the above B2 preparation of raw materials phase 4, another reference process for B3 seed microsphere swelling is as follows:

[0156] Add the first raw material phase 4 prepared in step B2 into the raw material phase 3 prepared in step B1 in N batches. During the addition of each batch of the first raw material phase 4 to the raw material phase 3, the temperature must be maintained at 30-50°C with stirring;

[0157] Calculated according to the mass of the first raw material phase 4, the mass ratio of each batch of the first raw material phase 4 to the total mass of the first raw material phase 4 is 20-50wt%; the interval time between the addition of the previous batch and the next batch is 10-120min.

[0158] After all batches of the first raw material phase four are added, keep warm at the addition temperature for 8 to 16 hours, then raise the temperature to 60 to 80 degrees Celsius, react at 60 to 80 degrees Celsius for 2 to 4 hours, and then proceed to the second raw material phase four addition stage after the reaction is completed.

[0159] The reference addition process of the second raw material phase 4 is as follows: the second raw material phase 4 prepared in step B2 is added to the raw material phase 3 prepared in step B1 in N batches. During the addition of each batch of the second raw material phase 4 to the raw material phase 3, the temperature must be maintained at 30-50°C, accompanied by stirring;

[0160] The time interval from the completion of adding the second raw material phase 4 of the previous batch to the raw material phase 3 to the start of adding the second raw material phase 4 of the next batch to the raw material phase 3 is 10-120 minutes; and during this time interval, there is a process of heating-keeping-cooling treatment to ensure that the temperature of each batch of the second raw material phase 4 is 30-50°C when adding. This cycle is repeated until all batches of the first raw material phase 4 are added;

[0161] Finally, the temperature is raised (the heating rate does not exceed 10°C / h) to 60-80°C, and the swelling reaction is carried out at 60-80°C for 4-24 hours; after the reaction, the porogen is removed by ultrasonic washing, centrifugation, and Soxhlet extraction to obtain the final resin microspheres. Finally, the particle size of the prepared resin microspheres is 4-9 μm.

[0162] For the heating-keeping-cooling treatment, the generally referenced heating rate is no more than 10°C / h, for example, the heating rate is 2°C / h, 3°C / h, 4°C / h, 5°C / h, 6°C / h, 7°C / h, 8°C / h, 9°C / h;

[0163] The heat preservation treatment temperature for reference can be any temperature between 60 and 80°C, such as 65°C, 67°C, 70°C, 73°C, etc.

[0164] The insulation treatment time for reference may be any time selected from 5-60 min, for example, 5 min, 8 min, 10 min, 15 min, 20 min, 25 min, 30 min, 35 min, 40 min, 45 min, 50 min, 55 min, 60 min, etc.

[0165] For example, after the second raw material phase 4 of the previous batch is added at 40°C and kept at 40°C for half an hour, the following heating-keeping-cooling process is performed for reference: increase the temperature to 70°C at a rate of 5°C / h, keep at 70°C for half an hour, and then cool to 40°C.

[0166] After the heating-keeping-cooling process is completed, the next batch of the second raw material phase 4 can be added at 40° C., and the cycle is repeated until the last batch of the second raw material phase 4 is added, and then the temperature is kept at 40° C. for half an hour;

[0167] Finally, the temperature is raised (the heating rate does not exceed 5°C / h) to 70 degrees Celsius, and the total reaction is carried out at 70 degrees Celsius for 4-24 hours. After the reaction is completed, the porogen is removed by ultrasonic washing, centrifugation, and Soxhlet extraction to obtain the final resin microspheres.

[0168] Based on the preparation method provided by the present invention, the present invention can also provide resin microsphere particles: the particle size of the resin microsphere particles is 4-9 μm; and / or,

[0169] The cross-linking degree of the resin microsphere particles is 30%-45%.

[0170] Based on the preparation method provided by the present invention, the present invention can also provide a resin microsphere particle group: the resin microsphere particle group includes resin microsphere particles with a particle size of 4-9 μm, accounting for 92.6-97.3wt%; and / or,

[0171] The resin microsphere particle group comprises resin microsphere particles having a crosslinking degree of 30%-45%; and / or,

[0172] The polydispersity coefficient of the resin microsphere particles contained in the resin microsphere particle group is 1 to 1.2, and the preferred dispersion coefficient is 1.023-1.097.

[0173] Based on the preparation method provided by the present invention, the present invention can also provide a chromatographic filler: the chromatographic filler comprises resin microsphere particles and / or a group of resin microsphere particles prepared by any of the above methods.

[0174] Based on the preparation method provided by the present invention, the present invention can also provide a chromatographic column: the chromatographic column comprises resin microsphere particles, and / or a group of resin microsphere particles, and / or chromatographic fillers prepared by any of the above methods.

