Photo-thermal dual-curing glass-like polymer and preparation method thereof
Through the photothermal double curing method, the combination of modified resin and transesterification catalyst is combined to form a carbon-carbon double bond structure, which solves the problems of high energy consumption and poor mechanical properties of glass-like polymers during the curing process, and achieves efficient production and excellent results Glass-like polymer with mechanical properties.
Patent Information
- Application Number
- CN202411044455.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-12-03
AI Technical Summary
The existing glass-like polymers consume high energy and have poor mechanical properties during curing, which limits their application in the field of materials.
Using the photothermal double curing method, through the combination of modified resin, transesterification catalyst, reactive diluent and initiator, chemical reactions are initiated using light sources or thermal fields to form a carbon-carbon double bond structure, achieving rapid curing and optimizing the three-dimensional crosslinking network Structure, improve mechanical properties.
It significantly improves the production efficiency of glass-like polymers, reduces energy consumption during curing and forming, and ensures the high performance of the products, and has excellent mechanical properties and network recombination capabilities.
Smart Images

Figure CN119060245A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of polymer synthesis, and in particular relates to a glass-like polymer capable of photothermal dual curing and a preparation method thereof. Background Art
[0002] The network structure of thermosetting resin brings excellent mechanical properties and corrosion resistance. Combining it with reinforced fibers to make composite materials further strengthens its advantages, which establishes the important position of thermosetting resin in the field of materials. However, its insoluble and non-melting properties bring difficulties to environmental governance. Therefore, promoting the research of new biodegradable and reprocessable resins is of great significance to its development.
[0003] Introducing reversible covalent bonds into thermosetting resins can prepare a dynamic polymer - glass-like polymer. This type of material is a cross-linked polymer with the properties of thermosetting materials below the glass transition temperature (Tg), but above the topological network solidification transition temperature (Tv), it can undergo a reversible exchange reaction, while maintaining the number and type of covalent bonds unchanged, rearranging its network topology, thus having thermal reversibility. At the same time, the dissociation reaction of its reversible covalent bonds also enables it to undergo chemical degradation under certain conditions. Therefore, this type of dynamic polymer is expected to become a new type of resin with both mechanical properties and reprocessing properties.
[0004] However, existing glass-like polymers have high curing energy consumption and poor mechanical properties. Summary of the invention
[0005] Based on the above problems, the present invention provides a glass-like polymer that can be subjected to photothermal dual curing and a preparation method thereof. The method can not only significantly improve the production efficiency of the glass-like polymer and reduce the energy consumption in the curing and molding process, but also the high-precision and stable process molding process effectively ensures the high performance of the product.
[0006] The first aspect of the present invention provides a method for preparing a glass-like polymer capable of photothermal dual curing, comprising:
[0007] (1) Mixing a modified resin, an ester exchange catalyst, a reactive diluent and an initiator, wherein the initiator comprises a thermal initiator and / or a photoinitiator, wherein the modified resin has the following structure:
[0008]
[0009] Among them, R 1 for R 2 is a hydrogen atom or a methyl group, R 3 is a hydrogen atom or a methyl group or a benzene ring;
[0010] (2) Adding an external light source or an external heating field to the product obtained in step (1) to obtain a glass-like polymer.
[0011] Furthermore, the raw materials for preparing the modified resin include epoxy resin, unsaturated carboxylic acid and ester exchange catalyst.
[0012] Furthermore, the molar ratio of the epoxy resin, the unsaturated carboxylic acid and the transesterification catalyst is 1:(2-4):(0.02-0.2).
[0013] Furthermore, the epoxy resin, the unsaturated carboxylic acid and the transesterification catalyst are mixed, the stirring speed is controlled to be 200-500 r / min, the mixture is reacted at 120° C.-140° C. for at least 1 hour, and excess unsaturated carboxylic acid is removed to obtain the modified resin.
[0014] Furthermore, the epoxy resin includes at least one of bisphenol A diglycidyl ether, bisphenol F diglycidyl ether, difunctional glycidyl ether and multifunctional glycidyl ether.
[0015] Furthermore, the unsaturated carboxylic acid includes at least one of acrylic acid, methacrylic acid, crotonic acid, cinnamic acid, sorbic acid, maleic acid and trans-butenedioic acid.
