Fluorine-containing copolymer, preparation method thereof and battery
By using copolymerization reactions such as tetrafluoroethylene in hydrogen fuel cells, fluorine-containing copolymers with high water resistance and high ion exchange capacity are formed, which solves the problems of insufficient existing resin capacity and process complexity, and achieves high energy Applicability and cost-effectiveness of density fuel cells.
Patent Information
- Application Number
- CN202411174092.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-12-03
AI Technical Summary
The ion exchange capacity of the proton exchange resin in existing hydrogen fuel cells is insufficient, which cannot meet the high energy density requirements. The improvement process is high and complex and may lead to deterioration of the resin properties, resulting in the fuel cell being perforated and broken under working conditions, causing short circuits. .
Using fluorine-containing copolymers, copolymerization reactions are carried out in the polymerization reactor through comonomers such as tetrafluoroethylene and hexafluoropropylene to form fluorine-containing sulfonic acid resins with high water resistance and high ion exchange capacity, avoiding additional crosslinking agents. The use of the process simplifies the process.
The fluorine-containing copolymer with high water resistance and high ion exchange capacity is achieved, which reduces production costs, simplifies process steps, is suitable for high energy density fuel cell applications, and significantly improves the performance of the proton exchange membrane.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the field of polymer materials, and in particular to a fluorine-containing copolymer, a method for preparing the fluorine-containing copolymer, and a battery comprising a diaphragm made of the fluorine-containing copolymer. Background Art
[0002] In the past decade, new energy vehicles powered by batteries have achieved extremely rapid development. As the core of these new energy vehicles, the research and development of lithium-ion and hydrogen fuel cell technologies has received great attention, and the diaphragm in the battery is one of the most critical components of the battery. For example, proton exchange diaphragms made of hydrogen ion exchange resins are needed in hydrogen fuel cells. Such resins were first developed in the 1960s and were prepared by copolymerization of tetrafluoroethylene and perfluorosulfonyl vinyl ether (PSVE) monomer solutions / emulsions / suspensions. Because of its excellent chemical stability and proton conductivity, after decades of development, such resins are still the only ion exchange resins commercialized in the field of hydrogen fuel cells to date.
[0003] However, with the current demand for high energy density in fuel cell stacks, the ion exchange capacity of currently available commercial resins (0.9-1.0 mmol / g) can no longer meet the demand. In order to increase the ion exchange capacity of the resin, various manufacturers and scientific research institutions have invested a lot of scientific research funds, manpower and resources to try to improve the resin synthesis technology, such as changing the type and process conditions of the copolymerization reaction, adjusting the type and relative content of the copolymer monomer, but the above attempts have not achieved satisfactory results. Specifically, these attempts cannot achieve a satisfactory increase in the ion exchange capacity of the resin, or require additional cross-linking agents, or the manufacturing process is complicated and the cost is too high, making it completely unsuitable for commercialization, and it may also cause the degradation of other properties of the resin, such as the decrease in water resistance will cause the proton exchange membrane to be perforated and ruptured under working conditions, and then cause the fuel cell to short-circuit.
[0004] Therefore, the art urgently needs to develop a new technology to synthesize a fluorinated sulfonic acid resin with high water resistance and high ion exchange capacity by a low-cost and simple process. All technical problems in the art are unexpectedly solved. Summary of the invention
[0005] The first aspect of the present invention provides a fluorine-containing copolymer, wherein the fluorine-containing copolymer comprises copolymerized units derived from the following compounds:
[0006] Compound I shown in formula I
[0007]
[0008] In Formula I, each of R1, R2, R3 and R4 is independently a fluorine atom or a perfluoro C1-C6 alkyl group;
[0009] Compound II shown in formula II
[0010] CF2=CF-[OCFR5CFR6] x -O-[CR7R8] y -SO3R9 Formula II
[0011] In Formula II, each of R5, R6, R7 and R8 is independently a fluorine atom, a chlorine atom, a perfluoro C1-C6 alkyl group or a perfluoro C1-C6 alkoxy group; R9 is a fluorine atom, a chlorine atom or a perfluoro C1-C6 alkyl group; x is 0, 1 or 2, and y is 2, 3, 4, 5 or 6;
[0012] Any one or both of the compound III shown in formula III and the compound IV shown in formula IV
[0013] (F2C=FR 10 )-A-(CR 11 =CF2) Formula III
[0014] In Formula III, R 10 and R 11 Each of them is independently a fluorine atom, a chlorine atom, a perfluoro C1-C6 alkyl group or a perfluoro C1-C6 alkoxy group; A is a covalent bond, or is a C1-C8 alkylene group optionally substituted by at least one of fluorine, chlorine, C1-C3 alkyl, fluorinated C1-C3 alkyl, C1-C3 alkoxy, and fluorinated C1-C3 alkoxy;
[0015] (F2C=FR 12 )-Ar-(CR 13 =CF2) Formula IV
[0016] In Formula IV, R 12 and R 13 Each of them is independently a fluorine atom, a chlorine atom, a perfluoro C1-C6 alkyl group or a perfluoro C1-C6 alkoxy group; A is a C6-C6 group optionally substituted by at least one of fluorine and chlorine. 12 Arylene or C7-C 16 Arylene alkyl.
