Preparation method and application of polymethacrylimide foam

Through the preparation method of polymethacryimide foam without methacrylonitrile, combined with heat resistance and antioxidants, the problems of high production costs and poor performance are solved, and high-performance and low-cost foam materials are realized. in high temperature environment.

CN119060237APending Publication Date: 2024-12-03CHANGSHA ZHENXIANG MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411085875.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing polymethacryimide foam has high production costs, and the foam produced by low-cost replacement raw materials has poor performance and is difficult to meet application needs.

Method used

Using the preparation method without methacrylonitrile, using methacrylic acid, N,N dimethacrylamide, acrylonitrile, third monomer, toughening modifier, initiator, foaming agent and crosslinking agent, etc. The raw materials are used to improve the heat resistance and stability of the foam through the combination of heat-resistant additives and antioxidants, and the molding quality is improved through gradient heating and tempering treatment.

Benefits of technology

The performance and cost balance of polymethacryimide foam is achieved, with uniform cell cells, suitable density, thermal deformation temperature above 180℃, low thermal creep, excellent mechanical properties, and suitable for high temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004985160700000151
    Figure BDA0004985160700000151
Patent Text Reader

Abstract

The invention discloses a preparation method and application of polymethacrylimide foam. The polymethacrylimide foam is prepared from the following raw materials: methacrylic acid, N, N-dimethylacrylamide, acrylonitrile, a third monomer, a toughening modifier, an initiator, a foaming agent and a cross-linking agent. The third monomer comprises at least one of acrylamide and methacrylamide. The preparation raw materials of the polymethacrylimide foam do not comprise methacrylonitrile. The preparation raw materials of the polymethacrylimide provided by the invention do not comprise methacrylonitrile, and under the synergistic effect of the raw materials, the performance of the obtained polymethacrylimide foam is maintained, the raw material cost of the polymethacrylimide foam is reduced, and the mechanical property is excellent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of functional foam materials, and in particular relates to a preparation method of polymethacrylimide foam and application thereof. Background Art

[0002] The main raw materials for producing polymethacrylimide (PMI) foam are methacrylonitrile and methacrylic acid, among which methacrylonitrile is somewhat dangerous and the price of methacrylonitrile raw material is relatively high. Therefore, the price of using methacrylonitrile to produce PMI foam is relatively high, which limits the application field of PMI foam. Using low-cost acrylonitrile to replace methacrylonitrile as a raw material can produce low-priced PMI foam, but the material properties of the produced PMI foam, such as heat resistance, compression strength and other properties, are reduced, which is difficult to meet the requirements of the application field.

[0003] Therefore, it is urgent to develop a polymethacrylimide (PMI) foam that maintains the material properties of methacrylimide (PMI) foam and is low in price. Summary of the invention

[0004] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the present invention provides a polymethacrylimide foam which maintains the material properties of the polymethacrylimide foam without adding methacrylonitrile as a raw material.

[0005] A polymethacrylimide foam according to the first embodiment of the present invention, wherein the raw materials for preparing the polymethacrylimide foam include: methacrylic acid, N,N-dimethylacrylamide, acrylonitrile, a third monomer, a toughening modifier, an initiator, a foaming agent and a crosslinking agent;

[0006] The third monomer includes at least one of acrylamide and methacrylamide;

[0007] The raw materials for preparing the polymethacrylimide foam do not include methacrylonitrile.

[0008] The embodiments according to the first aspect of the present invention have at least the following beneficial effects:

[0009] The raw materials for preparing the polymethacrylimide provided by the present invention do not include methacrylonitrile. Under the synergistic effect of the raw materials in the present invention, the performance of the obtained polymethacrylimide foam is maintained while the cost of the raw materials of the polymethacrylimide foam is reduced. The pore diameter of the polymethacrylimide foam is 0.1 mm to 1 mm, and the density is 25 to 250 kg / m 3The foam has no obvious discoloration after long-term use at 150℃, the heat deformation temperature is higher than 180℃, the thermal creep at 0.3MPa150℃ is less than 1%, and the density exceeds 200 kg / m 3 The thermal creep at 0.5MPa and 150℃ is less than 1%, and the mechanical properties are excellent.

[0010] According to some embodiments of the present invention, the raw materials for preparing the polymethacrylimide foam include, by weight:

[0011] 80-100 parts of methacrylic acid, 40-100 parts of N,N-dimethylacrylamide, 30-60 parts of acrylonitrile, 1-10 parts of the third monomer, 0.15-0.25 parts of a toughening modifier, 0.1-1 parts of an initiator, 3-10 parts of a foaming agent and 0.5-15 parts of a crosslinking agent.

[0012] According to some embodiments of the present invention, the raw materials for preparing the polymethacrylimide foam further include: a heat-resistant additive; the heat-resistant additive includes: at least one of N,N'-(4,4'-methylenediphenyl)bismaleimide and N-phenylmaleimide.

[0013] In addition to conventional copolymers (methacrylic acid, acrylonitrile, N,N-dimethylacrylamide), initiators, foaming agents and crosslinking agents, the raw materials of the invention further adopt heat-resistant additives, wherein the heat-resistant additives are selected from N,N'-(4,4'-methylenediphenyl)bismaleimide and / or N-phenylmaleimide, which can realize the embedding of reactive groups on the main chain of the molecular chain of methacrylic acid and N,N-dimethylacrylamide copolymers, and N,N'-(4,4'-methylenediphenyl)bismaleimide and N-phenylmaleimide have rigid benzene rings, thereby improving the heat-resistant temperature of the foam, and the crosslinkability of the two is low, and the crosslinking degree of the prepolymer will not be increased and the foaming difficulty will not be caused.