[0016] Furthermore, the transesterification catalyst includes at least one of an amine catalyst, an amine having an amidine group and a derivative thereof.
[0017] Furthermore, the reactive diluent includes at least one of a monofunctional acrylate derivative, a difunctional acrylate derivative, a multifunctional acrylate derivative and an acrylic acid-modified compound.
[0018] Furthermore, the thermal initiator includes at least one of the free radical initiators ester peroxide, acyl peroxide, ketone peroxide, and azo initiator.
[0019] Furthermore, the photoinitiator includes at least one of acylphosphine oxides, benzophenones and benzil types.
[0020] Furthermore, the modified resin, the transesterification catalyst, the active diluent, the initiator and other additives are mixed, and the other additives include at least one of a toughening agent, a defoaming agent, a leveling agent and an antioxidant.
[0021] Furthermore, the mass ratio of the modified resin, the transesterification catalyst, the active diluent and the initiator is (25-60): (2-5): (45-75): (0.5-2.5).
[0022] The second aspect of the present invention provides a glass-like polymer capable of photothermal dual curing, which is prepared by the method described in the first aspect.
[0023] Compared with the prior art, the present invention has at least the following beneficial effects:
[0024] (1) The present invention provides a method for preparing glass-like polymers by applying an external light source or a heat field. This method can not only achieve rapid curing at room temperature and avoid side reactions or catalyst deactivation at high temperatures, but also its system composition makes it easier to achieve regulation of resin properties.
[0025] (2) The glass-like polymer prepared by the present invention can be cured under the action of a single external heating field or light source, or can be cured by a dual photothermal curing method, due to the carbon-carbon double bond structure in its structure, which brings excellent time and space selectivity to the processing of the product. In addition, the rigid network constructed based on the carbon-carbon double bond enables the photocurable glass-like polymer to have excellent mechanical properties, making it have the potential to be used as a matrix for photocurable composite materials, thereby giving the composite materials reprocessing properties.
[0026] (3) The present invention modifies epoxy resin with unsaturated carboxylic acid, constructs β-hydroxy ester bond as the reversible covalent bond of the system, and introduces carbon-carbon double bond as the basis of rigid network structure. By optimizing the ratio of the modified resin system, its three-dimensional cross-linked network structure is improved, the mechanical properties and network reorganization ability of the glass-like polymer are regulated, and a rigid glass-like polymer with good mechanical properties and network reorganization ability is prepared. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 is the infrared spectrum of phenol A diglycidyl ether, methacrylic acid and modified resin A1 in Example 1;
[0028] Figure 2 This is the infrared spectrum of the glass-like polymer of Example 1 before and after curing. DETAILED DESCRIPTION
[0029] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments, and the following examples are only descriptive, not restrictive, and cannot be used to limit the scope of protection of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0030] The present invention is further described in detail below in conjunction with the embodiments. The technical solution of the present application is based on the following principles: glass-like polymers are cross-linked polymers with thermosetting material properties below the glass transition temperature (Tg), but above the topological network solidification transition temperature (Tv), they can undergo reversible exchange reactions under the action of a catalyst, while maintaining the number and type of covalent bonds unchanged, while rearranging their network topological structure, thereby having thermally reversible properties. However, traditional glass-like polymer thermoforming processes usually require harsh conditions of high temperature, high pressure, and long periods of time, and their long production cycles also lead to higher energy consumption. In addition, the processing of large products and high-precision products also has high requirements for molding equipment, which further limits the development of thermoforming processes in some application scenarios.
[0031] The photocuring reaction is a chemical reaction initiated by a light source with a certain amount of energy. The reaction system consists of monomers or oligomers, active diluents and photoinitiators. The ground state molecules of the initiator absorb light energy and undergo electronic transitions to become excited state molecules. The excited state molecules cannot exist stably due to their high energy. Some of them are inactivated, and the other part undergoes electron and energy transfer to become active species. Free radical photoinitiators can produce free radical active species, inducing unsaturated resins to undergo addition reactions on carbon-carbon double bonds (C=C), and then cross-link to form a three-dimensional network molecular structure. This method can not only achieve rapid curing at room temperature, avoiding side reactions or catalyst deactivation at high temperatures, but also its system composition makes it easier to control the properties of the resin.