[0017] According to one embodiment of the first aspect of the present application, the compound I is tetrafluoroethylene, hexafluoropropylene, octafluorobutene, decafluoropentene, dodecafluorohexene or tetradecafluoroheptene. According to another embodiment of the first aspect of the present application, in formula II, each of R5, R6, R7 and R8 is independently a fluorine atom, a chlorine atom, a perfluoro C1-C3 alkyl group or a perfluoro C1-C3 alkoxy group; R9 is a fluorine atom, a chlorine atom or a perfluoro C1-C3 alkyl group; x is 0 or 1 or 2, and y is 2, 3 or 4.
[0018] According to another embodiment of the first aspect of the present application, in Formula III, R 10 and R 11 Each of them is independently a fluorine atom, a chlorine atom, a perfluoro C1-C3 alkyl group or a perfluoro C1-C3 alkoxy group; A is a covalent bond, or is a C1-C3 alkylene group optionally substituted by at least one of fluorine and chlorine.
[0019] According to another embodiment of the first aspect of the present application, in Formula IV, R 12 and R 13 Each of A is independently a fluorine atom, a chlorine atom, a perfluoro C1-C3 alkyl group or a perfluoro C1-C3 alkoxy group. According to another embodiment of the first aspect of the present application, A is a C6-C3 alkyl group optionally substituted with at least one of fluorine, chlorine, C1-C3 alkyl group, fluorinated C1-C3 alkyl group, C1-C3 alkoxy group, fluorinated C1-C3 alkoxy group 10 Arylene or C7-C 12 Arylene alkyl.
[0020] According to another embodiment of the first aspect of the present application, the compound I is tetrafluoroethylene. According to another embodiment of the first aspect of the present application, the compound II is CF2=CF-[OCF2CF(CF3)] x -O-[CF2] y -SO3F, wherein x is 0 or 1, and y is 2, 3 or 4. According to another embodiment of the first aspect of the present application, compound III has a structure shown in the following formula III',
[0021]
[0022] Where R 14 , R 15 , R 16 and R 17 Each of which is independently hydrogen, fluorine or chlorine. According to another embodiment of the first aspect of the present application, compound IV is 1,1,2,3,4,4-hexafluoro-1,3-butadiene.
[0023] According to another embodiment of the first aspect of the present application, the total molar amount of all comonomers forming the fluorinated copolymer is 100 mol%, and the content of the compound I is 60-79 mol%. According to another embodiment of the first aspect of the present application, the total molar amount of all comonomers forming the fluorinated copolymer is 100 mol%, and the content of the compound II is 20-39 mol%. According to another embodiment of the first aspect of the present application, the total molar amount of all comonomers forming the fluorinated copolymer is 100 mol%, and the content of the compound III is 0-3 mol%. According to another embodiment of the first aspect of the present application, the total molar amount of all comonomers forming the fluorinated copolymer is 100 mol%, and the content of the compound IV is 0-3 mol%.
[0024] According to another embodiment of the first aspect of the present application, the number average molecular weight Mn of the fluorine-containing polymer is 10,000 to 500,000.
[0025] The second aspect of the present application provides a method for preparing the fluorine-containing copolymer of the present application, the method comprising adding compound I, compound II, compound III and / or compound IV into a polymerization reactor to allow copolymerization to occur, and water and an initiator are also added into the polymerization reactor.
[0026] According to one embodiment of the second aspect of the present application, the molar ratio of compound I added to the polymer reactor to compound II is 1-5:1. According to another embodiment of the second aspect of the present application, the molar ratio of the molar amount of compound I added to the polymer reactor to (the total molar amount of compound III and compound IV) is 100-500:1. According to another embodiment of the second aspect of the present application, the mass of water added to the reactor is 1-15 times the total mass of all comonomers. According to another embodiment of the second aspect of the present application, the copolymerization reaction is carried out at a temperature of 20-70°C for 1-12 hours.
[0027] The third aspect of the present application provides a battery, at least a portion of which comprises the fluorine-containing copolymer of the present application, or comprises the fluorine-containing copolymer prepared by the method of the present application.
[0028] According to one embodiment of the third aspect of the present application, the product is a fuel cell, and the proton exchange membrane of the fuel cell comprises the fluorine-containing copolymer.