[0014] According to some embodiments of the present invention, the raw materials for preparing the polymethacrylimide foam further include: an antioxidant; the antioxidant includes triphenyl phosphite.

[0015] The triphenyl phosphite antioxidant added in the present invention can resist the high-temperature oxidative decomposition of the foam material at high temperatures, further improve its high-temperature resistance and improve the stability of the polymerization reaction process.

[0016] According to some embodiments of the present invention, the initiator includes at least one of a peroxide and an azo compound.

[0017] According to some embodiments of the present invention, the peroxide includes at least one of dilauroyl peroxide, bis(4-tert-butylcyclohexyl)peroxydicarbonate, tert-butyl peroxy-2-ethylhexanoate, and tert-butyl peroxybenzoate.

[0018] According to some embodiments of the present invention, the azo compound includes at least one of azobisisobutyronitrile and azobisisoheptylnitrile.

[0019] According to some embodiments of the present invention, the foaming agent includes at least one of an amide foaming agent and an alcohol foaming agent.

[0020] According to some embodiments of the present invention, the amide foaming agent includes at least one of formamide and N,N-dimethylformamide.

[0021] According to some embodiments of the present invention, the alcohol foaming agent includes at least one of tert-butyl alcohol and isopropyl alcohol.

[0022] According to some embodiments of the present invention, the cross-linking agent includes at least one or more combinations of zinc methacrylate, magnesium methacrylate, allyl methacrylate, itaconic acid, tert-butyl methacrylate, acrylamide and methacrylamide.

[0023] According to some embodiments of the present invention, the raw materials for preparing the polymethacrylimide foam include, by weight:

[0024] 80-100 parts of methacrylic acid, 40-100 parts of N,N-dimethylacrylamide, 30-60 parts of acrylonitrile, 1-10 parts of the third monomer, 0.3-0.4 parts of heat-resistant additives, 0.6-0.7 parts of antioxidants, 0.15-0.25 parts of toughening modifiers, 0.1-1 parts of initiators, 3-10 parts of foaming agents and 0.5-15 parts of crosslinking agents, 0.3-2.5 parts of heat-resistant additives and 0.2-2 parts of antioxidants.

[0025] The crosslinking agent component in the present invention will not self-polymerize during the reaction process. At the same time, by controlling the amount of the crosslinking agent, defects such as excessive viscosity of the prepolymer, difficulty in defoaming, and brittleness of the prepolymer caused by excessive crosslinking agent are avoided, thereby significantly improving the molding quality and performance of the foam.

[0026] According to some embodiments of the present invention, the toughening modifier includes zinc stearate.

[0027] According to some embodiments of the present invention, the raw materials for preparing the polymethacrylimide foam include, by weight:

[0028] 80-100 parts of methacrylic acid, 40-100 parts of N,N-dimethylacrylamide, 30-60 parts of acrylonitrile, 1-10 parts of the third monomer, 0.3-0.4 parts of heat-resistant additives, 0.6-0.7 parts of antioxidants, 0.15-0.25 parts of toughening modifiers, 0.1-1 parts of initiators, 3-10 parts of foaming agents and 0.5-15 parts of crosslinking agents, 0.3-2.5 parts of heat-resistant additives, 0.2-2 parts of antioxidants and 0.15-0.4 parts of toughening modifiers.

[0029] The toughening agent in the present invention is preferably zinc stearate. Zinc stearate also acts as a surfactant, which can increase the cross-linking of the material while maintaining a certain toughness.

[0030] According to some preferred embodiments of the present invention, the raw materials for preparing the polymethacrylimide foam include, by weight:

[0031] 85-95 parts of methacrylic acid, 40-50 parts of N,N-dimethylacrylamide, 30-50 parts of acrylonitrile, 1-10 parts of the third monomer, 0.1-1 parts of initiator, 3-10 parts of foaming agent and 0.5-15 parts of cross-linking agent, 0.3-0.4 parts of heat-resistant additive, 0.6-0.7 parts of antioxidant and 0.15-0.25 parts of toughening modifier.

[0032] According to a second aspect of the present invention, a method for preparing a polymethacrylimide foam comprises the following steps:

[0033] S1. The raw materials for preparing the polymethacrylimide foam are mixed and reacted to obtain a prepolymer;

[0034] S2. The prepolymer obtained in step S1 is pre-treated by heating, foamed and then tempered.

[0035] According to some embodiments of the present invention, in step S1, the mixing reaction step includes: keeping warm at 25-37° C. for 110-280 hours, and then keeping warm at 40-50° C. for 36-72 hours.

[0036] According to some embodiments of the present invention, in step S2, the heating temperature of the heating pretreatment is 50-110° C., and the heating time of the heating pretreatment is 20-35 hours.

[0037] According to some preferred embodiments of the present invention, in step S2, the heating preheating step includes a first stage preheating treatment, a second stage preheating treatment and a third stage preheating treatment;

[0038] The temperature of the first stage preheating treatment is 50-65°C, and the time of the first stage preheating treatment is 10-18 hours;

[0039] The temperature of the second stage preheating treatment is 75-85°C, and the time of the second stage preheating treatment is 3-10 hours;

[0040] The temperature of the third stage preheating treatment is 90-100° C., and the time of the third stage preheating treatment is 2-6 hours.

[0041] In the present invention, it is preferred to use a temperature gradient increasing treatment method to make the material heated more evenly, which is beneficial to the subsequent foaming process.

[0042] According to some embodiments of the present invention, the temperature of the foaming molding is 140-250° C., and the time of the foaming molding is 2-9 hours.