[0175] Example 1

[0176] Deblocking treatment:

[0177] After washing styrene and divinylbenzene three times with 1 M sodium hydroxide solution, the pH of the washing solution was close to neutral.

[0178] Raw material phase 1: Add 350mL ethanol, 100mL water, and 100mL ethylene glycol methyl ether to a 1000mL three-necked flask, place in a water bath, maintain the water temperature at 40 degrees Celsius, turn on stirring, and stir at a speed of 200r / min. After stirring for 5 minutes, weigh 9g polyvinyl pyrrolidone and 0.6g polyvinyl alcohol (molecular weight of 5000) and add them to the mixed solution;

[0179] Raw material phase 2: Weigh 85g of deblocked styrene into a beaker, then weigh 2.5g of azobisisobutyronitrile and add it to the weighed styrene. Place the beaker in a 50-degree water bath and stir with a glass rod to dissolve the azobisisobutyronitrile;

[0180] Synthesis of seed microspheres (seed balls): Keep the water temperature at 40 degrees Celsius, add the prepared raw material phase 2 into the three-necked flask containing the raw material phase 1, and stir during the period. The stirring speed is 350r / min. After the addition is completed, keep warm at 40 degrees Celsius for half an hour, then heat to 45 degrees Celsius, keep warm at 45 degrees Celsius for half an hour, continue to heat to 50 degrees Celsius, keep warm at 50 degrees Celsius for half an hour, continue to heat and keep warm (each time the temperature rises by 5 minutes, and then keeps warm for half an hour) until 75 degrees Celsius, and react at 75 degrees Celsius for 20 hours.

[0181] After the reaction, centrifuge and wash three times with ethanol and acetone respectively. The washing process is as follows: after adding ethanol / acetone, ultrasonic dispersion for 5 minutes, and then centrifuge at a speed of 3000r / min and a centrifugal time of 2min.

[0182] Transfer the washed balls to a watch glass and dry them in an oven at 60 degrees Celsius. Store the dried balls in a ziplock bag to prevent them from absorbing water.

[0183] The average particle size of the prepared seed microspheres (seed microspheres-1) is 1.9 μm, and the polydispersity coefficient is 1.029.

[0184] Example 2

[0185] Deblocking treatment:

[0186] After washing styrene and divinylbenzene three times with 1 M sodium hydroxide solution, the pH of the washing solution was close to neutral.

[0187] Raw material phase 1: Add 350 mL of ethanol, 100 mL of water, and 100 mL of ethylene glycol methyl ether to a 1000 mL three-necked flask, place in a water bath, maintain the water temperature at 40 degrees Celsius, turn on stirring, and stir at a speed of 200 r / min. After stirring for 5 minutes, weigh 7 g of polyvinyl pyrrolidone and 1 g of polyvinyl alcohol (molecular weight of 5000) and add them to the mixed solution.

[0188] Raw material phase 2: Weigh 85g of deblocked styrene into a beaker, then weigh 2.1g of azobisisobutyronitrile and add it to the weighed styrene. Place the beaker in a 50-degree water bath to dissolve the azobisisobutyronitrile;

[0189] Synthesis of seed microspheres (seed balls): Keep the water temperature at 40 degrees Celsius, add the prepared raw material phase 2 into the three-necked flask containing the raw material phase 1, and stir during the period. The stirring speed is 400r / min. After the addition is completed, keep warm at 40 degrees Celsius for half an hour, then heat to 45 degrees Celsius, keep warm at 45 degrees Celsius for half an hour, continue to heat to 50 degrees Celsius, keep warm at 50 degrees Celsius for half an hour, continue to heat and keep warm (each time the temperature rises by 5 minutes, and then keeps warm for half an hour) until 75 degrees Celsius, and react at 75 degrees Celsius for 20 hours.

[0190] After the reaction, centrifuge and wash three times with ethanol and acetone respectively. The washing process is as follows: after adding ethanol / acetone, ultrasonic dispersion for 5 minutes, and then centrifuge at a speed of 3000r / min and a centrifugal time of 2min.

[0191] Transfer the washed balls to a watch glass and dry them in an oven at 60 degrees Celsius. Store the dried balls in a ziplock bag to prevent them from absorbing water.

[0192] The prepared seed microspheres (seed microspheres-2) have a particle size of 2.3 μm and a polydispersity coefficient of 1.039.

[0193] Example 3 (Ball-3)

[0194] Deblocking treatment:

[0195] After washing styrene and divinylbenzene three times with 1 M sodium hydroxide solution, the pH of the washing solution was close to neutral.

[0196] Raw material phase 1: Add 350 mL ethanol, 100 mL water, and 60 mL ethylene glycol methyl ether to a 1000 mL three-necked flask, place in a water bath, maintain the water temperature at 40 degrees Celsius, turn on stirring, and stir at a speed of 200 r / min. After stirring for 5 minutes, weigh 8 g polyvinyl pyrrolidone and 0.9 g hydroxypropyl methylcellulose and add them to the mixed solution.

