Thermal association gel as well as preparation method and application thereof

Thermal associative gel prepared by using alkenyl amide monomers, functional monomers and crosslinking agents at high temperatures is solved, and the problem of low structural strength and inconvenient use of polymer gels at high temperatures is achieved, thus achieving efficient slot holes The sealing effect of type reservoir is suitable for deep drilling and development of Tahe carbonate reservoir.

CN119060248APending Publication Date: 2024-12-03CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310648591.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-06-02
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing polymer gel leak plugging agent has low structural strength and limited temperature resistance under high temperature environments. It has many formula components and is not easy to mix evenly, which affects the on-site use effect and is difficult to meet the high temperature of the Tahe carbonate reservoir. Salt characteristics requirements.

Method used

Thermal associative gel is prepared by reacting alkenyl amide monomer, functional monomer and crosslinking agent under the action of initiators, including alkenyl hydrophobic monomer, alkenyl cyclic monomer and alkenyl sulfonic acid monomer, and optimized formula and preparation methods to improve structural strength and high temperature resistance.

Benefits of technology

The prepared thermally associative gel has high structural strength and high temperature resistance at 140°C. It can effectively block cracks of 1 to 3 mm wide, maintain a long-term sealing and pressure bearing capacity, and solve the problem of the existing technology. Issues of inconvenience in use and poor results.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060248A_ABST
    Figure CN119060248A_ABST
Patent Text Reader

Abstract

The invention provides thermal association gel as well as a preparation method and application thereof. The thermal association gel is obtained by reacting an alkenyl amide monomer, a functional monomer and a cross-linking agent under the action of an initiator, and has the advantages of high structural strength, good high-temperature resistance and good leaking stoppage performance. The thermal association gel has the advantages of fewer raw material types and simple preparation method, is a finished product before entering the stratum, and overcomes the problems of more gel components, inconvenience in use, difficulty in uniform mixing and influence on the plugging effect in the prior art. The plugging agent can be used as a plugging agent for continuously and effectively plugging fracture-cavity type oil reservoirs at the highest high temperature of 140 DEG C.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of oil reservoir plugging, and in particular relates to a thermally associated gel and a preparation method and application thereof. Background Art

[0002] The deep carbonate reservoirs in Tahe Oilfield are well developed with fractures and caves, and are highly heterogeneous, making it very easy for malignant leakage to occur during drilling. However, commonly used plugging agents such as bridging materials, cement, and high water loss consolidation have poor universality for Tahe fracture-cavity leakage and cannot meet the drilling plugging requirements of this type of reservoir. Compared with conventional plugging agents, gel plugging agents have the advantages of strong retention capacity and resistance to formation fluid dilution in fracture-cavity malignant leakage. The research and application of this type of technology is of great significance for effectively plugging malignant leakage in carbonate fracture-cavity reservoirs.

[0003] The gel plugging agents in the prior art have the following main deficiencies when facing high temperature environments:

[0004] (1) The main agent of the gel is mostly polyacrylamide polymer, which has limited structural strength and temperature resistance;

[0005] (2) High temperature will reduce the structural strength of the gel;

[0006] (3) The high temperature resistance time is too short, it cannot continue to function at high temperatures, and the high temperature stability is insufficient;

[0007] (4) The gel formula has many components, which is inconvenient to use and difficult to mix evenly, affecting the on-site use effect.

[0008] The Tahe carbonate reservoir has high temperature and high salt characteristics, specifically, the temperature is 120℃ to 140℃, and the mineralization is 210g / L to 240g / L. The high temperature and high salt characteristics of the Tahe carbonate reservoir, especially the high temperature characteristics, restrict the effective application of polyacrylamide polymer gel plugging agents in its plugging. Therefore, the study of efficient plugging materials suitable for the Tahe carbonate reservoir is of great significance for the efficient drilling and development of the Tahe deep carbonate reservoir, which is also a key issue to be solved in this field. Summary of the invention

[0009] In view of the problems in the prior art that polymer gel plugging agents have low structural strength and limited temperature resistance, and the gel formula has many components, which makes it inconvenient to use and difficult to mix evenly, affecting the on-site use effect, the purpose of the present invention is to provide a thermally associated gel for plugging with high associated structural strength and good stability at high temperature, as well as a preparation method and application thereof.

[0010] To achieve the above object, the first aspect of the present invention provides a thermally associative gel, the raw materials of which include vinyl amide monomers, functional monomers, crosslinking agents and initiators;

[0011] The functional monomers are selected from at least two of alkenyl hydrophobic monomers, alkenyl cyclic monomers and alkenyl sulfonic acid monomers.