[0032] Based on this, the first aspect of the present invention provides a method for preparing a glass-like polymer capable of photothermal dual curing, the method comprising:
[0033] S1: Mix the modified resin, transesterification catalyst, active diluent and initiator to react
[0034] According to an embodiment of the present invention, the structural formula of the modified resin is
[0035] Among them, R 1 for R 2 is a hydrogen atom or a methyl group, R 3 It is a hydrogen atom, a methyl group or a benzene ring.
[0036] Further, the raw materials for preparing the modified resin include epoxy resin, unsaturated carboxylic acid and ester exchange catalyst. Specifically, the preparation method includes: mixing the epoxy resin, the unsaturated carboxylic acid and the ester exchange catalyst, controlling the stirring speed to 200-500r / min, reacting at least 1h under the condition of 120℃-140℃, and removing the excess unsaturated carboxylic acid to obtain the modified resin. In this process, the epoxy group in the epoxy resin and the carboxylic acid group in the unsaturated carboxylic acid form a β-hydroxy ester bond under the action of the ester exchange catalyst. The ester bond has a reversible reaction that exchanges with each other, and the hydroxyl group can provide more dynamic reaction sites, so that the system has a network reorganization ability, so that it is easy to form hydrogen bonds after subsequent curing to further improve the mechanical properties. At the same time, the double bonds introduced into the molecular chain at both ends by the unsaturated carboxylic acid are extremely active, so that the modified resin can be quickly cured to form a highly cross-linked rigid network structure, so that it has good mechanical properties and corrosion resistance.
[0037] Furthermore, the molar ratio of the epoxy resin, the unsaturated carboxylic acid and the transesterification catalyst is 1:(2-4):(0.02-0.2). Thus, by controlling the raw materials for preparing the modified resin within the above range, the three-dimensional cross-linked network structure of the modified resin is improved, the mechanical properties and network reorganization ability of the glass-like polymer are regulated, and a rigid glass-like polymer with good mechanical properties and network reorganization ability is prepared.
[0038] According to an embodiment of the present invention, the epoxy resin in the raw materials used for the modified resin includes at least one of bisphenol A diglycidyl ether, bisphenol F diglycidyl ether, difunctional glycidyl ether such as (poly)ethylene glycol diglycidyl ether, and multifunctional glycidyl ether such as glycerol triglycidyl ether. The epoxy resin described in the present invention has the following characteristics: ① It contains two or more highly active terminal epoxy groups that can participate in the ring-opening esterification reaction; ② It is liquid at room temperature, has moderate viscosity, and the reaction process with carboxylic acid is easy to design.
[0039] According to an embodiment of the present invention, the unsaturated carboxylic acid in the raw material used for the modified resin includes at least one of carboxylic acids containing single or multiple carbon-carbon double bonds, such as acrylic acid, methacrylic acid, crotonic acid, cinnamic acid, sorbic acid, cis / trans butenedioic acid, etc. The unsaturated carboxylic acid in the present invention has the following characteristics: ① containing one or more carboxyl groups, which can undergo a ring-opening esterification reaction with the epoxy group in the epoxy resin; ② containing one or more unsaturated bonds, thereby participating in the construction of a carbon-carbon rigid skeleton; ③ the melting point is not higher than 140°C, and the boiling point is not higher than 160°C, so that the reaction system can form a homogeneous state.
[0040] According to an embodiment of the present invention, the ester exchange catalyst in the modified resin raw material includes at least one of an amine catalyst, an amine having an amidine group and its derivatives, such as one or more of 1,5,7-triazidebicyclo(4.4.0)dec-5-ene, stannous octoate, 1,8-diazabicyclo[5.4.0]undec-7-ene, and 1,5-diazabicyclo(4.3.0)non-5-ene.
[0041] In this step, the modified resin is mixed with an ester exchange catalyst, an active diluent and an initiator, wherein the initiator includes an initiator and / or a photoinitiator. The active diluent can adjust the viscosity of the system to improve its photocuring performance on the one hand, and can adjust the network structure of the resin after curing to change its mechanical properties on the other hand.