[0197] Raw material phase 2: Weigh 85g of deblocked styrene into a beaker, then weigh 2.5g of azobisisobutyronitrile and add it to the weighed styrene. Place the beaker in a 50-degree water bath to dissolve the azobisisobutyronitrile;

[0198] Synthesis of seed microspheres (seed balls): Keep the water temperature at 40 degrees Celsius, add the prepared raw material phase 2 into the three-necked flask containing the raw material phase 1, and stir during the period. The stirring speed is 400r / min. After the addition is completed, keep warm at 40 degrees Celsius for half an hour, then heat to 45 degrees Celsius, keep warm at 45 degrees Celsius for half an hour, continue to heat to 50 degrees Celsius, keep warm at 50 degrees Celsius for half an hour, continue to heat and keep warm (each time the temperature rises by 5 minutes, and then keeps warm for half an hour) until 75 degrees Celsius, and react at 75 degrees Celsius for 20 hours.

[0199] After the reaction, centrifuge and wash three times with ethanol and acetone respectively. The washing process is as follows: after adding ethanol / acetone, ultrasonic dispersion for 5 minutes, and then centrifuge at a speed of 3000r / min and a centrifugal time of 2min.

[0200] Transfer the washed balls to a watch glass and dry them in an oven at 60 degrees Celsius. Store the dried balls in a ziplock bag to prevent them from absorbing water.

[0201] The prepared seed microspheres (seed microspheres-3) have a particle size of 2.2 μm and a polydispersity coefficient of 1.076.

[0202] Example 4 (Ball-4)

[0203] Deblocking treatment:

[0204] After washing styrene and divinylbenzene three times with 1 M sodium hydroxide solution, the pH of the washing solution was close to neutral.

[0205] Raw material phase 1: Add 350 mL ethanol, 100 mL water, and 60 mL ethylene glycol methyl ether to a 1000 mL three-necked flask, put it in a water bath, maintain the water temperature at 40 degrees Celsius, turn on the stirring, and stir at a speed of 200 r / min. After stirring for 5 minutes, weigh 7.5 g polyvinyl alcohol (molecular weight is 89000) and 1 g hydroxypropyl methylcellulose and add them to the mixed solution.

[0206] Raw material phase 2: Weigh 85g of deblocked styrene into a beaker, then weigh 2.5g of azobisisobutyronitrile and add it to the weighed styrene. Place the beaker in a 50-degree water bath to dissolve the azobisisobutyronitrile;

[0207] Synthesis of seed microspheres (seed balls): Keep the water temperature at 40 degrees Celsius, add the prepared raw material phase 2 into the three-necked flask containing the raw material phase 1, and stir during the period. The stirring speed is 400r / min. After the addition is completed, keep warm at 40 degrees Celsius for half an hour, then heat to 45 degrees Celsius, keep warm at 45 degrees Celsius for half an hour, continue to heat to 50 degrees Celsius, keep warm at 50 degrees Celsius for half an hour, continue to heat and keep warm (each time the temperature rises by 5 minutes, and then keeps warm for half an hour) until 75 degrees Celsius, and react at 75 degrees Celsius for 20 hours.

[0208] After the reaction, centrifuge and wash three times with ethanol and acetone respectively. The washing process is as follows: after adding ethanol / acetone, ultrasonic dispersion for 5 minutes, and then centrifuge at a speed of 3000r / min and a centrifugal time of 2min.

[0209] Transfer the washed balls to a watch glass and dry them in an oven at 60 degrees Celsius. Store the dried balls in a ziplock bag to prevent them from absorbing water.

[0210] The prepared seed microspheres (seed microspheres-3) have a particle size of 1.9 μm and a polydispersity coefficient of 1.091.

[0211] Comparative Example 1

[0212] This comparative example is basically the same as Example 3, except that:

[0213] Comparative sample-1: 8 g of polyvinyl pyrrolidone was weighed from the raw material phase 1 and added to the mixed solution, and no hydroxypropyl methylcellulose was added. The rest was the same as in Example 3; finally, the particle size of the prepared seed microspheres (comparative sample-1) was 2.4 μm; and the polydispersity coefficient was 1.232.

[0214] Comparative sample-2: 0.9 g of hydroxypropyl methylcellulose was weighed from the raw material phase 1 and added to the mixed solution. No polyvinyl pyrrolidone was added, and the rest was the same as in Example 3. Finally, the particle size of the prepared seed microspheres (comparative sample-2) was 6.6 μm, and the polydispersity coefficient was 1.319.