[0012] According to a specific embodiment of the present invention, the amount of the vinyl amide monomer is 10 to 12 parts by mass, the amount of the functional monomer is 8 to 10 parts by mass, the amount of the cross-linking agent is 0.3 to 0.6 parts by mass, and the amount of the initiator is 0.03 to 0.05 parts by mass;

[0013] Preferably, the amount of the vinyl amide monomer is 10.1 to 11.7 parts by mass, the amount of the functional monomer is 8.3 to 9.9 parts by mass, the amount of the crosslinking agent is 0.35 to 0.55 parts by mass, and the amount of the initiator is 0.03 to 0.05 parts by mass.

[0014] According to a specific embodiment of the present invention, the vinyl amide monomer is selected from two of acrylamide, N,N-dimethylacrylamide, N,N-diethylacrylamide and N-isopropylacrylamide;

[0015] and / or

[0016] The alkenyl hydrophobic monomer is selected from one of dimethyldiallylhexadecylammonium chloride, N-hexadecylacrylamide and N-octadecylacrylamide; and / or

[0017] The alkenyl cyclic monomer is vinyl pyrrolidone; and / or

[0018] The alkenyl sulfonic acid monomer is selected from 2-acrylamide-2-methylpropane sulfonic acid and / or methylpropane sulfonic acid;

[0019] and / or

[0020] The cross-linking agent is at least one of hexamethylenetetramine, hydroquinone, phenolic acid, zirconium acetate and terephthalaldehyde; and / or

[0021] The initiator is at least one of potassium persulfate, ammonium persulfate and azobisisobutylamidine hydrochloride.

[0022] According to a specific embodiment of the present invention, the functional monomers include alkenyl hydrophobic monomers and alkenyl sulfonic acid monomers;

[0023] Preferably, taking the mass of the functional monomer as 100%, the functional monomer includes 30.8 wt % to 34 wt % of the olefinic hydrophobic monomer and 66 wt % to 69.2 wt % of the olefinic sulfonic acid monomer.

[0024] According to a specific embodiment of the present invention, the functional monomer includes the alkenyl hydrophobic monomer and the alkenyl cyclic monomer;

[0025] Preferably, taking the mass of the functional monomer as 100%, the functional monomer includes 42 wt % of the alkenyl hydrophobic monomer and 58 wt % of the alkenyl cyclic monomer.

[0026] The second aspect of the present invention provides a method for preparing the thermally associated gel according to the first aspect of the present invention, comprising the following steps:

[0027] 1) mixing the vinyl amide monomer, the functional monomer, the cross-linking agent and the first solvent to obtain a monomer-cross-linking agent solution;

[0028] 2) allowing the monomer-crosslinking agent solution to react under the action of the initiator, and drying to obtain the thermally associated gel.

[0029] According to a specific embodiment of the present invention, the first solvent is water.

[0030] According to a specific embodiment of the present invention, in step 1), the pH of the monomer-crosslinking agent solution is adjusted to neutral, and then the step 2) is performed; and / or

[0031] In step 2), the reaction solution obtained by the reaction is purified and then dried;

[0032] Preferably, the pH is adjusted with sodium hydroxide (e.g., 20 wt % sodium hydroxide aqueous solution);

[0033] Preferably, the purification is to precipitate the reaction solution with a second solvent, filter, collect the filter residue and perform the drying; and / or

[0034] The second solvent is ethanol and / or acetone.

[0035] According to a specific embodiment of the present invention, the reaction conditions are 60° C. to 65° C. for 6 h to 8 h; and / or

[0036] The drying temperature is 65°C to 75°C; and / or the drying time is 18h to 24h;

[0037] Preferably, the reaction is carried out under anaerobic conditions.

[0038] Use of the thermal associative gel according to the first aspect of the present invention or the thermal associative gel prepared by the method according to the second aspect of the present invention in plugging leaks in high-temperature fracture-vuggy reservoirs, especially as a plugging agent;

[0039] Preferably, the elevated temperature is up to 140°C.