[0043] According to some embodiments of the present invention, the foaming and molding step includes: a first stage of foaming and heating, a second stage of foaming and heating, and a third stage of foaming and heating;

[0044] The temperature of the first stage of foaming and heating is 110-150°C, and the time of the first stage of foaming and heating is 2-5h;

[0045] The temperature of the second stage of foaming and heating is 160-185°C, and the time of the second stage of foaming and heating is 30-90 minutes;

[0046] The temperature of the third stage of foaming and heating is 195-205° C., and the time of the third stage of foaming and heating is 1-3 hours.

[0047] According to some embodiments of the present invention, the foaming and molding step includes: a first stage of foaming and heating, a second stage of foaming and heating, a third stage of foaming and heating, and a fourth stage of foaming and heating;

[0048] The temperature of the first stage of foaming and heating is 110-150°C, and the time of the first stage of foaming and heating is 2-5h;

[0049] The temperature of the second stage of foaming and heating is 160-185°C, and the time of the second stage of foaming and heating is 30-90 minutes;

[0050] The temperature of the third stage of foaming and heating is 195-205°C, and the time of the third stage of foaming and heating is 30-60 minutes;

[0051] The temperature of the fourth stage of foaming and heating is 205-220° C., and the time of the fourth stage of foaming and heating is 2-4 hours.

[0052] The foaming step is performed by gradually increasing the temperature to perform gradient foaming, so that the foaming is more uniform.

[0053] According to some embodiments of the present invention, the temperature of the tempering treatment is 130-200° C., and the time of the tempering treatment is 12-18 hours.

[0054] According to some preferred embodiments of the present invention, the tempering treatment step is: treating at 130-140° C. for 3-6 hours and then treating at 160-180° C. for 5-12 hours.

[0055] The purpose of tempering under the above conditions is to cause the molecular chain to creep at high temperature above the glass transition temperature, thereby eliminating the molecular stress generated by the free foaming process, while eliminating the remaining foaming agent and other low-molecular substances in the foam, thereby enhancing the stability of the foam under high-temperature use.

[0056] The invention uses monomers of methacrylic acid, acrylonitrile, N,N-dimethylformamide, heat-resistant additives, antioxidants, toughening modifiers, initiators, foaming agents and crosslinking agents as basic raw materials, polymerizes to form hard, transparent and bubble-free methacrylic acid-methacrylonitrile-prepolymer (prepolymer) under the premise that the foaming agent is not decomposed; then performs heating pretreatment to make the heat in the material uniform before foaming and no heat gradient exists; then foaming is performed to make the foaming agent decompose to generate gas and foam to form a polymethacrylimide foam material with uniform pores; then performs tempering treatment to remove the internal stress of the foam formed by foaming and the small molecular substances remaining in the pores and between molecular chains, thereby significantly improving the thermal stability of the product.

[0057] Under the combined effect of the above raw materials, the foaming molding by the method provided by the present invention is smooth and of high molding quality. The prepared polymethacrylimide foam has uniform pores and similar performance to that of PMI foam using methacrylonitrile.

[0058] A polymethacrylimide foam according to an embodiment of the third aspect of the present invention is used in the fields of aviation, aerospace and rail transportation. DETAILED DESCRIPTION

[0059] To better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments. It should be understood by those skilled in the art that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0060] Unless otherwise specified, the experimental methods used in the examples are all conventional methods; the materials, reagents, etc. used, unless otherwise specified, can be obtained from commercial channels.

[0061] Methacrylic acid: CAS No. 155721;

[0062] N, N-dimethylacrylamide: CAS No. 110-26-9;

[0063] Acrylamide: CAS No. 79-06-1;

[0064] Azobisisobutyronitrile: CAS No. 78-67-1;

[0065] Tert-butyl peroxy(2-ethylhexanoate): CAS No. 3006-82-4;

[0066] Tert-butyl peroxybenzoate: CAS No. 614-45-9;

[0067] Tert-butyl peroxybenzoate: CAS No. 614-45-9;

[0068] Tert-butyl methacrylate: CAS No. 585-07-9;

[0069] N,N-dimethylformamide: CAS No. 585-07-9;

[0070] N-phenylmaleimide: CAS No. 941-69-5;

[0071] Triphenyl phosphite: CAS No. 101-02-0;

[0072] Zinc stearate: CAS No. 557-05-1.

[0073] Example 1

[0074] This embodiment provides a polymethacrylimide foam and a preparation method thereof, specifically:

[0075] This embodiment provides a polymethacrylimide foam, which uses the following components in parts by weight:

[0076] 100 parts of methacrylic acid, 60 parts of N,N-dimethylacrylamide, 30 parts of acrylonitrile, 5 parts of acrylamide;

[0077] Initiator: 0.06 parts of azobisisobutyronitrile, 0.19 parts of bis(4-tert-butylcyclohexyl)peroxydicarbonate, 0.07 parts of tert-butyl peroxy-2-ethylhexanoate, and 0.11 parts of tert-butyl peroxybenzoate;

[0078] Cross-linking agent: 0.3 parts of zinc methacrylate, 12 parts of tert-butyl methacrylate;

[0079] Blowing agent: 2.1 parts of N,N-dimethylformamide, 6.2 parts of tert-butyl alcohol;

[0080] Heat-resistant additive: 0.32 parts of N-phenylmaleimide;

[0081] Antioxidant: 2 parts of triphenyl phosphite;

[0082] Toughening modifier: 0.22 parts of zinc stearate.