[0215] Comparative sample-3: 11 g of polyvinyl pyrrolidone and 0.9 g of hydroxypropyl methylcellulose were weighed from the raw material phase 1 and added to the mixed solution, and the rest was the same as in Example 3; finally, the particle size of the prepared seed microspheres (comparative sample-3) was 1.8 μm; and the polydispersity coefficient was 1.205.

[0216] Comparative sample-4:

[0217] In the raw material phase 1-1, half of the amount of ethanol, water, and ethylene glycol methyl ether solvent mixed solution (350 mL ethanol, 100 mL water, 100 mL ethylene glycol methyl ether) was taken, and 8 g of polyvinyl pyrrolidone was weighed and added to the mixed solution in the manner of Example 3;

[0218] In the raw material phase 1-2, take the other half amount of ethanol, water, ethylene glycol methyl ether solvent mixed solution (350mL ethanol, 100mL water, 100mL ethylene glycol methyl ether), and weigh 0.9g hydroxypropyl methylcellulose and add it to the mixed solution in the manner of Example 3;

[0219] The preparation of raw material phase 2 is the same as in Example 3;

[0220] Synthesis of seed microspheres: According to the method of Example 3, the prepared raw material phase 2 was added to the three-necked flask containing the raw material phase 1, accompanied by stirring during the period, the stirring speed of the stirring was 350r / min, and after the addition was completed;

[0221] The temperature was raised as in Example 3, the stirring speed was controlled, and the raw material phase 1-2 was added in batches before each heating. The rest was the same as in Example 3. Finally, the particle size of the prepared seed microspheres (comparative sample 3) was 2.0 μm, and the polydispersity coefficient was 1.174.

[0222] Example 5

[0223] In this example, the seed microspheres prepared in the example, i.e., seed microspheres-1, were used to prepare resin microspheres. The specific steps are as follows:

[0224] Raw material phase 3: Add 150 mL ultrapure water to a 500 mL three-necked flask, weigh 1.5 g sodium dodecyl sulfonate and add it to the water, turn on the stirring at a speed of 200 r / min. After the sodium dodecylbenzene sulfonate is dissolved, weigh 3 g of the bulbs and add them to the solution.

[0225] Ultrasonicate the three-necked flask for 40 minutes to evenly disperse the bulbs. Place the three-necked flask containing the bulbs in a water bath, maintain the temperature at 40 degrees Celsius, and use mechanical stirring at a stirring speed of 350 r / min.

[0226] Raw material phase 4:

[0227] The first portion: weigh 1g of sodium dodecyl sulfate and add it to 100mL of water, add 4g of styrene, 8g of divinylbenzene (purity 80%), 2mL of dibutyl phthalate, and 2mL of toluene, and disperse by ultrasonic. Take the liquid and observe it under a microscope until there are no obvious oil droplets. Then add 1.5g of benzoyl peroxide and 0.4g of azobisisobutyronitrile and disperse it evenly by ultrasonic.

[0228] The second batch: weigh 0.5g sodium dodecyl sulfate and add it to 50mL water, add 2g styrene and 4g divinylbenzene (purity 80%), disperse by ultrasonic, observe the liquid under a microscope until there are no obvious oil drops, then add 0.7g benzoyl peroxide and disperse by ultrasonic.

[0229] Swelling of seed microspheres: add 40 mL of the first raw material phase 4 to the raw material phase 3, stir for 10 minutes, then add 30 mL of the first raw material phase 4 to the raw material phase 3, stir for half an hour, then add the remaining 30 mL of the first raw material phase 4 and swell for 12 hours;

[0230] After the swelling is completed, the temperature is raised to 70 degrees Celsius and the reaction is carried out for 2 hours;

[0231] Then, cool down to 50 degrees Celsius;

[0232] Continue to add 20 mL of the second raw material phase four, stir at 50 degrees Celsius for 10 minutes, raise the temperature to 70 degrees Celsius and react for half an hour; then lower the temperature to 50 degrees Celsius, add 10 mL of the second raw material phase four, maintain at 50 degrees Celsius for 10 minutes, raise the temperature to 70 degrees Celsius and react for half an hour; repeat the above process until the addition of raw material phase four is complete.

[0233] After the addition of raw material phase 4 is completed, the temperature is raised to 70 degrees Celsius, the reaction is carried out for 10 hours, and the heating is stopped.

[0234] After washing with ethanol for several times, the mixture was extracted and dried at 50 degrees Celsius to constant weight. The particle size of the resin microspheres was measured to be 4.3 μm, the polydispersity coefficient was 1.037, and the cross-linking degree was 41%.

[0235] Example 6

[0236] In this example, the seed microspheres prepared in the example, i.e., seed microspheres-2, were used to prepare resin microspheres. The specific steps are as follows:

[0237] Raw material phase 3: Add 150 mL ultrapure water to a 500 mL three-necked flask, weigh 1.5 g sodium dodecyl sulfonate and add it to the water, turn on the stirring at a speed of 200 r / min. After the sodium dodecylbenzene sulfonate is dissolved, weigh 2.5 g of the bulbs and add them to the solution.