[0029] Some implementations of the present application are described below, but the present application is not limited to these specific implementations. The protection scope of the present application is defined by the claims. DETAILED DESCRIPTION
[0030] "Range" disclosed herein is in the form of lower limit and upper limit. It can be one or more lower limits, and one or more upper limits respectively. A given range is defined by selecting a lower limit and an upper limit. The selected lower limit and upper limit define the boundaries of a particular range. All ranges that can be defined in this way are inclusive and combinable, i.e. any lower limit can be combined with any upper limit to form a range. For example, a range of 60-120 and 80-110 is listed for a particular parameter, and it is understood that a range of 60-110 and 80-120 is also expected. In addition, if the minimum range values 1 and 2 are listed, and if the maximum range values 3, 4 and 5 are listed, the following ranges can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5.
[0031] In the present invention, unless otherwise specified, the numerical range "ab" represents an abbreviation of any real number combination between a and b, where a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" have been listed in this document, and "0-5" is just an abbreviation of these numerical combinations.
[0032] In the present invention, unless otherwise specified, all embodiments and preferred embodiments mentioned herein can be combined with each other to form a new technical solution.
[0033] In the present invention, unless otherwise specified, all technical features and preferred features mentioned herein can be combined with each other to form a new technical solution.
[0034] In the present invention, if there is no special explanation, the "including" mentioned herein means open or closed. For example, the "including" may mean that other components not listed may also be included, or only the listed components may be included.
[0035] In the present invention, when describing the spatial relationship of a specific component or object relative to other components or objects, the terms "inside", "outside", "above", "below", etc. are used to indicate that the former is located inside, outside, above or below the latter, and the two may be in direct contact, or be separated by a certain distance or separated by a third component or object.
[0036] It should be emphasized that what is described below are only some specific embodiments of the present invention, and the protection scope of the present invention is not limited to these specific embodiments. The protection scope of the present invention is defined by the claims of the present invention, and may include any technical solutions within the scope of the claims, including but not limited to further improvements and substitutions to these specific embodiments.
[0037] The fluorinated copolymer of the present application is prepared by copolymerization using compounds I to IV as comonomers, and thus the fluorinated copolymer of the present application comprises copolymerized units formed by copolymerization of the comonomers, specifically, by addition polymerization of vinyl double bonds.
[0038] According to one embodiment of the present application, the copolymer is prepared by copolymerizing compound I, compound II and compound III.
[0039] According to another embodiment of the present application, the copolymer is prepared by copolymerizing compound I, compound II and compound IV.
[0040] According to another embodiment of the present application, the copolymer is prepared by copolymerizing compound I, compound II, compound III and compound IV.
[0041] According to a specific embodiment of the present application, the fluorine-containing copolymer uses only the above-mentioned comonomer as its comonomer, and does not contain other comonomers.
[0042] According to another specific embodiment of the present application, the fluorine-containing copolymer only contains compound I, compound II, compound III and / or compound IV as polyene compounds, but does not contain any other cross-linking agent, and it is not necessary to add any other cross-linking agent during or after the copolymerization reaction.
[0043] According to one embodiment of the present application, the compound I has a structure shown in Formula I:
[0044]
[0045] In formula I, each of R1, R2, R3 and R4 is independently a fluorine atom or a perfluoro C1-C6 alkyl group; for example, each of R1, R2, R3 and R4 is independently a fluorine atom or a perfluoro C1-C4 alkyl group; or each of R1, R2, R3 and R4 is independently a fluorine atom or a perfluoro C1-C3 alkyl group; or each of R1, R2, R3 and R4 is independently a fluorine atom or a perfluoro C1-C2 alkyl group; according to a specific embodiment of the present application, the compound I is tetrafluoroethylene, hexafluoropropylene, octafluorobutene, decafluoropentene, dodecafluorohexene or tetradecafluoroheptene, more specifically tetrafluoroethylene.
[0046] According to one embodiment of the present application, based on the total molar amount of all copolymer units in the fluorinated copolymer as 100 mol%, the content of the copolymer units formed by compound I is 60-79 mol%, or 62-78 mol%, or 64-76 mol%, or 65-75 mol%, or 66-74 mol%, or 66-72 mol%, or 71-79 mol%, or 60-69 mol%, or within the numerical range obtained by combining any two of the above end values.
[0047] According to one embodiment of the present application, compound II has a structure shown in formula II:
[0048] CF2=CF-[OCFR5CFR6] x -O-[CR7R8] y -SO3R9 Formula II
[0049] In formula II, each of R5, R6, R7 and R8 is independently a fluorine atom, a chlorine atom, a perfluoro C1-C6 alkyl group or a perfluoro C1-C6 alkoxy group; for example, each of R5, R6, R7 and R8 is independently a fluorine atom, a chlorine atom, a perfluoro C1-C4 alkyl group or a perfluoro C1-C4 alkoxy group; or each of R5, R6, R7 and R8 is independently a fluorine atom, a chlorine atom, a perfluoro C1-C2 alkyl group or a perfluoro C1-C2 alkoxy group; R9 is a fluorine atom, a chlorine atom or a perfluoro C1-C6 alkyl group; for example, R9 is a fluorine atom, a chlorine atom or a perfluoro C1-C4 alkyl group; or R9 is a fluorine atom, a chlorine atom or a perfluoro C1-C2 alkyl group; x is 0, 1 or 2, y is 2, 3, 4, 5 or 6; or x is 0 or 1, y is 2, 3 or 4.