[0083] The specific steps of the preparation method of polymethacrylimide foam are:

[0084] S1. Mix the above components evenly according to the ratio to obtain a mixed liquid, and then press the elastomer sealing strip into the edge groove of the fluorine-sprayed stainless steel frame mold. At the same time, cover both sides with clean glass coated with external release agent and fix it firmly with a clamp. Pour the mixed liquid into the mold from the screw hole above the mold, and seal the screw hole with a screw wrapped with raw tape to obtain a reaction device. (The elastomer is rubber, and the specific material is EPDM strip or silicone rubber strip; the mold is 45mm thick, 1000mm long, and 800mm wide) Put the reaction device into the water for polymerization, first keep it at 34℃ for 96h, then increase the temperature by 0.5℃ every 12h, and keep it warm for 48h after heating to 45℃ to obtain a bubble-free prepolymer;

[0085] S2. The foam-free prepolymer is subjected to high temperature pretreatment, foaming demoulding, and tempering post-treatment to obtain a polymethacrylimide foam material;

[0086] The high temperature pretreatment is carried out as follows: the bubble-free prepolymer is heated to 55°C and maintained for 5 hours, then heated to 65°C and maintained for 7 hours, then heated to 75°C and maintained for 8 hours, then heated to 90°C and maintained for 3 hours, and finally heated to 100°C and maintained for 2 hours;

[0087] The non-foamed prepolymer after high-temperature pretreatment is heated and foamed to obtain polymethacrylimide foam with 95% of the pore diameters within the range of 0.4 to 0.8 mm.

[0088] The foaming is carried out as follows: the foam-free prepolymer after high-temperature pretreatment is first heated to 130°C and maintained for 3 hours, then heated to 160°C and maintained for 45 minutes, then heated to 180°C and maintained for 35 minutes, then heated to 205°C and maintained for 35 minutes, and then heated to 220°C and maintained for 2.5 hours;

[0089] The polymethacrylimide foam is subjected to a post-tempering treatment to remove internal stress and residual small molecules. The post-tempering treatment is implemented as follows: the polymethacrylimide foam is first heated to 130°C and maintained for 3.5 hours, then heated to 160°C and maintained for 6 hours, and finally heated to 180°C and maintained for 6 hours.

[0090] Finally, the density is 25-35 kg / m 3 Polymethacrylimide foam material, the heat deformation temperature of which is greater than 180°C at normal pressure (DIN 53424 Test of rigid foam materials - Determination of thermal stability of material shape under bending load and pressure load (pressure load));

[0091] The 3h hot pressing creep rate at 150℃ and 0.3MPa is less than 0.35% (GB / T 15048-1994 Compression creep test method for rigid foam plastics (Method B));

[0092] The room temperature compression strength is greater than 0.4Mpa (GB / T 8813-2008 Compression test method for rigid foam plastics).

[0093] Example 2

[0094] This embodiment provides a polymethacrylimide foam and a preparation method thereof, specifically:

[0095] This embodiment provides a polymethacrylimide foam, which uses the following components in parts by weight:

[0096] 90 parts of methacrylic acid, 65 parts of N,N-dimethylacrylamide, 9 parts of acrylamide;

[0097] Initiator: 0.05 parts of dilauroyl peroxide, 0.18 parts of bis(4-tert-butylcyclohexyl)peroxydicarbonate, 0.16 parts of tert-butyl peroxy-2-ethylhexanoate, and 0.09 parts of tert-butyl perbenzoate;

[0098] Cross-linking agent: 0.3 parts of zinc methacrylate, 1.8 parts of itaconic acid, 1.9 parts of tert-butyl methacrylate;

[0099] Foaming agent: 2.8 parts of formamide, 1.3 parts of tert-butyl alcohol, 2.8 parts of isopropanol;

[0100] Heat-resistant additive: 0.34 parts of N,N'-(4,4'-methylenediphenyl)bismaleimide;

[0101] Toughening modifier: 0.23 parts of zinc stearate.

[0102] The specific steps of the preparation method of polymethacrylimide foam are:

[0103] S1. After mixing the above components evenly according to the ratio to obtain a mixed liquid, press the elastomer sealing strip into the edge groove of the fluorine-sprayed stainless steel frame mold, and cover both sides with clean glass coated with external release agent and fix it firmly with a clamp, pour the mixed liquid into the mold from the screw hole above the mold, and seal the screw hole with a screw wrapped with raw tape to obtain a reaction device. (The elastomer is rubber, and the specific material is EPDM strip or silicone rubber strip; the thickness of the mold is 45mm, the length is 1000mm, and the width is 800mm) Put the reaction device into the water area for polymerization, first keep it at 32℃ for 48h, cool it down to 29℃ after the reaction and keep it for 96h, after obtaining a transparent prepolymer, heat it up to 35℃ for 12h, then heat it up to 40℃ for 12h, then heat it up to 42.5℃ for 12h, and finally heat it up at 45℃ for 24h to obtain a bubble-free prepolymer; in order to avoid excessive reaction in step S1, the reaction is carried out by first cooling and then heating.