[0238] Ultrasonicate the three-necked flask for 40 minutes to evenly disperse the bulbs. Place the three-necked flask containing the bulbs in a water bath, maintain the temperature at 40 degrees Celsius, and use mechanical stirring at a stirring speed of 400 r / min.

[0239] Raw material phase 4:

[0240] The first part: weigh 1g sodium dodecyl sulfonate and add it to 100mL water, add 3.5g styrene, 7g divinylbenzene (purity 65%), 2mL dibutyl phthalate, 2mL toluene, and disperse by ultrasonic. Take the liquid and observe it under a microscope until there are no obvious oil drops. Then add 1.2g benzoyl peroxide and 0.3g azobisisobutyronitrile and disperse by ultrasonic.

[0241] The second portion: weigh 0.5g sodium dodecyl sulfate and add it to 50mL water, add 1.2g styrene and 2.3g divinylbenzene (purity 80%), disperse by ultrasonic, observe the liquid under a microscope until there are no obvious oil drops, then add 0.4g benzoyl peroxide and disperse by ultrasonic evenly.

[0242] Swelling of seed microspheres: add 40 mL of the first raw material phase 4 to the raw material phase 3, stir for 10 minutes, then add 30 mL of the first raw material phase 4 to the raw material phase 3, stir for half an hour, then add the remaining 30 mL of the first raw material phase 4 and swell for 12 hours;

[0243] After the swelling is completed, the temperature is raised to 70 degrees Celsius and the reaction is carried out for 2 hours;

[0244] Then, cool down to 50 degrees Celsius;

[0245] Continue to add 20 mL of the second raw material phase four, stir at 50 degrees Celsius for 10 minutes, raise the temperature to 70 degrees Celsius and react for half an hour; then lower the temperature to 50 degrees Celsius, add 10 mL of the second raw material phase four, maintain at 50 degrees Celsius for 10 minutes, raise the temperature to 70 degrees Celsius and react for half an hour; repeat the above process until the addition of raw material phase four is complete.

[0246] After the addition of raw material phase 4 is completed, the temperature is raised to 70 degrees Celsius, the reaction is carried out for 10 hours, and the heating is stopped.

[0247] After washing with ethanol for several times, extraction was performed and drying was performed at 50 degrees Celsius to constant weight to obtain resin microspheres 6-A.

[0248] In addition, the samples of resin microspheres 6-B, 6-C and 6-D were prepared in the same manner as the steps of resin microspheres 6-A. The properties of the samples obtained are shown in Table 1:

[0249] Average particle size μm Polydispersity coefficient Degree of crosslinking Resin microspheres 6-A 5.3 1.046 38% Resin microspheres 6-B 5.5 1.049 37% Resin microspheres 6-C 5.4 1.039 36% Resin microspheres 6-D 5.3 1.043 37%

[0250] Comparative Example 2

[0251] Comparative Sample-5-A:

[0252] The preparation of raw material phase 3 is the same as in Example 6;

[0253] The preparation of raw material phase 4 is the same as in Example 6;

[0254] Swelling of seed microspheres:

[0255] At 40 degrees Celsius, the first raw material phase 4 was added dropwise to the raw material phase 3 for 5 hours, and then the temperature was raised to 45 degrees Celsius and kept at 45 degrees Celsius for 8 hours;

[0256] After the swelling is completed, the temperature is raised to 70 degrees Celsius and the reaction is carried out for 2 hours;

[0257] Then, the temperature was lowered to 50 degrees Celsius, and the second portion of the raw material phase 4 was added dropwise for 5 hours, and then kept at 50 degrees Celsius for 5 hours;

[0258] After the swelling was completed, the temperature was raised to 70 degrees Celsius, the reaction was carried out for 5 hours, and the heating was stopped to obtain the resin microsphere comparison sample-5-A.

[0259] In addition, according to the same steps as the comparative sample-5-A, the comparative sample-5-B, comparative sample-5-C and comparative sample-5-D were prepared respectively. The properties of the final samples are shown in Table 2:

[0260]

[0261]

[0262] Comparative Sample-6: basically the same as Example 6, the only difference is that the seed microspheres are replaced by Comparative Sample-1 in Comparative Example 1; finally, the average particle size of the resin microspheres was measured to be 5.6 μm, the polydispersity coefficient was 1.328, and the crosslinking degree was 34%.

[0263] Comparative Sample-7: basically the same as Example 6, the only difference is that the seed microspheres are replaced by Comparative Sample-2 in Comparative Example 1; finally, the average particle size of the resin microspheres was measured to be 21 μm, the polydispersity coefficient was 1.394, and the crosslinking degree was 28%.