[0050] According to a specific embodiment of the present application, the compound II is CF2=CF-[OCF2CF(CF3)] x -O-[CF2] y -SO3F, wherein x is 0 or 1, and y is 2, 3 or 4. According to an exemplary embodiment of the present application, the compound II is CF2=CF-O-CF2CF(CF3)-O-CF2CF2-SO2F.
[0051] According to a more specific embodiment of the present application, based on the total molar amount of all copolymer units in the fluorinated copolymer as 100 mol%, the content of the copolymer units formed by compound II is 20-39 mol%, or 22-38 mol%, or 24-36 mol%, or 26-35 mol%, or 25-34 mol%, or 26-33 mol%, or 27-32.7 mol%, or 28-32.7 mol%, or 29-30 mol%, or 31-32 mol%, or within the numerical range obtained by combining any two of the above end values.
[0052] According to one embodiment of the present application, the compound III has a structure shown in formula III:
[0053] (F2C=FR 10 )-A-(CR 11 =CF2) Formula III
[0054] In Formula III, R 10 and R 11 Each of them is independently a fluorine atom, a chlorine atom, a perfluoro C1-C6 alkyl group or a perfluoro C1-C6 alkoxy group, for example, R 10 and R 11 Each of them is independently a fluorine atom, a chlorine atom, a perfluoro C1-C4 alkyl group or a perfluoro C1-C4 alkoxy group, or R 10 and R 11 Each of them is independently a fluorine atom, a chlorine atom, a perfluoro C1-C2 alkyl group or a perfluoro C1-C2 alkoxy group; A is a covalent bond, or a C1-C8 alkylene group optionally substituted by at least one of fluorine, chlorine, C1-C3 alkyl, fluorinated C1-C3 alkyl, C1-C3 alkoxy, and fluorinated C1-C3 alkoxy, such as C1-C6 alkylene group optionally substituted by at least one of fluorine, chlorine, C1-C2 alkyl, fluorinated C1-C2 alkyl, C1-C2 alkoxy, and fluorinated C1-C2 alkoxy, or C1-C3 alkylene group optionally substituted by at least one of fluorine, chlorine, C1-C2 alkyl, fluorinated C1-C2 alkyl, C1-C2 alkoxy, and fluorinated C1-C2 alkoxy. According to an exemplary embodiment, the compound III is 1,1,2,3,4,4-hexafluoro-1,3-butadiene.
[0055] According to a more specific embodiment of the present application, based on the total molar amount of all copolymer units in the fluorinated copolymer as 100 mol%, the content of the copolymer units formed by compound III is 0-3 mol%, or 0.05-3.5 mol%, or 0.08-3 mol%, or 0.1-2.5 mol%, or 0.15-2 mol%, or 0.16-1.8 mol%, or 0.15-1.5 mol%, or 0.16-1.2 mol%, or 0.18-1 mol%, or 0.19-0.8 mol%, or 0.2-0.5 mol%, or within the numerical range obtained by combining any two of the above end values.
[0056] According to one embodiment of the present application, the compound IV has a structure shown in Formula IV:
[0057] (F2C=FR 12 )-Ar-(CR 13 =CF2) Formula IV
[0058] In Formula IV, R 12 and R 13 Each of them is independently a fluorine atom, a chlorine atom, a perfluoro C1-C6 alkyl group or a perfluoro C1-C6 alkoxy group; for example, R 12 and R 13 Each of them is independently a fluorine atom, a chlorine atom, a perfluoro C1-C4 alkyl group or a perfluoro C1-C4 alkoxy group; or R 12 and R 13 Each of them is independently a fluorine atom, a chlorine atom, a perfluoro C1-C2 alkyl group or a perfluoro C1-C2 alkoxy group; A is a C6-C2 group optionally substituted by at least one of fluorine and chlorine. 12 Arylene or C7-C 16 Arylene, for example, A is a C6-C6 alkyl group optionally substituted with at least one of fluorine and chlorine. 10 Arylene or C7-C 14 Arylene, or A is C6-C8 arylene or C7-C 12 According to a specific embodiment of the present application, the compound IV has a structure shown in the following formula IV':
[0059]
[0060] Where R 14 , R 15 , R 16 and R 17 Each of which is independently hydrogen, fluorine or chlorine. According to an exemplary embodiment of the present application, R 14, R 15 , R 16 and R 17 Each of them is hydrogen.