[0104] S2. The foam-free prepolymer is subjected to high temperature pretreatment, foaming demoulding, and tempering post-treatment to obtain a polymethacrylimide foam material;

[0105] The high temperature pretreatment is carried out as follows: the bubble-free prepolymer is heated to 55°C and maintained for 8 hours, 60°C and maintained for 7 hours, then heated to 80°C and maintained for 6 hours, then heated to 90°C and maintained for 3 hours, and finally heated to 100°C and maintained for 3 hours;

[0106] The foaming of the foam-free prepolymer after high temperature pretreatment is heated to obtain a polymethacrylimide foam in which 95% of the pore sizes are within the range of 0.2 to 0.6 mm (untempered foam properties: heat deformation temperature is 160° C. (DIN 53424 Test of rigid foam materials - Determination of thermal stability of material shape under bending load and pressure load (pressure load)), and the 3h hot pressing creep rate under 150° C. and 0.3 MPa conditions is less than 0.5% (GB / T 15048-1994 Compression creep test method for rigid foam plastics (method B)); wherein the foaming is carried out according to the following method: the foam-free prepolymer after high temperature pretreatment is first heated to 120° C. and maintained for 2.5 hours, then heated to 145° C. and maintained for 1 hour, then heated to 165° C. and maintained for 30 minutes, then heated to 195° C. and maintained for 35 minutes, and then heated to 210° C. and maintained for 3 hours;

[0107] The polymethacrylimide foam is subjected to a post-tempering treatment to remove internal stress and residual small molecules. The post-tempering treatment is implemented as follows: the polymethacrylimide foam is first heated to 130°C and maintained for 3.5 hours, then heated to 165°C and maintained for 6 hours, and then heated to 180°C and maintained for 6 hours.

[0108] Finally, the density can be obtained to be 50-70 kg / m 3Polymethacrylimide foam, the heat deformation temperature of this foam is greater than 180°C;

[0109] The 3h hot pressing creep rate at 150℃ and 0.3MPa is less than 0.3%;

[0110] The room temperature compression strength is greater than 1.2Mpa (GB / T 8813-2008 Compression test method for rigid foam plastics).

[0111] Example 3

[0112] This embodiment provides a polymethacrylimide foam and a preparation method thereof, specifically:

[0113] This embodiment provides a polymethacrylimide foam and a preparation method thereof, specifically:

[0114] 100 parts of methacrylic acid, 40 parts of acrylonitrile, 40 parts of N,N-dimethylacrylamide;

[0115] Initiator: 0.08 parts of azobisisobutyronitrile, 0.23 parts of bis(4-tert-butylcyclohexyl)peroxydicarbonate, 0.19 parts of tert-butyl peroxy-2-ethylhexanoate, and 0.11 parts of tert-butyl peroxybenzoate;

[0116] Cross-linking agent: 1.7 parts of magnesium methacrylate, 2.1 parts of itaconic acid, 3.5 parts of tert-butyl methacrylate;

[0117] Foaming agent: 2.0 parts of N,N-dimethylformamide, 1.5 parts of isopropanol;

[0118] Heat-resistant additive: 0.35 parts of N,N'-(4,4'-methylenediphenyl)bismaleimide;

[0119] Antioxidant: 0.29 parts of tris[2,4-di-tert-butylphenyl]phosphite;

[0120] Toughening modifier: 0.25 parts of zinc stearate.

[0121] The specific steps of the preparation method of polymethacrylimide foam are:

[0122] S1. Mix the above components evenly according to the ratio to obtain a mixed liquid, and then press the elastomer sealing strip into the edge groove of the fluorine-sprayed stainless steel frame mold. At the same time, cover both sides with clean glass coated with external release agent and fix it firmly with a clamp. Pour the mixed liquid into the mold from the screw hole above the mold, and seal the screw hole with a screw wrapped with raw tape to obtain a reaction device. (The elastomer is rubber, and the specific material is EPDM strip or silicone rubber strip; the mold is 45mm thick, 1000mm long, and 800mm wide) Put the reaction device into the water for polymerization, first keep it at 34℃ for 150h to obtain a transparent prepolymer, then keep it at 40℃ for 12h, and keep it at 45℃ for 24h to obtain a bubble-free prepolymer;

[0123] S2. The foam-free prepolymer is subjected to high temperature pretreatment, foaming demoulding, and tempering post-treatment to obtain a polymethacrylimide foam material;

[0124] The high temperature pretreatment is carried out as follows: the bubble-free prepolymer is heated to 50°C and maintained for 5 hours, then heated to 55°C and maintained for 5 hours, then heated to 65°C and maintained for 7 hours, then heated to 80°C and maintained for 3 hours, and finally heated to 95°C and maintained for 3 hours;

[0125] The foaming of the foam-free prepolymer after high-temperature pretreatment is carried out by heating to obtain a polymethacrylimide foam in which 95% of the pore sizes are within the range of 0.3 to 1 mm (untempered foam properties: heat deformation temperature is 160° C. (DIN 53424 Test of rigid foam materials - Determination of thermal stability of material shape under bending load and pressure load (pressure load)), and the 3h hot pressing creep rate under 150° C. and 0.3 MPa conditions is less than 0.7% (GB / T 15048-1994 Compression creep test method for rigid foam plastics (method B)); wherein the foaming is carried out according to the following method: the foam-free prepolymer after high-temperature pretreatment is first heated to 145° C. and maintained for 3 hours, then heated to 165° C. and maintained for 45 minutes, then heated to 200° C. and maintained for 35 minutes, and finally heated to 210° C. and maintained for 3 hours.

[0126] Then, the polymethacrylimide foam is subjected to a tempering post-treatment to remove internal stress and residual small molecules. The tempering post-treatment is implemented as follows: the polymethacrylimide foam is first heated to 130° C. and maintained for 3 hours, then heated to 160° C. and maintained for 6 hours, and then heated to 180° C. and maintained for 6 hours.

[0127] The density is 50~120 kg / m 3 Polymethacrylimide foam. The heat deformation temperature of this foam is greater than 180°C (DIN 53424 Test of rigid foam materials - Determination of thermal stability of material shape under bending load and pressure load (pressure load));

[0128] The 3h hot pressing creep rate at 150℃ and 0.3MPa is less than 0.3% (GB / T 15048-1994 Compression creep test method for rigid foam plastics (Method B));

[0129] The room temperature compression strength is greater than 1.0Mpa (GB / T 8813-2008 Compression test method for rigid foam plastics).