[0264] Comparative Sample-8: basically the same as Example 6, except that the seed microspheres are replaced by Comparative Sample-3 in Comparative Example 1; finally, the average particle size of the resin microspheres was measured to be 4.2 μm, the polydispersity coefficient was 1.228, and the crosslinking degree was 37%.

[0265] Comparative Sample-9: basically the same as Example 6, except that the seed microspheres are replaced by Comparative Sample-4 in Comparative Example 1; finally, the average particle size of the resin microspheres was measured to be 4.8 μm, the polydispersity coefficient was 1.227, and the crosslinking degree was 34%.

[0266] Example 7

[0267] In this example, the seed microspheres prepared in the example, i.e., seed microspheres-3 in Example 3, were used to prepare resin microspheres. The specific steps are as follows:

[0268] Raw material phase 3: Add 150 mL ultrapure water to a 500 mL three-necked flask, weigh 1.5 g sodium dodecyl sulfonate and add it to the water, turn on the stirring at a speed of 200 r / min. After the sodium dodecylbenzene sulfonate is dissolved, weigh 3 g of the bulbs and add them to the solution.

[0269] The three-necked flask was ultrasonicated for 40 minutes to evenly disperse the bulb-3. The three-necked flask containing the bulb was placed in a water bath, maintained at a temperature of 40 degrees Celsius, and mechanically stirred at a stirring speed of 350 r / min.

[0270] Raw material phase 4:

[0271] The first portion: weigh 1g of sodium dodecyl sulfate and add it to 100mL of water, add 4g of styrene, 8g of divinylbenzene (purity 80%), 2mL of dibutyl phthalate, and 2mL of toluene, and disperse by ultrasonic. Take the liquid and observe it under a microscope until there are no obvious oil droplets. Then add 1.5g of benzoyl peroxide and 0.4g of azobisisobutyronitrile and disperse it evenly by ultrasonic.

[0272] The second batch: weigh 0.5g sodium dodecyl sulfate and add it to 50mL water, add 2g styrene and 4g divinylbenzene (purity 80%), disperse by ultrasonic, observe the liquid under a microscope until there are no obvious oil drops, then add 0.7g benzoyl peroxide and disperse by ultrasonic.

[0273] Swelling of seed microspheres: add 40 mL of the first raw material phase 4 to the raw material phase 3, stir for 10 minutes, then add 30 mL of the first raw material phase 4 to the raw material phase 3, stir for half an hour, then add the remaining 30 mL of the first raw material phase 4 and swell for 12 hours;

[0274] After the swelling is completed, the temperature is raised to 70 degrees Celsius and the reaction is carried out for 2 hours;

[0275] Then, cool down to 50 degrees Celsius;

[0276] Continue to add 20 mL of the second raw material phase four, stir at 50 degrees Celsius for 10 minutes, raise the temperature to 70 degrees Celsius and react for half an hour; then lower the temperature to 50 degrees Celsius, add 10 mL of the second raw material phase four, maintain at 50 degrees Celsius for 10 minutes, raise the temperature to 70 degrees Celsius and react for half an hour; repeat the above process until the addition of raw material phase four is complete.

[0277] After the addition of raw material phase 4 is completed, the temperature is raised to 70 degrees Celsius, the reaction is carried out for 10 hours, and the heating is stopped.

[0278] After washing with ethanol for several times, the mixture was extracted and dried at 50 degrees Celsius to constant weight. The particle size of the resin microspheres was measured to be 4.8 μm, the polydispersity coefficient was 1.113, and the cross-linking degree was 39%.

[0279] Example 8

[0280] In this example, the seed microspheres prepared in the example, i.e., seed microspheres-4 of Example 4, were used to prepare resin microspheres. The specific steps are as follows:

[0281] Raw material phase 3: Add 150 mL ultrapure water to a 500 mL three-necked flask, weigh 1.5 g sodium dodecyl sulfonate and add it to the water, turn on the stirring at a speed of 200 r / min. After the sodium dodecylbenzene sulfonate is dissolved, weigh 3 g of the bulbs and add them to the solution.

[0282] The three-necked flask was ultrasonicated for 40 minutes to evenly disperse the bulb-4. The three-necked flask containing the bulb was placed in a water bath, maintained at 40 degrees Celsius, and mechanically stirred at a stirring speed of 350 r / min.

[0283] Raw material phase 4:

[0284] The first portion: weigh 1g of sodium dodecyl sulfate and add it to 100mL of water, add 4g of styrene, 8g of divinylbenzene (purity 80%), 2mL of dibutyl phthalate, and 2mL of toluene, and disperse by ultrasonic. Take the liquid and observe it under a microscope until there are no obvious oil droplets. Then add 1.5g of benzoyl peroxide and 0.4g of azobisisobutyronitrile and disperse it evenly by ultrasonic.