[0042] According to an embodiment of the present invention, the mass ratio of the modified resin, the transesterification catalyst, the active diluent and the initiator in the above mixing process is (25-60): (2-5): (45-75): (0.5-2.5). The inventors found that if the active diluent content is too high, the viscosity of the resin system is significantly reduced, and the comprehensive performance of the product after curing is significantly reduced, which is not conducive to the high performance of the composite material. If the active diluent content is too low, there is a concentrated heat release phenomenon during the curing process, which leads to yellowing of the resin; if the photoinitiator content is too high, the absorption of ultraviolet light by the initiator during the photocuring process will cause its penetration depth to decrease, which is not conducive to the deep curing of the product. If the photoinitiator content is too low, the photocuring efficiency is reduced and the curing effect of the product is poor. Therefore, the photothermal dual-curing glass polymer system composed of the present application can be used to prepare rigid glass polymers with excellent mechanical properties and network reorganization capabilities.
[0043] According to an embodiment of the present invention, the reactive diluent includes at least one of a monofunctional acrylate derivative such as 2-hydroxy-3-phenoxypropyl acrylate, a difunctional acrylate derivative such as 2-acrylate-2-hydroxy-1,3-propylene glycol, a multifunctional acrylate derivative such as trimethylolpropane triacrylate, and an acrylic acid modified compound. The reactive diluent in the present invention has the following characteristics: ① It has one or more highly active carbon-carbon double bond groups, which can participate in free radical or cationic reactions in the light / heat curing process; ② It is liquid at room temperature, has a boiling point higher than 150°C, and has a lower viscosity than the modified resin, and can be used to adjust the curing performance of the system.
[0044] According to an embodiment of the present invention, the thermal initiator includes one or more of a free radical initiator ester peroxide such as dicyclohexyl peroxydicarbonate, an acyl peroxide such as benzoyl peroxide, a ketone peroxide such as methyl ethyl ketone peroxide, and an azo initiator such as azobisisoheptonitrile; the photoinitiator includes one or more of an acyl phosphorus oxide such as trimethylbenzoyl-diphenylphosphine oxide, a benzophenone such as 2,4-dihydroxybenzophenone, and a benzil such as α, α-dimethoxy-α-phenylacetophenone; the photo / thermal initiator in the present invention has the following characteristics: ① The state at room temperature can be solid or liquid, has good thermal stability, and has a certain solubility in the resin ③ It can form free radicals or cationic active species under the action of an external light source or a thermal field, thereby initiating carbon-carbon double bond addition crosslinking.
[0045] Furthermore, other additives may be added during the mixing of the modified resin, the transesterification catalyst, the active diluent and the initiator, and the other additives include at least one of a toughening agent, a defoaming agent, a leveling agent and an antioxidant. For example, toughening agents include but are not limited to styrene, polyolefin, polyester products and nanoparticles; defoaming agents include but are not limited to organosilicon and polyether modified silicone oil defoaming agents; leveling agents include but are not limited to polyacrylate, polyether modified silicone oil and polyester modified silicone oil; antioxidants include but are not limited to hindered phenols and aromatic amine antioxidants.
[0046] S2: Adding an external light source or an external heating field to the product obtained in step S1 to obtain a glass-like polymer.
[0047] In this step, according to the product requirements and the type of initiator added, the product obtained in step S1 is fully cured within 30 seconds under the action of an external light source or within 2 hours under the action of an external heating field, that is, the photo / thermal initiator decomposes to produce active species, which then initiates the free radical polymerization reaction of the carbon-carbon double bonds of the glass-like polymer to obtain a glass-like polymer.
[0048] According to an embodiment of the present invention, the wavelength of the ultraviolet light used in the above-mentioned additional light source is in the range of 320 to 400 nm. Specifically, a specific wavelength curing device should be selected according to the type of ultraviolet initiator, and the light intensity should be greater than 8 mW / cm 2 , the irradiation distance is 5-30cm, and the ambient temperature is 20-50℃.
[0049] The present invention provides a method for preparing glass-like polymers by applying an external light source or a thermal field. This method can not only significantly improve the production efficiency of glass-like polymers and reduce energy consumption during the curing and molding process, but also the high-precision and stable molding process effectively ensures the high performance of the product. Specifically, the Tg of the glass-like polymer obtained by the present invention can reach 115.4°C, indicating that it has good heat resistance and dimensional stability; the tensile strength of the light-cured glass-like polymer obtained by the present invention can reach 71.4MPa, and the tensile modulus can reach 2.30GPa, and the tensile strength of the heat-cured glass-like polymer can reach 71.0MPa, and the tensile modulus can reach 2.10GPa, indicating that the glass-like polymers obtained by the two methods have excellent mechanical properties.