[0061] According to a more specific embodiment of the present application, based on the total molar amount of all copolymer units in the fluorinated copolymer as 100 mol%, the content of the copolymer units formed by compound IV is 0-3 mol%, or 0.05-3.5 mol%, or 0.08-3 mol%, or 0.1-2.5 mol%, or 0.15-2 mol%, or 0.16-1.8 mol%, or 0.15-1.5 mol%, or 0.16-1.2 mol%, or 0.18-1 mol%, or 0.19-0.8 mol%, or 0.2-0.5 mol%, or within the numerical range obtained by combining any two of the above end values.
[0062] According to one embodiment of the present application, the number average molecular weight Mn of the fluorine-containing polymer is 10,000 to 500,000, for example, 20,000 to 400,000, or 30,000 to 300,000, or 40,000 to 250,000, or 50,000 to 200,000, or 60,000 to 150,000, or 70,000 to 120,000, or 80,000 to 100,000, or within the numerical range obtained by combining any two of the above end values. The number average molecular weight of the fluorine-containing copolymer of the present application can be detected by techniques known in the art, such as gel permeation chromatography, size exclusion chromatography, etc.
[0063] According to one embodiment of the present application, the ion exchange capacity of the fluorinated copolymer of the present application is 1.3-1.8 mmol / g, for example, 1.4-1.7 mmol / g, or 1.5-1.6 mmol / g.
[0064] According to one embodiment of the present application, the fluorine-containing copolymer of the present application has water resistance, for example, its weight loss rate in water resistance detection is ≤0.01%.
[0065] According to one embodiment of the present application, the fluorine-containing copolymer of the present application is formed by copolymerizing compound I, compound II and compound III in a polymerization reactor.
[0066] According to another embodiment of the present application, the fluorine-containing copolymer of the present application is formed by copolymerizing compound I, compound II and compound IV in a polymerization reactor.
[0067] According to one embodiment of the present application, the fluorine-containing copolymer of the present application is formed by copolymerizing compound I, compound II, compound III and compound IV in a polymerization reactor.
[0068] According to one embodiment of the present application, the copolymerization reaction is carried out at a temperature of 20-70°C for 1-12 hours, for example, at 30-60°C, 40-50°C for 2-10 hours, or 3-8 hours, or 4-7 hours, or 5-6 hours, or within the numerical range obtained by combining any two of the above end values.
[0069] According to one embodiment of the present application, the molar ratio of compound I to compound II added to the polymer reactor is 1-5:1; for example, the molar ratio is 1-4:1, or the molar ratio is 1-3:1, or the molar ratio is 1-2:1, or within the numerical range obtained by combining any two of the above end values.
[0070] According to one embodiment of the present application, the molar ratio of the molar amount of compound I added to the polymer reactor to (the total molar amount of compound III and compound IV) is 100-500:1, for example, the molar ratio is 150-450:1, or the molar ratio is 180-400:1, or the molar ratio is 200-350:1, or the molar ratio is 220-320:1, or the molar ratio is 250-300:1, or the molar ratio is 260-280:1, or within the numerical range obtained by combining any two of the above end values. For the case of using compound III without using compound IV, "the total molar amount of compound III and compound IV" means the molar amount of compound III; for the case of using compound IV without using compound III, "the total molar amount of compound III and compound IV" means the molar amount of compound IV; for the case of using compound III and compound IV at the same time, "the total molar amount of compound III and compound IV" means the molar amount of compound III + the molar amount of compound IV.
[0071] According to one embodiment of the present application, for the embodiment of adding compound III and compound IV simultaneously, the molar ratio of compound III and compound IV is 10:1 to 1:10, or the molar ratio is 8:1 to 1:8, or the molar ratio is 6:1 to 1:6, or the molar ratio is 5:1 to 1:5, or the molar ratio is 4:1 to 1:4, or the molar ratio is 3:1 to 1:3, or the molar ratio is 2:1 to 1:1, or within the numerical range obtained by combining any two of the above end values.
[0072] According to one embodiment of the present application, water and an initiator are also added to the polymerization reactor during the copolymerization reaction.
[0073] According to one embodiment of the present application, the mass of water added to the reactor is 1-15 times the total mass of all comonomers, for example, 1.5-12 times, or 1-10 times, or 1-8 times, or 1-6 times, or 1-5 times, or 1-4 times, or 1-3 times, or 1-2 times, or within the numerical range obtained by combining any two of the above end values.
[0074] According to one embodiment of the present application, the initiator is a peroxide initiator, such as ammonium persulfate. According to one embodiment of the present application, the mass of the initiator added to the reactor is 0.001% to 5% by mass of the total mass of all comonomers, such as 0.005% to 4% by mass, or 0.01% to 3% by mass, or 0.05% to 2% by mass, or 0.1% to 1.5% by mass, or 0.5% to 1% by mass, or 0.6% to 0.8% by mass, or within the numerical range obtained by combining any two of the above end values.