[0130] Example 4

[0131] This embodiment provides a polymethacrylimide foam and a preparation method thereof, specifically:

[0132] This embodiment provides a polymethacrylimide foam, which uses the following components in parts by weight:

[0133] 90 parts of methacrylic acid, 40 parts of acrylonitrile, 45 parts of N,N-dimethylacrylamide, 5 parts of acrylamide;

[0134] Initiator: 0.1 parts of azobisisobutyronitrile, 0.3 parts of bis(4-tert-butylcyclohexyl)peroxydicarbonate, 0.20 parts of tert-butyl peroxy-2-ethylhexanoate, and 0.11 parts of tert-butyl perbenzoate;

[0135] Cross-linking agent: 5 parts of acrylamide, 0.6 parts of zinc methacrylate, 1.3 parts of itaconic acid, 3.3 parts of tert-butyl methacrylate;

[0136] Foaming agent: 1.5 parts of formamide, 1.5 parts of isopropanol, 1.0 parts of tert-butanol;

[0137] Heat-resistant additive: 0.35 parts of N-phenylmaleimide;

[0138] Antioxidant: 0.69 parts of tris[2,4-di-tert-butylphenyl]phosphite;

[0139] Toughening modifier: 0.15 parts of zinc stearate.

[0140] The specific steps of the preparation method of polymethacrylimide foam are:

[0141] S1. Mix the above components evenly according to the ratio to obtain a mixed liquid, and then press the elastomer sealing strip into the edge groove of the fluorine-sprayed stainless steel frame mold. At the same time, cover both sides with clean glass coated with external release agent and fix it firmly with a clamp. Pour the mixed liquid into the mold from the screw hole above the mold, and seal the screw hole with a screw wrapped with raw tape to obtain a reaction device. (The elastomer is rubber, and the specific material is EPDM strip or silicone rubber strip; the mold is 45mm thick, 1000mm long, and 800mm wide) Put the reaction device into the water for polymerization, first keep it at 34℃ for 150h to obtain a transparent prepolymer, then keep it at 40℃ for 12h, and keep it at 45℃ for 24h to obtain a bubble-free prepolymer;

[0142] S2. The foam-free prepolymer is subjected to high temperature pretreatment, foaming demoulding, and tempering post-treatment to obtain a polymethacrylimide foam material;

[0143] The high temperature pretreatment is carried out as follows: the bubble-free prepolymer is heated to 50°C and maintained for 5 hours, then 55°C and maintained for 6 hours, then heated to 60°C and maintained for 7 hours, then heated to 80°C and maintained for 6 hours, and finally heated to 100°C and maintained for 2 hours;

[0144] The foaming of the foam-free prepolymer after high temperature pretreatment is heated to obtain a polymethacrylimide foam in which 95% of the pore sizes are within the range of 100 to 300 μm (untempered foam properties: heat deformation temperature is 190° C. (DIN 53424 Test of rigid foam materials - Determination of thermal stability of material shape under bending load and pressure load (pressure load)), and the 3h hot pressing creep rate under 150° C. and 0.5 MPa conditions is less than 0.5% (GB / T 15048-1994 Compression creep test method for rigid foam plastics (method B)); wherein the foaming is carried out according to the following method: the foam-free prepolymer after high temperature pretreatment is first heated to 140° C. and maintained for 2 hours, then heated to 175° C. and maintained for 35 minutes, then heated to 200° C. and maintained for 35 minutes, then heated to 205° C. and maintained for 3 hours;

[0145] The polymethacrylimide foam is subjected to a post-tempering treatment to remove internal stress and residual small molecules. The post-tempering treatment is carried out as follows: the polymethacrylimide foam is first heated to 130°C and maintained for 3 hours, then heated to 160°C and maintained for 6 hours, and then heated to 180°C and maintained for 6 hours.

[0146] The density can be 90~220 kg / m 3 High temperature resistant polymethacrylimide foam, the heat deformation temperature of which is greater than 210°C (DIN 53424 Test of rigid foam materials - Determination of the thermal stability of the material shape under bending load and pressure load (pressure load));

[0147] The 3h hot pressing creep rate at 150℃ and 0.5MPa is less than 0.1% (GB / T 15048-1994 Compression creep test method for rigid foam plastics (Method B));

[0148] The room temperature compression strength is greater than 2.5Mpa (GB / T 8813-2008 Compression test method for rigid foam plastics).

[0149] The density of the foam obtained in Example 4 is relatively the highest. Under the same test conditions, the higher the density of the same foam, the higher the compression strength and heat deformation temperature, and the smaller the hot compression creep rate.

[0150] Example 5

[0151] This embodiment provides a polymethacrylimide foam and a preparation method thereof, specifically:

[0152] This embodiment provides a polymethacrylimide foam, which uses the following components in parts by weight:

[0153] 100 parts of methacrylic acid, 60 parts of N,N-dimethylacrylamide, 20 parts of acrylonitrile, 5 parts of acrylamide;

[0154] Initiator: 0.12 parts of dilauroyl peroxide, 0.25 parts of bis(4-tert-butylcyclohexyl)peroxydicarbonate, 0.25 parts of tert-butyl peroxy-2-ethylhexanoate, and 0.12 parts of tert-butyl perbenzoate;

[0155] Cross-linking agent: 0.5 parts of zinc methacrylate, 2.7 parts of tert-butyl methacrylate;

[0156] Blowing agent: 3.0 parts of tert-butyl alcohol;

[0157] Heat-resistant additive: 1 part of N-phenylmaleimide;

[0158] Antioxidant: 0.69 parts of tris[2,4-di-tert-butylphenyl]phosphite;

[0159] Toughening modifier: 0.46 parts of zinc stearate.