[0050] The second aspect of the present invention provides a glass-like polymer capable of photothermal dual curing, which is prepared by the method described in the first aspect. It should be noted that the features and advantages described above for the method for preparing a glass-like polymer capable of photothermal dual curing are also applicable to the glass-like polymer capable of photothermal dual curing, and will not be described in detail here.
[0051] The present invention will be further described below by way of examples, but the protection scope of the present invention is not limited to these embodiments. The present invention may also have other various embodiments, and those skilled in the art may make various corresponding changes and deformations according to the present invention without departing from the spirit and essence of the present invention, but these corresponding changes and deformations shall all belong to the protection scope of the claims attached to the present invention.
[0052] Example 1
[0053] (1) Weigh 10 g of bisphenol A diglycidyl ether, 17.2 g of methacrylic acid and 0.3475 g of 1,5,7-triazidobicyclo(4.4.0)dec-5-ene and mix them uniformly. Control the stirring speed to 300 r / min. React at 130° C. for 1 h. Remove the excess unsaturated carboxylic acid to obtain 18.95 g of modified resin A1 (the infrared spectra of bisphenol A diglycidyl ether, methacrylic acid and modified resin A1 are as follows: Figure 1 shown);
[0054] (2) After the reaction is completed, wait until the system is cooled to below 40° C., weigh 52.24 g of 2-hydroxy-3-phenoxypropyl acrylate, 1.39 g of 1,5,7-triazidobicyclo(4.4.0)dec-5-ene, and 0.72 g of benzoyl peroxide, add them to the modified resin A1, and mix well.
[0055] (3) A certain amount of resin was added to a polytetrafluoroethylene mold and cured in an oven at 100°C for 2 h to obtain a heat-cured glass-like polymer. The infrared spectra of the glass-like polymer before and after curing are shown in FIG. Figure 2 As shown in the figure, it can be seen that after solidification, the carbon-carbon double bond (peak position 1407cm -1 ) peak intensity decreases, indicating that cross-linking and curing occurs, and the system also has a β-hydroxy ester bond structure.
[0056] Example 2
[0057] (1) Weigh 10 g of bisphenol A diglycidyl ether, 17.2 g of methacrylic acid and 0.3475 g of 1,5,7-triazidobicyclo(4.4.0)dec-5-ene and mix them uniformly. Control the stirring speed to 300 r / min. React at 130° C. for 1 h. Remove excess unsaturated carboxylic acid to obtain 18.95 g of modified resin.
[0058] (2) After the reaction is completed, wait until the system is cooled to below 40° C., weigh 26.12 g of 2-hydroxy-3-phenoxypropyl acrylate, 0.695 g of 1,5,7-triazidobicyclo(4.4.0)dec-5-ene, and 0.54 g of benzoyl peroxide, add them to the modified resin, and mix well.
[0059] (3) A certain amount of resin is added into a polytetrafluoroethylene mold and cured in an oven at 100° C. for 2 h to obtain a heat-cured glass-like polymer.
[0060] Example 3
[0061] (1) Weigh 10 g of bisphenol A diglycidyl ether, 17.2 g of methacrylic acid and 0.3475 g of 1,5,7-triazidobicyclo(4.4.0)dec-5-ene and mix them uniformly. Control the stirring speed to 300 r / min. React at 130° C. for 1 h. Remove excess unsaturated carboxylic acid to obtain 18.95 g of modified resin.
[0062] (2) After the reaction is completed, wait until the system is cooled to below 40° C., weigh 13.06 g of 2-hydroxy-3-phenoxypropyl acrylate, 0.3475 g of 1,5,7-triazidobicyclo(4.4.0)dec-5-ene, and 0.32 g of benzoyl peroxide, add them to the modified resin, and mix well.
[0063] (3) A certain amount of resin is added into a polytetrafluoroethylene mold and cured in an oven at 100° C. for 2 h to obtain a heat-cured glass-like polymer.