[0075] According to one embodiment of the present application, during the copolymerization reaction, the polymerization reactor is evacuated to keep the oxygen content at a low level, for example, less than 50 ppm, or less than 30 ppm, or less than 20 ppm, or less than 15 ppm.
[0076] According to another embodiment of the present application, the compound II and compound IV are mixed with water and an optional emulsifier to prepare an emulsion and add it to the reactor. The compound I and compound III are gaseous at normal temperature and pressure and are added to the reactor in the form of gas.
[0077] A very important advantage of the present invention is that there is no need to add an additional cross-linking agent to the copolymer after the copolymerization reaction to perform an additional post-cross-linking step. Therefore, it has the advantages of simple process steps and low process cost. The prepared resin has a high molecular weight and has both high water resistance and high ion exchange capacity. It is suitable for applications such as high energy density fuel cells. Compared with the existing fluorinated or perfluorinated polymers widely used in proton exchange membranes, it has achieved significant technical progress.
[0078] The fluorinated copolymer of the present application can be used to prepare a proton exchange membrane for use in batteries requiring proton exchange, such as hydrogen fuel cells.
[0079] Some specific implementation methods of the present application are introduced in the following examples.
[0080] Example
[0081] The preferred embodiments of the present invention are specifically listed in the following examples, but it should be understood that the protection scope of the present application is not limited thereto. Any equivalent changes or modifications made according to the essence of the present application should be included in the protection scope of the present application.
[0082] The raw materials used in the following examples are all commercially available reagents and are used directly without further treatment. The water used is deionized water.
[0083] The NMR spectra of the fluorinated copolymers prepared in the following examples were detected using a nuclear magnetic resonance instrument, and the capacity of the proton exchange membranes was determined by acid-base titration.
[0084] The water resistance of the fluorinated copolymers prepared in the following examples was tested by the following method: 100 g of the polymer resin was added to 100° C. boiling water for 24 h, and then the liquid was removed by filtration, the resin was collected, and the weight loss of the resin was tested after drying.
[0085] Embodiment 1:
[0086] In this example, a fluorine-containing copolymer simultaneously comprising Compound I, Compound II, and Compound IV was synthesized.
[0087] 5000 g of deionized water, 150 g of 20 wt% perfluoropolyether-6100 aqueous solution, 500 g of CF2=CF-O-CF2CF(CF3)-O-CF2CF2-SO2F monomer, and 5 g of 1,4-bis(1,2,2-trifluorovinyl)benzene were mixed to form a water droplet emulsion, and then the water droplet emulsion was added to an 8-liter high-pressure reactor. The reactor was evacuated and replaced three times, and the oxygen content in the reactor was measured to be about 14 ppm. The materials in the reactor were continuously stirred, and the stirring rate was set to 500 rpm. The materials in the reactor were heated to a temperature of about 83°C using a reactor jacket. Tetrafluoroethylene gas was introduced into the pressure reactor to increase the pressure to 0.5 MPa. 400 ml of deionized water pre-dissolved with 0.3 g of ammonium persulfate was pumped into the reactor to start the reaction. The tetrafluoroethylene pressure was maintained at about the initial value within about 4 minutes after the start of the reaction. At this time, the tetrafluoroethylene was stopped and the reaction was continued without introducing tetrafluoroethylene into the reactor. Within the next 120 minutes, the reaction pressure gradually decreased from about 0.5 MPa at the beginning to about 0.2 MPa. The reaction temperature was then reduced to below 50°C and the reaction system was vented to atmospheric pressure. The reaction produced 7000 grams of an aqueous dispersion of the copolymer. The total weight percentage of the copolymer emulsion obtained after precipitation and separation was 10.7%. The average particle size was about 131 nanometers. The emulsion was condensed, washed and dried to obtain 720 grams of a fluorine-containing copolymer product.
[0088] According to solid-state nuclear magnetic resonance detection, the molar content of copolymer units formed by tetrafluoroethylene in the polymer is 71.3%, the molar content of copolymer units formed by CF2=CF-O-CF2CF(CF3)-O-CF2CF2-SO2F is 28.5%, and the molar content of copolymer units formed by 1,4-bis(1,2,2-trifluorovinyl)benzene is 0.2%.
[0089] The fluorinated copolymer prepared in Example 1 was hydrolyzed and acidified, and then made into a proton exchange membrane.
[0090] The ion exchange membrane capacity of the fluorinated copolymer of the present application measured by acid-base titration is 1.43 mmol / L. After 24 hours of boiling water treatment, the weight loss of the resin is measured to be 0.05%.
[0091] Embodiment 2:
[0092] In this example, a fluorine-containing copolymer comprising Compound I, Compound II, and Compound III was synthesized.