[0040] Beneficial effects of the present invention:

[0041] In view of the problems of low structural strength and limited temperature resistance of polymer gel plugging agents in the prior art, the gel formula has many components, which makes it inconvenient to use and difficult to mix evenly, affecting the on-site use effect, the present invention provides a thermal association gel and its preparation method and application. The thermal association gel is obtained by reacting an olefinic amide monomer, a functional monomer and a cross-linking agent under the action of an initiator, and has the advantages of high structural strength, good high temperature resistance and good plugging performance:

[0042] (1) The thermally associated gel has a structural strength of about 3500 Pa to 3750 Pa at 140° C., and has a high structural strength at high temperatures;

[0043] (2) At 140° C. and 3.5 MPa, the thermally associated gel has a leakage of 64 to 82 mL when plugging a 1 mm wide crack for 0.5 h, a leakage of 56 to 84 mL when plugging a 2 mm wide crack for 0.5 h, and a leakage of 52 to 72 mL when plugging a 3 mm wide crack for 0.5 h. The leakage when plugging a 1 to 3 mm wide crack is relatively small, and the plugging effect is good;

[0044] (3) The thermally associated gel has a sealing strength of 8 MPa for cracks with a width of 1 to 3 mm at 140°C, and can maintain a sealing pressure bearing capacity of 8 MPa for at least 1 hour, achieving a long-term and effective sealing effect at high temperature.

[0045] The thermally associated gel has fewer raw material types, a simple preparation method, and is already a finished product before entering the formation. It overcomes the problems in the prior art of having more gel components, being inconvenient to use, and being difficult to mix evenly, which affects the plugging effect. It can be used as a plugging agent to effectively plug fracture-cavity oil reservoirs at high temperatures of up to 140°C. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] Figure 1 This is a graph showing the change in shear force versus shear time during the thermal association performance evaluation experiment for the thermal association gel prepared in Examples 1 to 3. DETAILED DESCRIPTION

[0047] The present invention will be further described below in conjunction with examples, but the examples of the present invention are only exemplary descriptions, and the implementation methods do not constitute limitations of the present invention under any circumstances.

[0048] Example 1

[0049] 1) Weigh 4.25 g of acrylamide, 5.88 g of N-isopropylacrylamide, 3.35 g of dimethyldiallylhexadecylammonium chloride, 6.52 g of 2-acrylamide-2-methylpropanesulfonic acid, 0.15 g of zirconium acetate and 0.2 g of hydroquinone, mix with 200 mL of deionized water, and stir evenly to obtain a monomer-crosslinking agent solution;

[0050] 2) The pH of the monomer-crosslinker solution was adjusted to neutral with a 20 wt % sodium hydroxide aqueous solution, 0.05 g of potassium persulfate was added, nitrogen was passed to drive out oxygen for 20 min, the water bath temperature was increased to 60° C., the reaction was carried out for 8 h, the reaction solution was precipitated with ethanol, filtered, the filter residue was collected, dried at 60° C. for 18 h, and crushed to obtain a thermally associated gel plugging agent.

[0051] Example 2

[0052] 1) Weigh 5.38 g of acrylamide, 6.35 g of N,N-diethylacrylamide, 2.55 g of N-octadecylacrylamide, 5.72 g of methylpropanesulfonic acid, 0.4 g of cyclohexamethylenetetramine and 0.15 g of phenolic formaldehyde, mix with 200 mL of deionized water, and stir evenly to obtain a monomer-crosslinking agent solution;

[0053] 2) The pH of the monomer-crosslinker solution was adjusted to neutral with a 20% sodium hydroxide aqueous solution, 0.03 g of azobisisobutylamidine hydrochloride was added, nitrogen was passed to drive out oxygen for 20 minutes, the water bath temperature was increased to 63°C, the reaction was carried out for 6 hours, the reaction solution was precipitated with acetone, filtered, the filter residue was collected, dried at 70°C for 20 hours, and crushed to obtain a thermally associated gel plugging agent.

[0054] Example 3

[0055] 1) Weigh 6.42 g of N,N-dimethylacrylamide, 5.15 g of N-isopropylacrylamide, 3.55 g of N-hexadecylacrylamide, 4.88 g of vinylpyrrolidone, 0.25 g of cyclohexamethylenetetramine and 0.3 g of terephthalaldehyde, mix with 200 mL of deionized water, and stir evenly to obtain a monomer-crosslinking agent solution;

[0056] 2) The pH of the monomer-crosslinker solution was adjusted to neutral with a 20% sodium hydroxide aqueous solution, 0.03 g of azobisisobutylamidine hydrochloride was added, nitrogen was passed to drive out oxygen for 20 minutes, the water bath temperature was increased to 65°C, the reaction was carried out for 8 hours, the reaction solution was precipitated with acetone, filtered, the filter residue was collected, dried at 75°C for 24 hours, and crushed to obtain a thermally associated gel plugging agent.