[0064] Example 4
[0065] (1) Weigh 10 g of bisphenol A diglycidyl ether, 17.2 g of methacrylic acid and 0.3475 g of 1,5,7-triazidobicyclo(4.4.0)dec-5-ene and mix them uniformly. Control the stirring speed to 300 r / min. React at 130° C. for 1 h. Remove excess unsaturated carboxylic acid to obtain 18.95 g of modified resin.
[0066] (2) After the reaction is completed, wait until the system is cooled to below 40° C., weigh 52.24 g of 2-hydroxy-3-phenoxypropyl acrylate, 1.39 g of 1,5,7-triazidobicyclo(4.4.0)dec-5-ene, and 0.72 g of trimethylbenzoyl-diphenylphosphine oxide, add them to the modified resin, and mix well.
[0067] (3) Take a certain amount of resin and add it to the polytetrafluoroethylene mold. Use a 385nm ultraviolet lamp with an irradiation distance of 10cm and a light intensity of 16mW / cm 2 , light-cured for 1 min to obtain a light-cured glass-like polymer.
[0068] Example 5
[0069] (1) Weigh 10 g of bisphenol A diglycidyl ether, 17.2 g of methacrylic acid and 0.3475 g of 1,5,7-triazidobicyclo(4.4.0)dec-5-ene and mix them uniformly. Control the stirring speed to 300 r / min. React at 130° C. for 1 h. Remove excess unsaturated carboxylic acid to obtain 18.95 g of modified resin.
[0070] (2) After the reaction is completed, wait until the system is cooled to below 40° C., weigh 52.24 g of 2-hydroxy-3-phenoxypropyl acrylate, 1.39 g of 1,5,7-triazidobicyclo(4.4.0)dec-5-ene, and 1.44 g of trimethylbenzoyl-diphenylphosphine oxide, add them to the modified resin, and mix them evenly.
[0071] (3) Take a certain amount of resin and add it to the polytetrafluoroethylene mold. Use a 385nm ultraviolet lamp with an irradiation distance of 10cm and a light intensity of 16mW / cm 2 , light-cured for 1 min to obtain a light-cured glass-like polymer.
[0072] Example 6
[0073] (1) Weigh 10 g of bisphenol A diglycidyl ether, 17.2 g of methacrylic acid and 0.3475 g of 1,5,7-triazidobicyclo(4.4.0)dec-5-ene and mix them uniformly. Control the stirring speed to 300 r / min. React at 130° C. for 1 h. Remove excess unsaturated carboxylic acid to obtain 18.95 g of modified resin.
[0074] (2) After the reaction is completed, wait until the system is cooled to below 40° C., weigh 52.24 g of 2-hydroxy-3-phenoxypropyl acrylate, 1.39 g of 1,5,7-triazidobicyclo(4.4.0)dec-5-ene, 0.72 g of trimethylbenzoyl-diphenylphosphine oxide, and 0.72 g of benzoyl peroxide, add them to the modified resin, and mix them evenly.
[0075] (3) Take a certain amount of resin and add it to the polytetrafluoroethylene mold. Use a 385nm ultraviolet lamp with an irradiation distance of 10cm and a light intensity of 16mW / cm 2 , light-cured for 1 minute to obtain a light-thermal dual-cured glass-like polymer.
[0076] Example 7
[0077] (1) Weigh 10 g of bisphenol A diglycidyl ether, 17.2 g of methacrylic acid and 0.3475 g of 1,5,7-triazidobicyclo(4.4.0)dec-5-ene and mix them uniformly. Control the stirring speed to 300 r / min. React at 130° C. for 1 h. Remove excess unsaturated carboxylic acid to obtain 18.95 g of modified resin.
[0078] (2) After the reaction is completed, wait until the system is cooled to below 40° C., weigh 98.4 g of diallyl terephthalate, 1.39 g of 1,5,7-triazidobicyclo(4.4.0)dec-5-ene, and 1.2 g of tert-butyl peroxybenzoate, add them to the modified resin, and mix well.
[0079] (3) A certain amount of resin is added into a polytetrafluoroethylene mold and cured in an oven at 120° C. for 2 h to obtain a heat-cured glass-like polymer.
[0080] Example 8
[0081] (1) Weigh 10 g of bisphenol A diglycidyl ether, 17.2 g of methacrylic acid and 0.3475 g of 1,5,7-triazidobicyclo(4.4.0)dec-5-ene and mix them uniformly. Control the stirring speed to 300 r / min. React at 130° C. for 1 h. Remove excess unsaturated carboxylic acid to obtain 18.95 g of modified resin.