[0093] 5000 g of deionized water, 150 g of 20 wt% perfluoropolyether-6100 aqueous solution, and 500 g of CF2=CF-O-CF2CF(CF3)-O-CF2CF2-SO2F monomer were mixed to form a water droplet emulsion, which was then added to an 8-liter high-pressure reactor. The reactor was evacuated and replaced three times, and the oxygen content in the reactor was measured to be about 14 ppm. Then 5 g of hexafluorobutadiene gas was introduced into the reactor. The materials in the reactor were continuously stirred, and the stirring rate was set to 500 rpm. The materials in the reactor were heated to a temperature of about 83° C. with a reactor jacket. Tetrafluoroethylene gas was introduced into the pressure reactor to increase the pressure to 0.5 MPa. 400 ml of deionized water pre-dissolved with 0.3 g of ammonium persulfate was pumped into the reactor to start the reaction. The tetrafluoroethylene pressure was maintained at about the initial value within about 4 minutes after the start of the reaction. At this time, the tetrafluoroethylene is stopped, and the reaction is continued without introducing tetrafluoroethylene into the reactor. Within the next 120 minutes, the reaction pressure gradually decreases from about 0.5MPa at the beginning to about 0.2MPa. Then the reaction temperature is reduced to below 50°C, and the reaction system is vented to atmospheric pressure. The aqueous dispersion generated by the reaction is precipitated and separated to obtain a copolymer emulsion. The emulsion is condensed, washed, and dried to obtain a fluorine-containing copolymer product.
[0094] According to solid-state nuclear magnetic resonance detection, the molar content of copolymer units formed by tetrafluoroethylene in the polymer is 68.8%, the molar content of copolymer units formed by CF2=CF-O-CF2CF(CF3)-O-CF2CF2-SO2F is 32.7%, and the molar content of copolymer units formed by hexafluorobutadiene is 0.5%.
[0095] The fluorinated copolymer prepared in Example 2 was hydrolyzed and acidified, and then prepared into a proton exchange membrane.
[0096] The ion exchange membrane capacity of the fluorinated copolymer of the present application measured by acid-base titration is 1.54 mmol / L. After 24 hours of boiling water treatment, the weight loss of the resin is measured to be 0.08%.
[0097] Comparative Example 1:
[0098] In this example, a fluorine-containing copolymer containing only compound I and compound II but not compound III and compound IV was synthesized.
[0099] 5000 g of deionized water, 150 g of 20 wt% perfluoropolyether-6100 aqueous solution and 500 g of CF2=CF-O-CF2CF(CF3)-O-CF2CF2-SO2F monomer were mixed to form a water droplet emulsion, which was then added to an 8-liter high-pressure reactor. The reactor was evacuated and replaced three times, and the oxygen content in the reactor was measured to be about 14 ppm. The materials in the reactor were continuously stirred, and the stirring rate was set to 500 rpm. The materials in the reactor were heated to a temperature of about 83° C. with a reactor jacket. Tetrafluoroethylene gas was introduced into the pressure reactor to increase the pressure to 0.5 MPa. 400 ml of deionized water pre-dissolved with 0.3 g of ammonium persulfate was pumped into the reactor to start the reaction. The tetrafluoroethylene pressure was maintained at about the initial value within about 4 minutes after the reaction started. At this time, the introduction of tetrafluoroethylene was stopped, and the reaction was continued without introducing tetrafluoroethylene into the reactor. In the next 120 minutes, the reaction pressure gradually decreased from about 0.5 MPa at the beginning to about 0.2 MPa. Then the reaction temperature was reduced to below 50°C, and the reaction system was evacuated to atmospheric pressure. The aqueous dispersion generated by the reaction was precipitated and separated to obtain a copolymer emulsion. The emulsion was coagulated, washed, and dried to obtain a fluorinated copolymer product.
[0100] According to solid-state nuclear magnetic resonance detection, the molar content of copolymer units formed by tetrafluoroethylene in the polymer is 73.8%, and the molar content of copolymer units formed by CF2=CF-O-CF2CF(CF3)-O-CF2CF2-SO2F is 26.2%.
[0101] The fluorine-containing copolymer prepared in Comparative Example 1 was hydrolyzed and acidified, and then prepared into a proton exchange membrane.
[0102] The ion exchange membrane capacity of the fluorinated copolymer of the present application measured by acid-base titration is 1.30 mmol / L. After 24 hours of boiling water treatment, the weight loss of the resin is measured to be 2.1%.