[0057] Evaluation of thermally associated gel properties

[0058] 1. Evaluation of thermal association

[0059] The structural strength of the hydrated thermally associative gels prepared in Examples 1 to 3 was measured to evaluate the thermally associative properties of the thermally associative gels. The specific steps are as follows:

[0060] ⅰ First, weigh 100 mL of water into a 250 mL beaker, then weigh 5 g of the thermally associated gel prepared in any one of Examples 1 to 3, add it to the beaker containing 100 mL of water, and place it at room temperature for hydration for 24 hours to obtain a hydrated thermally associated gel;

[0061] ⅱ Using HAAKE RS6000 high temperature and high pressure rheometer at 140℃ and normal pressure, the -1 The shear rate is used to measure the structural strength of the hydrated thermally associated gel obtained in step i;

[0062] According to the above method, the thermally associated gels prepared in Examples 1 to 3 were hydrated and then their structural strengths were measured.

[0063] For specific results, see Figure 1 .

[0064] Figure 1 It reflects the change of shear force with shear time during the experiment of the thermally associated gel prepared in Examples 1 to 3 after hydration. It can be seen that with the increase of shear time, the shear force rises rapidly to a peak value and then drops rapidly, and finally tends to be stable. The peak value to which the shear force rises in the process of increasing shear time is the structural strength of the thermally associated gel. It can be seen from the figure that the structural strength of the thermally associated gel prepared in Examples 1 to 3 is about 3500 to 3750Pa, which has a high structural strength, proving that the thermally associated gel prepared in Examples 1 to 3 has good thermal association performance, which helps it to be used as a plugging agent to achieve effective plugging under high temperature conditions.

[0065] 2. Evaluation of plugging performance

[0066] The thermally associative gels prepared in Examples 1 to 3 were used to seal cracks of different widths at high temperatures to evaluate the plugging performance of the thermally associative gels at high temperatures.

[0067] The specific steps are as follows:

[0068] Testing instrument: UDL-150-10 high temperature and high pressure leak plugging instrument;

[0069] Experimental temperature: 140℃;

[0070] A. Weigh 100 mL of water into a 250 mL beaker, then weigh 5 g of the thermally associated gel prepared in any one of Examples 1 to 3, add it to the beaker containing 100 mL of water, and hydrate at room temperature for 24 hours to obtain a hydrated thermally associated gel;

[0071] B. First, the leakage of the hydrated thermally associated gel prepared in step A when plugging cracks with widths of 1 mm, 2 mm, and 3 mm is measured and recorded when the pressure is 3.5 MPa and the experimental time is 0.5 h;

[0072] C. Then, the pressure is increased gradually from 3.5 MPa at a rate of 0.5 MPa per hour. After each increase of 0.5 MPa, the pressure is stabilized for 1 hour. If there is no sudden drop in the experimental pressure, the pressure bearing capacity of the thermally associated gel at 140°C when sealing cracks with widths of 1 mm, 2 mm, and 3 mm can be obtained;

[0073] According to steps A, B, and C, experiments were carried out using the thermally associated gels prepared in Examples 1 to 3, respectively.

[0074] The specific results are shown in Tables 1 and 2.

[0075] Table 1. Leakage of thermally associated gel at 140°C, 3.5 MPa, 0.5 h

[0076]

[0077] Table 2. Pressure bearing capacity of thermally associated gel for sealing cracks of different widths

[0078]

[0079] It can be seen from Table 1 that the thermally associated gels prepared in Examples 1 to 3 have a leakage of 64 to 82 mL for plugging 1 mm wide cracks, 56 to 84 mL for plugging 2 mm wide cracks, and 52 to 72 mL for plugging 3 mm wide cracks at 140°C, 3.5 MPa, and a plugging time of 0.5 h. It can be seen from the above data that the thermally associated gels prepared in Examples 1 to 3 have a small leakage when plugging 1 to 3 mm wide cracks at high temperature (140°C), indicating that the thermally associated gels prepared in Examples 1 to 3 have a good plugging effect on 1 to 3 mm wide cracks at 140°C and have good plugging performance.

[0080] From the data in Table 2, it can be seen that the thermally associated gels prepared in Examples 1 to 3 have a sealing strength of 8 MPa for 1 mm wide cracks, 2 mm wide cracks and 3 mm wide cracks at 140°C, and can maintain a sealing pressure bearing capacity of 8 MPa for at least 1 hour, indicating that the thermally associated gels prepared in Examples 1 to 3 can achieve continuous, effective and stable sealing of 1 to 3 mm wide cracks at a high temperature of 140°C, meeting the requirement of long-term high temperature resistance.

[0081] Based on the experimental results of the thermal association performance evaluation and plugging performance evaluation of the thermal association gel prepared in Examples 1 to 3, it can be seen that the thermal association gel prepared in Examples 1 to 3 has high structural strength and the ability to achieve continuous and stable high-strength plugging of 1 to 3 mm wide cracks under high temperature conditions of 140°C, and can be used in the plugging operations of the Tahe carbonate fracture-cavity high-temperature oil reservoir, which is of great significance for the efficient drilling and development of the Tahe deep carbonate oil reservoir.