[0285] The second batch: weigh 0.5g sodium dodecyl sulfate and add it to 50mL water, add 2g styrene and 4g divinylbenzene (purity 80%), disperse by ultrasonic, observe the liquid under a microscope until there are no obvious oil drops, then add 0.7g benzoyl peroxide and disperse by ultrasonic.

[0286] Swelling of seed microspheres: add 40 mL of the first raw material phase 4 to the raw material phase 3, stir for 10 minutes, then add 30 mL of the first raw material phase 4 to the raw material phase 3, stir for half an hour, then add the remaining 30 mL of the first raw material phase 4 and swell for 12 hours;

[0287] After the swelling is completed, the temperature is raised to 70 degrees Celsius and the reaction is carried out for 2 hours;

[0288] Then, cool down to 50 degrees Celsius;

[0289] Continue to add 20 mL of the second raw material phase four, stir at 50 degrees Celsius for 10 minutes, raise the temperature to 70 degrees Celsius and react for half an hour; then lower the temperature to 50 degrees Celsius, add 10 mL of the second raw material phase four, maintain at 50 degrees Celsius for 10 minutes, raise the temperature to 70 degrees Celsius and react for half an hour; repeat the above process until the addition of raw material phase four is complete.

[0290] After the addition of raw material phase 4 is completed, the temperature is raised to 70 degrees Celsius, the reaction is carried out for 10 hours, and the heating is stopped.

[0291] After washing with ethanol for several times, the mixture was extracted and dried at 50 degrees Celsius to constant weight. The particle size of the resin microspheres was measured to be 4.3 μm, the polydispersity coefficient was 1.127, and the cross-linking degree was 36%.

[0292] Example 9

[0293] In this example, the seed microspheres prepared in the example, i.e., seed microspheres-1, were used to prepare resin microspheres. The specific steps are as follows:

[0294] Raw material phase 3: Add 150 mL ultrapure water to a 500 mL three-necked flask, weigh 1.5 g sodium dodecyl sulfonate and add it to the water, turn on the stirring at a speed of 200 r / min. After the sodium dodecylbenzene sulfonate is dissolved, weigh 3 g of the bulbs and add them to the solution.

[0295] Ultrasonicate the three-necked flask for 40 minutes to evenly disperse the bulbs. Place the three-necked flask containing the bulbs in a water bath, maintain the temperature at 40 degrees Celsius, and use mechanical stirring at a stirring speed of 350 r / min.

[0296] Raw material phase 4:

[0297] The first portion: weigh 1g of sodium dodecyl sulfate and add it to 100mL of water, add 4g of styrene, 9g of divinylbenzene (purity 80%), 2.5mL of dibutyl phthalate, and 2mL of toluene, and disperse by ultrasonic. Take the liquid and observe it under a microscope until there are no obvious oil droplets. Then add 1.5g of benzoyl peroxide and 0.4g of azobisisobutyronitrile and disperse it evenly by ultrasonic.

[0298] The second batch: weigh 0.5g sodium dodecyl sulfate and add it to 50mL water, add 2g styrene and 4.5g divinylbenzene (purity 80%), disperse by ultrasonic, observe the liquid under a microscope until there are no obvious oil drops, then add 0.7g benzoyl peroxide and disperse by ultrasonic.

[0299] Swelling of seed microspheres: add 40 mL of the first raw material phase 4 to the raw material phase 3, stir for 10 minutes, then add 30 mL of the first raw material phase 4 to the raw material phase 3, stir for half an hour, then add the remaining 30 mL of the first raw material phase 4 and swell for 12 hours;

[0300] After the swelling is completed, the temperature is raised to 70 degrees Celsius and the reaction is carried out for 2 hours;

[0301] Then, cool down to 50 degrees Celsius;

[0302] Continue to add 20 mL of the second raw material phase four, stir at 50 degrees Celsius for 10 minutes, raise the temperature to 70 degrees Celsius and react for half an hour; then lower the temperature to 50 degrees Celsius, add 10 mL of the second raw material phase four, maintain at 50 degrees Celsius for 10 minutes, raise the temperature to 70 degrees Celsius and react for half an hour; repeat the above process until the addition of raw material phase four is complete.

[0303] After the addition of raw material phase 4 is completed, the temperature is raised to 70 degrees Celsius, the reaction is carried out for 10 hours, and the heating is stopped.

[0304] After washing with ethanol for several times, the mixture was extracted and dried at 50 degrees Celsius to constant weight. The particle size of the resin microspheres was measured to be 4.1 μm, the polydispersity coefficient was 1.046, and the cross-linking degree was 43%.