Claims
1. A fluorine-containing copolymer, comprising copolymerization units derived from the following compounds: Compound I shown in formula I In Formula I, each of R1, R2, R3 and R4 is independently a fluorine atom or a perfluoro C1-C6 alkyl group; Compound II shown in formula II CF2=CF-[OCFR5CFR6] x -O-[CR7R8] y -SO3R9 Formula II In Formula II, each of R5, R6, R7 and R8 is independently a fluorine atom, a chlorine atom, a perfluoro C1-C6 alkyl group or a perfluoro C1-C6 alkoxy group; R9 is a fluorine atom, a chlorine atom or a perfluoro C1-C6 alkyl group; x is 0, 1 or 2, and y is 2, 3, 4, 5 or 6; Any one or both of the compound III shown in formula III and the compound IV shown in formula IV (F2C=FR 10 )-A-(CR 11 =CF2) Formula III In Formula III, R 10 and R 11 Each of them is independently a fluorine atom, a chlorine atom, a perfluoro C1-C6 alkyl group or a perfluoro C1-C6 alkoxy group; A is a covalent bond, or is a C1-C8 alkylene group optionally substituted by at least one of fluorine, chlorine, C1-C3 alkyl, fluorinated C1-C3 alkyl, C1-C3 alkoxy, and fluorinated C1-C3 alkoxy; (F2C=FR 12 )-Ar-(CR 13 =CF2) Formula IV In Formula IV, R 12 and R 13 Each of them is independently a fluorine atom, a chlorine atom, a perfluoro C1-C6 alkyl group or a perfluoro C1-C6 alkoxy group; A is a C6-C6 group optionally substituted by at least one of fluorine and chlorine. 12 Arylene or C7-C 16 Arylene alkyl.
2. The fluorinated copolymer according to claim 1, characterized in that The compound I is tetrafluoroethylene, hexafluoropropylene, octafluorobutene, decafluoropentene, dodecafluorohexene or tetradecafluoroheptene; In formula II, each of R5, R6, R7 and R8 is independently a fluorine atom, a chlorine atom, a perfluoro C1-C3 alkyl group or a perfluoro C1-C3 alkoxy group; R9 is a fluorine atom, a chlorine atom or a perfluoro C1-C3 alkyl group; x is 0 or 1 or 2, and y is 2, 3 or 4.
3. The fluorinated copolymer according to claim 1, characterized in that In Formula III, R 10 and R 11 Each of them is independently a fluorine atom, a chlorine atom, a perfluoro C1-C3 alkyl group or a perfluoro C1-C3 alkoxy group; A is a covalent bond, or a C1-C3 alkylene group optionally substituted by at least one of fluorine and chlorine; In Formula IV, R 12 and R 13 Each of them is independently a fluorine atom, a chlorine atom, a perfluoro C1-C3 alkyl group or a perfluoro C1-C3 alkoxy group; A is a C6-C6 group optionally substituted by at least one of fluorine, chlorine, C1-C3 alkyl group, fluorinated C1-C3 alkyl group, C1-C3 alkoxy group, fluorinated C1-C3 alkoxy group 10 Arylene or C7-C 12 Arylene alkyl.
4. The fluorinated copolymer according to claim 1, characterized in that The compound I is tetrafluoroethylene; The compound II is CF2=CF-[OCF2CF(CF3)] x -O-[CF2] y -SO3F, wherein x is 0 or 1, and y is 2, 3 or 4; Compound III is 1,1,2,3,4,4-hexafluoro-1,3-butadiene; Compound IV has the structure shown in the following formula IV', Where R 14 , R 15 , R 16 and R 17 Each of which is independently hydrogen, fluorine or chlorine.
5. The fluorinated copolymer according to claim 1, characterized in that Based on the total molar amount of all comonomers forming the fluorine-containing copolymer as 100 mol%, the content of compound I is 60-79 mol%, the content of compound II is 20-39 mol%, the content of compound III is 0-3 mol%, and the content of compound IV is 0-3 mol%.
6. The fluorinated copolymer according to claim 1, characterized in that The fluorine-containing polymer has a number average molecular weight Mn of 10,000 to 500,000.
7. A method for preparing a fluorinated copolymer as claimed in any one of claims 1 to 6, characterized in that: The method comprises adding compound I, compound II, compound III and / or compound IV into a polymerization reactor to make copolymerization reaction occur, and water and an initiator are also added into the polymerization reactor.
8. The method according to claim 7, characterized in that The molar ratio of compound I added to the polymer reactor to compound II is 1-5:1; the molar ratio of the molar amount of compound I added to the polymer reactor to (the total molar amount of compound III and compound IV) is 100-500:1; the mass of water added to the reactor is 1-15 times the total mass of all copolymer monomers; the copolymerization reaction is carried out at a temperature of 20-70°C for 1-12 hours.
9. A battery, at least a part of which comprises the fluorinated copolymer according to any one of claims 1 to 6, or comprises the fluorinated copolymer prepared by the method according to any one of claims 7 to 8.
10. The battery according to claim 1, characterized in that The battery is a fuel cell, and the proton exchange membrane of the fuel cell comprises the fluorine-containing copolymer.
Citation Information
Cited By
Perfluorosulfonic acid resin, preparation method thereof, cross-linking type perfluorosulfonic acid proton exchange membrane and preparation method of cross-linking type perfluorosulfonic acid proton exchange membrane
CN122127525A
Perfluorosulfonic acid resin and its preparation method, cross-linked perfluorosulfonic acid proton exchange membrane and its preparation method
CN122127525B