[0082] (2) After the reaction is completed, wait until the system is cooled to below 40° C., weigh 98.4 g of diallyl terephthalate, 1.39 g of 1,5,7-triazidobicyclo(4.4.0)dec-5-ene, and 1.2 g of trimethylbenzoyl-diphenylphosphine oxide, add them to the modified resin, and mix them evenly.
[0083] (3) Take a certain amount of resin and add it to the polytetrafluoroethylene mold. Use a 385nm ultraviolet lamp with an irradiation distance of 10cm and a light intensity of 16mW / cm 2, light-cured for 1 min to obtain a light-cured glass-like polymer.
[0084] Comparative Example
[0085] (1) Weigh 21.2 g of bisphenol A ethoxylated diacrylate, 104.45 g of 2-hydroxy-3-phenoxypropyl acrylate, 3.965 g of 1,5,7-triazidobicyclo(4.4.0)dec-5-ene, and 1.3 g of trimethylbenzoyl-diphenylphosphine oxide, and mix well.
[0086] (2) Take a certain amount of resin and add it to the polytetrafluoroethylene mold. Use a 385nm ultraviolet lamp with an irradiation distance of 10cm and a light intensity of 16mW / cm 2 , light-cured for 1 min to obtain a light-cured glass-like polymer.
[0087] Performance Testing
[0088] 1. Resin mechanical property test: According to GB / T 1040.2-2022, the glass-like polymers prepared in Examples 1-8 and the comparative example were sampled in 1BA-type specimen specifications, with no less than 5 specimens in each group. An Instron 6800 universal material testing machine was used to continuously load the samples at a speed of 1 mm / min at room temperature, and the load-strain results of the samples were recorded. The tensile strength and tensile modulus were calculated as the mechanical property results of the products.
[0089]
[0090] Where, σ is the tensile strength of the sample, in MPa; P max ——The maximum load that the specimen can withstand before failure, in N; w——The width of the specimen, in mm; h——The thickness of the specimen, in mm.
[0091]
[0092] Where, E is the tensile modulus of the specimen, in GPa; Δσ is the increment of the tensile strength of the specimen within the longitudinal strain range of 0.001 to 0.003, in MPa; Δε is the strain increment of the specimen within the longitudinal strain range of 0.001 to 0.003, in mm / mm.
[0093] 2. Dynamic mechanical properties test: The glass-like polymers prepared in Examples 1-8 and the comparative example were prepared in the form of rectangular strips of 60 mm*10 mm*2.5 mm, and the dynamic mechanical properties were tested using the multiple frequency-strain mode of the Q800 DMA instrument of TA Company of the United States. A double cantilever fixture was used, the test frequency was 1 Hz, the amplitude was 20 μm, and the sample was heated at a heating rate of 5°C / min. The temperature of different glass-like polymers was scanned through the test and the relationship between temperature, storage modulus and loss factor was obtained.
[0094] 3. Stress relaxation test: The glass-like polymers obtained in Examples 1-8 and the comparative examples were prepared in the form of rectangular splines of 60mm*10mm*2.5mm, and the stress relaxation behavior test was performed using the stress relaxation mode of the Q800 DMA instrument of TA Company of the United States. A double cantilever fixture was used, and no prestress was applied. The temperature was kept constant for 5 minutes at a predetermined temperature to ensure that all parts of the spline were at the same temperature. After that, a constant strain of 1% was applied to the spline, and the curve of the relaxation modulus of the spline changing with time was recorded. According to the relaxation time corresponding to 1 / e of the relaxation modulus of the spline at different temperatures, the activation energy of the topological network exchange reaction of the glass-like polymer can be obtained, thereby quantitatively comparing its network reorganization ability.
[0095]
[0096] Among them, τ is relaxation time, s; A is pre-exponential factor; Ea is activation energy of topological network exchange reaction, kJ / mol.
[0097] The above test results are shown in Table 1.