Claims

1. A method for preparing resin microspheres, characterized in that: The process comprises the following steps: A. Seed microsphere synthesis stage A1 Prepare the raw materials phase 1: The raw material phase 1 includes a solvent; and at least two types of dispersants; A2 prepares raw materials for phase 2: The second raw material phase includes styrene and an initiator; A3 seed microsphere synthesis: The raw material phase 2 and the raw material phase 1 are added, and after the addition is completed, the mixture is reacted at 60-80° C. for 4-24 hours to obtain seed microspheres; B. Seed microsphere swelling stage B1 prepare raw materials for phase 3: The raw material phase three includes seed microspheres and an emulsifier; B2 prepares raw materials phase 4: The prepared raw material phase 4 includes styrene, divinylbenzene, a porogen, an emulsifier, an initiator and a surfactant. B3 seed microsphere swelling 1: Adding, swelling and reacting the raw material phase 3 and the raw material phase 4; The adding is performed in N times, where N is an integer ≥2.

2. The method for preparing resin microspheres according to claim 1, characterized in that: In A1, the raw material phase 1 includes two dispersants, type 1 and type 2; The type 1 dispersant is selected from any one or two of polyvinyl pyrrolidone and polyvinyl alcohol, wherein the molecular weight of the polyvinyl alcohol is ≥10000; The second type of dispersant is selected from any one or more of polyacrylic acid, polyvinyl alcohol, ethyl cellulose, hydroxypropyl methylcellulose, and hydroxy calcium phosphate, wherein the molecular weight of the polyvinyl alcohol is less than 10,000.

3. The method for preparing resin microspheres according to claim 2, characterized in that: The dosage ratio of the type 1 dispersant to the type 2 dispersant is (10-13): (0.5-1.5).

4. The method for preparing resin microspheres according to any one of claim 3, characterized in that: In the A, the mass ratio of styrene, initiator, dispersant and solvent is (30-80):(1-3):(5-10):(300-600).

5. The method for preparing resin microspheres according to any one of claim 4, characterized in that: In B1, the mass percentage of seed microspheres and emulsifier is (0.5-2): (0.5-1.5).

6. The method for preparing resin microspheres according to any one of claims 1 to 5, characterized in that: In B2, the raw material phase 4 includes a first raw material phase 4 and a second raw material phase 4; wherein, The mass percentages of styrene, divinylbenzene, porogen, emulsifier and initiator in the first raw material phase 4 are (1.5-3): (1-4): (1-2): (0.5-1.5): (0.5-1.5); and / or, The mass percentages of styrene, divinylbenzene, emulsifier and initiator in the second raw material phase four are (1.5-3):(1-4):(0.5-1.5):(0.5-1.5).

7. The method for preparing resin microspheres according to any one of claim 6, characterized in that: The amount ratio of the first raw material phase 4 to the raw material phase 3 is (1-2): (1-2); and / or, The usage ratio of the first raw material phase four to the second raw material phase four is (1-2): (1-2).

8. The method for preparing resin microspheres according to claim 7, characterized in that: In B3, First, the first raw material phase 4 is added, and the addition is performed in N times, where N is an integer ≥ 2; after the previous addition is completed, the temperature is raised to 60-80° C. for reaction, and then the temperature is lowered to below 50° C. for the next addition; after the first raw material phase 4 is added, it is swollen and then reacted at 60-80° C. for 4-24 hours; Then, the second raw material phase four is added, and the addition is carried out in N times, where N is an integer ≥ 2; after the previous addition is completed, the temperature is raised to 60-80°C for reaction, and then the temperature is lowered to below 50°C for the next addition; after the addition of the second raw material phase four is completed, it is swelled and then reacted at 60-80°C for 4-24 hours.

9. Resin microsphere particles, characterized in that: The resin microsphere particles are prepared by the method described in any one of claims 1 to 8; The particle size of the resin microsphere particles is 4-9 μm; and / or, The specific surface area of ​​the resin microsphere particles is 40-100m 2 / g; and / or, The cross-linking degree of the resin microsphere particles is 30%-45%.

10. A chromatographic filler or a chromatographic column, characterized in that: The chromatographic filler or chromatographic column comprises resin microsphere particles prepared by the method of any one of claims 1 to 8; and / or The resin microsphere particles according to claim 9.

Citation Information

Patent Citations

  • Swelling copolymerization preparation method of N-vinyl pyrrolidone and divinylbenzene monodisperse microsphere

    CN102382227B

  • Preparation of monodisperse porous polymer microsphere

    CN101434673A

  • Preparation method of monodisperse large-particle size crosslinked polymethyl methacrylate (PMMA) microspheres

    CN102786635A

  • Method of utilizing dual surfactants to prepare mono-disperse polystyrene microspheres

    CN106947026A

  • Preparation method of monodisperse polystyrene microspheres for calibrating PM10 cutter

    CN115197350A

Cited By

  • Preparation method of spherical phenolic resin

    CN121449841A