[0082] Although the present invention has been described with reference to specific embodiments, it will be appreciated by those skilled in the art that various changes may be made without departing from the true spirit and scope of the present invention. In addition, the subject matter, spirit and scope of the present invention may be varied to accommodate specific situations, materials, material combinations and methods. All of these changes are included within the scope of the claims of the present invention.

Claims

1. A thermally associative gel, the raw materials of which include vinyl amide monomers, functional monomers, crosslinking agents and initiators; The functional monomers are selected from at least two of alkenyl hydrophobic monomers, alkenyl cyclic monomers and alkenyl sulfonic acid monomers.

2. The thermally associated gel according to claim 1, It is characterized in that The amount of the vinyl amide monomer is 10 to 12 parts by mass, the amount of the functional monomer is 8 to 10 parts by mass, the amount of the cross-linking agent is 0.3 to 0.6 parts by mass, and the amount of the initiator is 0.03 to 0.05 parts by mass.

3. The thermally associated gel according to claim 1 or 2, It is characterized in that The alkenyl amide monomer is selected from two of acrylamide, N,N-dimethylacrylamide, N,N-diethylacrylamide and N-isopropylacrylamide; and / or The alkenyl hydrophobic monomer is selected from one of dimethyldiallylhexadecylammonium chloride, N-hexadecylacrylamide and N-octadecylacrylamide; and / or The alkenyl cyclic monomer is vinyl pyrrolidone; and / or The alkenyl sulfonic acid monomer is selected from 2-acrylamide-2-methylpropane sulfonic acid and / or methylpropane sulfonic acid; and / or The cross-linking agent is at least one of hexamethylenetetramine, hydroquinone, phenolic acid, zirconium acetate and terephthalaldehyde; and / or The initiator is at least one of potassium persulfate, ammonium persulfate and azobisisobutylamidine hydrochloride.

4. The thermally associated gel according to any one of claims 1 to 3, It is characterized in that The functional monomers include alkenyl hydrophobic monomers and alkenyl sulfonic acid monomers; Preferably, taking the mass of the functional monomer as 100%, the functional monomer includes 30.8 wt % to 34 wt % of the olefinic hydrophobic monomer and 66 wt % to 69.2 wt % of the olefinic sulfonic acid monomer.

5. The thermally associated gel according to any one of claims 1 to 3, It is characterized in that The functional monomers include the alkenyl hydrophobic monomer and the alkenyl cyclic monomer; Preferably, taking the mass of the functional monomer as 100%, the functional monomer includes 42 wt % of the alkenyl hydrophobic monomer and 58 wt % of the alkenyl cyclic monomer.

6. A method for preparing the thermally associated gel according to any one of claims 1 to 5, comprising the steps of: 1) mixing the vinyl amide monomer, the functional monomer, the cross-linking agent and the first solvent to obtain a monomer-cross-linking agent solution; 2) allowing the monomer-crosslinking agent solution to react under the action of the initiator, and drying to obtain the thermally associated gel.

7. The method according to claim 6, It is characterized in that The first solvent is water.

8. The method according to claim 7, It is characterized in that In step 1), the pH of the monomer-crosslinking agent solution is adjusted to neutral, and then the step 2) is performed; and / or In step 2), the reaction solution obtained by the reaction is purified and then dried; Preferably, the pH is adjusted with sodium hydroxide; Preferably, the purification is to precipitate the reaction solution with a second solvent, filter, collect the filter residue and perform the drying; and / or The second solvent is ethanol and / or acetone.

9. The method according to any one of claims 6 to 8, It is characterized in that The reaction conditions are 60°C to 65°C for 6h to 8h; Preferably, the reaction is carried out under anaerobic conditions.

10. Use of the thermal associative gel according to any one of claims 1 to 5 or the thermal associative gel prepared by the method according to any one of claims 6 to 9 in plugging high-temperature fracture-cavity oil reservoirs, especially as a plugging agent; Preferably, the elevated temperature is up to 140°C.

Citation Information

Patent Citations

  • Controllable cross-linked gel plugging agent and preparation method thereof

    CN111117582A

  • Gel cement, associated polymer and preparation method

    CN111268953A

  • Method for preparing high-temperature cross-linking plugging agent for high-permeability oil reservoir recovery

    CN113754827A

  • Hydrophobic associated polymer and preparation method therefor

    WO2017113773A1