[0160] The specific steps of the preparation method of polymethacrylimide foam are:

[0161] S1. Mix the above components evenly according to the ratio to obtain a mixed liquid, and then press the elastomer sealing strip into the edge groove of the fluorine-sprayed stainless steel frame mold. At the same time, cover both sides with clean glass coated with external release agent and fix it firmly with a clamp. Pour the mixed liquid into the mold from the screw hole above the mold, and seal the screw hole with a screw wrapped with raw tape to obtain a reaction device. (The elastomer is rubber, and the specific material is EPDM strip or silicone rubber strip; the mold is 45mm thick, 1000mm long, and 800mm wide) Put the reaction device into the water for polymerization, first keep it at 34℃ for 150h to obtain a transparent prepolymer, then keep it at 40℃ for 12h, and keep it at 45℃ for 24h to obtain a bubble-free prepolymer;

[0162] S2. The foam-free prepolymer is subjected to high temperature pretreatment, foaming demoulding, and tempering post-treatment to obtain a polymethacrylimide foam material;

[0163] The high temperature pretreatment is carried out as follows: the bubble-free prepolymer is heated to 50°C and maintained for 7 hours, then maintained at 60°C for 6 hours, then heated to 80°C and maintained for 6 hours, and then heated to 100°C and maintained for 4 hours;

[0164] Then, the high-temperature pretreated non-foamed prepolymer is heated and foamed to obtain a polymethacrylimide foam in which 95% of the pore sizes are within the range of 10 to 100 μm (untempered foam properties: heat deformation temperature is 160° C. (DIN 53424 Test of rigid foam materials - Determination of thermal stability of material shape under bending load and pressure load (pressure load)), and the 3h hot pressing creep rate under 150° C. and 0.3 MPa is less than 0.9% (GB / T 15048-1994 Compression creep test method for rigid foam plastics (method B)); wherein the foaming is carried out according to the following method: the high-temperature pretreated non-foamed prepolymer is first heated to 145° C. and maintained for 2 hours, then heated to 170° C. and maintained for 1 hour, and finally heated to 200° C. and maintained for 3 hours;

[0165] Then, the polymethacrylimide foam is subjected to a tempering post-treatment to remove internal stress and residual small molecules. The tempering post-treatment is implemented as follows: the polymethacrylimide foam is first heated to 130° C. and maintained for 3 hours, then heated to 160° C. and maintained for 6 hours, and then heated to 180° C. and maintained for 6 hours.

[0166] The density is 20~130 kg / m 3 Polymethacrylimide foam, the heat deformation temperature of which is greater than 180 ° C (DIN 53424 Test of rigid cellular materials - Determination of the thermal stability of the material shape under bending load and pressure load (pressure load));

[0167] The 3h hot pressing creep rate at 150℃ and 0.3MPa is less than 0.5% (GB / T 15048-1994 Compression creep test method for rigid foam plastics (Method B));

[0168] The room temperature compression strength is greater than 0.3Mpa (GB / T 8813-2008 Compression test method for rigid foam plastics).

[0169] Comparative Example 1

[0170] This comparative example provides a polymethacrylimide foam and a preparation method thereof. The difference between this example and the comparative example is that methacrylonitrile is added in this comparative example, specifically:

[0171] This embodiment provides a polymethacrylimide foam and a preparation method thereof, specifically:

[0172] This embodiment provides a polymethacrylimide foam, which uses the following components in parts by weight:

[0173] 100 parts of methacrylic acid, 75 parts of methacrylonitrile;

[0174] Initiator: 0.05 parts of azobisisobutyronitrile, 0.18 parts of bis(4-tert-butylcyclohexyl)peroxydicarbonate, 0.07 parts of tert-butyl peroxy-2-ethylhexanoate, and 0.12 parts of tert-butyl perbenzoate;

[0175] Cross-linking agent: 0.3 parts of magnesium methacrylate, 12 parts of tert-butyl methacrylate;

[0176] Blowing agent: 6.1 parts of N,N-dimethylformamide, 6.2 parts of isoalcohol;

[0177] Heat-resistant additive: 0.32 parts of N-phenylmaleimide;

[0178] Antioxidant: Antioxidant 168 0.16 parts;

[0179] Toughening modifier: 0.22 parts of zinc stearate.

[0180] The specific steps of the preparation method of polymethacrylimide foam are as follows:

[0181] In this embodiment, methacrylonitrile, a relatively expensive raw material, is used to react and polymerize with methacrylic acid and other additives to prepare polymethacrylimide foam. The procurement cost of methacrylonitrile raw material is 7 to 8 times higher than that of acrylonitrile and N, N-dimethylacrylamide. Accordingly, the production cost of polymethacrylimide foam prepared by using methacrylonitrile under the same process conditions is relatively high.

[0182] The density is 50~130 kg / m 3Polymethacrylimide foam material, the heat deformation temperature of which is greater than 180°C at normal pressure (DIN 53424 Test of rigid foam materials - Determination of thermal stability of material shape under bending load and pressure load (pressure load));

[0183] The 3h hot pressing creep rate at 150℃ and 0.3MPa is less than 0.3% (GB / T 15048-1994 Compression creep test method for rigid foam plastics (Method B));

[0184] The room temperature compression strength is greater than 0.6Mpa (GB / T 8813-2008 Compression test method for rigid foam plastics).

[0185] Comparative Example 2

[0186] This comparative example provides a polymethacrylimide foam and a preparation method thereof. The difference between this comparative example and Example 1 is that in the foaming molding step S2 of this comparative example, gradient heating is not used but single heating is used.