[0098] Table 1 Performance table of glass-like polymers obtained in various embodiments of the present invention
[0099]
[0100] As can be seen from the results in Table 1, in Examples 1-3 of the present invention, as the content of the reactive diluent decreases, the viscosity of the glass-like polymer system increases significantly, and the mechanical properties and heat resistance of the cured product are improved, but the increase in the content of the rigid structure is not conducive to the topological network exchange of the glass-like polymer, and the activation energy of the topological network exchange reaction continues to increase. In Examples 4-6 of the present invention, a single photocuring or photothermal dual curing method is used, which has excellent mechanical properties and similar reversible reaction activation energy compared to Example 1, indicating that glass-like polymers with excellent mechanical properties and thermal reversible properties can be prepared under the action of an external light source or thermal field. In Examples 7-8 of the present invention, a difunctional reactive diluent is used, and the obtained glass-like polymer has better mechanical properties and heat resistance, but the dense network structure causes its network exchange activation energy to increase. The modified epoxy raw material used in the comparative example does not contain hydroxyl groups, and its carbon-carbon double bond is inside the molecular chain, so the cross-linking degree of the cured sample is not high, and there is no hydrogen bonding to enhance the mechanical properties.
[0101] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a glass-like polymer capable of photothermal dual curing, characterized in that: include: (1) Mixing a modified resin, an ester exchange catalyst, a reactive diluent and an initiator, wherein the initiator comprises a thermal initiator and / or a photoinitiator, wherein the modified resin has the following structure: Among them, R1 is R2 is a hydrogen atom or a methyl group, and R3 is a hydrogen atom or a methyl group or a benzene ring; (2) Adding an external light source or an external heating field to the product obtained in step (1) to obtain a glass-like polymer.
2. The method according to claim 1, characterized in that The raw materials for preparing the modified resin include epoxy resin, unsaturated carboxylic acid and ester exchange catalyst. Optionally, the molar ratio of the epoxy resin, the unsaturated carboxylic acid and the transesterification catalyst is 1:(2-4):(0.02-0.2).
3. The method according to claim 2, characterized in that The epoxy resin, the unsaturated carboxylic acid and the transesterification catalyst are mixed, the stirring speed is controlled to be 200-500 r / min, the mixture is reacted at 120° C.-140° C. for at least 1 hour, and excess unsaturated carboxylic acid is removed to obtain the modified resin.
4. The method according to claim 2 or 3, characterized in that: The epoxy resin includes at least one of bisphenol A diglycidyl ether, bisphenol F diglycidyl ether, difunctional glycidyl ether and multifunctional glycidyl ether.
5. The method according to claim 2 or 3, characterized in that: The unsaturated carboxylic acid includes at least one of acrylic acid, methacrylic acid, crotonic acid, cinnamic acid, sorbic acid, maleic acid and trans-butenedioic acid.
6. The glass-like polymer according to any one of claims 1 to 3, characterized in that: The transesterification catalyst includes at least one of an amine catalyst, an amine having an amidine group and a derivative thereof.
7. The method according to any one of claims 1 to 3, characterized in that The reactive diluent includes at least one of a monofunctional acrylate derivative, a difunctional acrylate derivative, a multifunctional acrylate derivative and an acrylic acid-modified compound.
8. The method according to any one of claims 1 to 3, characterized in that The thermal initiator includes at least one of free radical initiators ester peroxide, acyl peroxide, ketone peroxide, and azo initiator; Optionally, the photoinitiator includes at least one of acylphosphorus oxides, benzophenones and benzil; Optionally, the modified resin, the transesterification catalyst, the active diluent, the initiator and other auxiliary agents are mixed, and the other auxiliary agents include at least one of a toughening agent, a defoaming agent, a leveling agent and an antioxidant.
9. The method according to any one of claims 1 to 3, characterized in that: The mass ratio of the modified resin, the transesterification catalyst, the active diluent and the initiator is (25-60): (2-5): (45-75): (0.5-2.5).
10. A glass-like polymer capable of photothermal dual curing, characterized in that: include: The method according to any one of claims 1 to 9 is used to prepare the present invention.
Citation Information
Patent Citations
Photothermal double-cured resin composition for pultrusion and glass fiber composite material prepared from photothermal double-cured resin composition
CN110437390A
4D printing photosensitive resin based on dynamic covalent bonds and preparation method thereof
CN112707984A
Composite, electrical machine, motor, transformer, structure, movable body and manufacturing method of composite
JP2017088739A