[0187] During the foaming process of this comparative example, the board is unstable, the local foaming speed is too fast, cracking and curling occur, and a flat foam board cannot be obtained.

[0188] Comparative Example 3

[0189] This comparative example provides a polymethacrylimide foam and a preparation method thereof. The difference between this comparative example and Example 1 is that the heat-resistant additive is tribromophenylmaleimide, and the other conditions are the same.

[0190] The introduction of bromine atoms in the heat-resistant additive of this comparative example may affect the forces and bonding conditions within the molecule, resulting in a decrease in the overall stability of the molecule. This may result in the new compound not being as good as N-phenylmaleimide in terms of heat resistance under high temperature conditions, and increasing the crosslinking degree of the prepolymer and causing difficulty in foaming.

[0191] Comparative Example 4

[0192] This comparative example provides a polymethacrylimide foam and a preparation method thereof. The difference between this comparative example and Example 1 is that the tempering temperature is 120° C., and the other conditions are the same as those in Example 1.

[0193] Comparative Example 5

[0194] This comparative example provides a polymethacrylimide foam and a preparation method thereof. The difference between this comparative example and Example 1 is that the tempering step is not included, and the other conditions are the same as those of Example 1.

[0195] Test Case

[0196] This test example tests the polymethacrylimide foams prepared in the examples and comparative examples. The specific test results are shown in Table 1.

[0197] DIN53424 Inspection of rigid foam materials - Determination of thermal stability of material shape under bending load and pressure load (pressure load);

[0198] GB / T 15048-1994 Compression creep test method for rigid cellular plastics (Method B);

[0199] GB / T 8813-2008 Compression test method for rigid cellular plastics.

[0200] Table 1. Properties of polymethacrylimide foam

[0201]

[0202] The raw materials for preparing the polymethacrylimide provided by the present invention do not include methacrylonitrile. Under the synergistic effect of the raw materials in the present invention, the pore diameter of the polymethacrylimide foam is 0.1 mm to 1 mm, and the density is 25 to 250 kg / m 3 The foam has no obvious discoloration after long-term use at 150℃, the heat deformation temperature is higher than 180℃, the thermal creep at 0.3MPa150℃ is less than 1%, and the density exceeds 200 kg / m 3 The thermal creep at 0.5MPa and 150°C is less than 1%, and the mechanical properties are excellent. The tempering temperature of Comparative Example 4 is low, resulting in a decrease in the stability of the polymethacrylimide foam under high temperature use. Comparative Example 5 does not include a tempering step, and the internal stress and residual small molecules cannot be removed, resulting in a decrease in the thermal stability of the polymethacrylimide foam under high temperature use.

[0203] The above embodiments are merely clear examples of the present invention and are not intended to limit the implementation methods. Those skilled in the art may make various modifications and alterations based thereon, all of which fall within the protection scope of the present invention.

Claims

1. A polymethacrylimide foam, characterized in that: The raw materials for preparing the polymethacrylimide foam include: methacrylic acid, N,N-dimethylacrylamide, acrylonitrile, a third monomer, a toughening modifier, an initiator, a foaming agent and a crosslinking agent; The third monomer includes at least one of acrylamide and methacrylamide; The raw materials for preparing the polymethacrylimide foam do not include methacrylonitrile.

2. The polymethacrylimide foam according to claim 1, characterized in that: The raw materials for preparing the polymethacrylimide foam further include: a heat-resistant additive; the heat-resistant additive includes: at least one of N, N'-(4, 4'-methylenediphenyl) bismaleimide and N-phenylmaleimide.

3. The polymethacrylimide foam according to claim 1, characterized in that: The raw materials for preparing the polymethacrylimide foam further include: an antioxidant; the antioxidant includes triphenyl phosphite.

4. The polymethacrylimide foam according to any one of claims 1 to 3, characterized in that: The initiator includes at least one of a peroxide and an azo compound.

5. The polymethacrylimide foam according to any one of claims 1 to 3, characterized in that: The foaming agent includes at least one of an amide foaming agent and an alcohol foaming agent.

6. The polymethacrylimide foam according to any one of claims 1 to 3, characterized in that: The cross-linking agent includes at least one of zinc methacrylate, magnesium methacrylate, allyl methacrylate, itaconic acid, tert-butyl methacrylate, acrylamide and methacrylamide.

7. A method for preparing a polymethacrylimide foam as claimed in any one of claims 1 to 6, characterized in that: The following steps are involved: S1. The raw materials for preparing the polymethacrylimide foam are mixed and reacted to obtain a prepolymer; S2. The prepolymer obtained in step S1 is pre-treated by heating, foamed and then tempered.

8. The method for preparing polymethacrylimide foam according to claim 7, characterized in that: In step S2, the heating temperature of the heating pretreatment is 50-110°C, and the heating time of the heating pretreatment is 20-35h.

9. The method for preparing polymethacrylimide foam according to claim 7, characterized in that: The foaming molding steps include: a first stage of foaming heating, a second stage of foaming heating, a third stage of foaming heating and a fourth stage of foaming heating; The temperature of the first stage of foaming and heating is 110-150°C, and the time of the first stage of foaming and heating is 2-5h; The temperature of the second stage of foaming and heating is 160-185°C, and the time of the second stage of foaming and heating is 30-90 minutes; The temperature of the third stage of foaming and heating is 195-205°C, and the time of the third stage of foaming and heating is 30-60 minutes; The temperature of the fourth stage of foaming and heating is 205-220° C., and the time of the fourth stage of foaming and heating is 2-4 hours.

10. Use of the polymethacrylimide foam according to any one of claims 1 to 6 in the fields of aviation, aerospace and rail transportation.