High-weather-resistance glass fiber reinforced plastic antenna housing and preparation method thereof
Through hydrochloric acid etching and modification of glass fibers, the mechanical and heat resistance of the radome is improved, and the problems of existing radomes are easily damaged and high temperature intolerance in open air environments are solved, and it is realized in outdoor and aviation applications. High performance and long life.
Patent Information
- Application Number
- CN202411163377.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-12-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing radomes are susceptible to natural factors in open air environments, resulting in reduced accuracy, easy damage and poor working reliability, and are intolerant to high temperature and aerodynamic loads, making it difficult to meet the long-term high heat resistance requirements such as outdoor and aviation.
Glass fibers that are etched and modified by hydrochloric acid are improved by chemical treatment such as ultrasonic cleaning, toluene dispersion, γ-methacryloyloxypropyltrimethoxysilane and diphenylmethane diisocyanate. Binding force and dispersion form a polymer network structure, improving the mechanical properties and heat resistance of the material.
The prepared fiberglass radome has good mechanical properties and heat resistance, and is suitable for applications in long-term outdoor high-temperature environments and high heat resistance requirements, extending service life and improving reliability.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of antenna cover materials, and in particular to a high-weather-resistant fiberglass antenna cover and a preparation method thereof. Background Art
[0002] With the large-scale application of 5G networks, a large number of related supporting facilities need to be built, such as network antennas. Antennas are usually placed in open-air environments. Due to the different environments in different regions and the large temperature difference between day and night, antennas may be directly attacked by natural storms, snow, sand and solar radiation during service, resulting in reduced antenna accuracy, easy damage and poor working reliability. Antenna covers are often required for protection. The purposes of using antenna covers usually include: 1. Protecting the antenna system from the influence of wind, rain, snow, sand and solar radiation, so that the working performance of the antenna system is relatively stable and reliable, while reducing the wear, corrosion and aging of the antenna system and extending its service life; 2. For high-speed aircraft, antenna covers can solve the problems caused by high temperature, aerodynamic load and other loads to the antenna.
[0003] FRP composite materials have excellent performance and are used in many fields. In particular, FRP has excellent prospects in the field of outdoor or marine equipment due to its light weight and high strength. The use of FRP materials for antenna covers is becoming more and more common. However, antenna covers are often used in complex atmospheric environments, which puts higher requirements on the weather resistance and corrosion resistance of FRP composite materials. Summary of the invention
[0004] To this end, the present invention provides a method for preparing a high-weather-resistant fiberglass antenna cover, the preparation steps comprising:
[0005] (1) preparing a hydrochloric acid solution; in an ultrasonic environment, soaking the glass fiber in acetone for more than 10 minutes to clean and degrease, then performing solid-liquid separation, drying at 60° C. for more than 20 minutes to obtain the cleaned glass fiber, soaking the cleaned glass fiber in anhydrous ethanol for more than 10 hours, then performing solid-liquid separation, washing the solid phase with deionized water for more than 2 times, then soaking it in the hydrochloric acid solution, heating it in a water bath to 80±5° C. and etching it for more than 6 hours, then performing solid-liquid separation, washing the solid phase with deionized water until the washed liquid is neutral, and obtaining the etched glass fiber;
[0006] (2) adding the etched glass fiber to toluene, stirring and dispersing with ultrasonic wave for more than 20 minutes to obtain a dispersion, placing the dispersion in a nitrogen protection environment, and then adding triethylamine, γ-methacryloxypropyltrimethoxysilane and diphenylmethane diisocyanate to the dispersion under stirring, and continuing to stir in a nitrogen atmosphere for more than 20 hours after the addition is completed. After the stirring is completed, the solid-liquid separation is carried out, the solid phase is washed with toluene for more than 2 times, and then washed with ethanol for more than 2 times, and dried at 60° C. for more than 5 hours to obtain a treated glass fiber;
[0007] (3) preparing a 3,5-diaminobenzoic acid N-methylpyrrolidone solution; adding the once treated glass fiber to the 3,5-diaminobenzoic acid N-methylpyrrolidone solution, and then heating the glass fiber in a water bath to 85±5° C. and keeping the temperature for more than 6 hours, condensing and refluxing during the insulation process, separating the solid and the liquid after the insulation is completed, washing the solid phase with deionized water for more than 3 times, and drying at 80° C. for more than 5 hours to obtain a modified glass fiber;
[0008] (4) Weigh the raw materials respectively: unsaturated polyester resin, the modified glass fiber, foaming agent, 3-isopropyl-dimethylbenzyl isocyanate, styrene, tert-butyl perbenzoate and a release agent, first place the foaming agent in a mold, and preheat the mold at 100° C. for 30 to 40 minutes, then mix the unsaturated polyester resin, modified glass fiber, 3-isopropyl-dimethylbenzyl isocyanate, styrene and the release agent to form a resin glue, pour the resin glue into the preheated mold, stir for 2 to 3 minutes to mix, then heat to 116±2° C. and keep warm, then add the tert-butyl perbenzoate, keep warm at 116±2° C. and stir for 20 to 30 seconds, then let it stand and cure, naturally cool to room temperature after curing, and demold to obtain the fiberglass antenna cover.
[0009] Furthermore, in the step (1), the concentration of the solute in the hydrochloric acid solution is 0.5 mol / L, the mass ratio of the glass fiber immersed in the anhydrous ethanol is glass fiber: anhydrous ethanol = 1:100; the mass ratio of the solid phase after washing with deionized water immersed in the hydrochloric acid solution is solid phase: hydrochloric acid solution = 1:100.
[0010] Furthermore, in the step (2), the mass ratio of the etched glass fiber to toluene is:
[0011] Toluene = 1:20, the mass ratio of added triethylamine, γ-methacryloxypropyl trimethoxysilane and diphenylmethane diisocyanate to the mass ratio of etched glass fiber in the dispersion is triethylamine:γ-methacryloxypropyl trimethoxysilane:diphenylmethane diisocyanate:etched glass fiber = 0.7-0.8:0.3-0.5:6-8:10.
[0012] Furthermore, in the step (3), in the N-methylpyrrolidone solution of 3,5-diaminobenzoic acid, the mass percentage of 3,5-diaminobenzoic acid is 3% to 4%, the solvent is N-methylpyrrolidone, and the mass ratio of the once-treated glass fiber added to the N-methylpyrrolidone solution of 3,5-diaminobenzoic acid is once-treated glass fiber: 3,5-diaminobenzoic acid N-methylpyrrolidone solution = 1:80.
[0013] Furthermore, in the step (4), the raw materials are calculated by weight as follows: 50 parts of unsaturated polyester resin; 4-5 parts of modified glass fiber; 0.8-1 part of foaming agent; 1-2 parts of 3-isopropyl-dimethylbenzyl isocyanate; 0.9-1 part of styrene; 0.5-0.6 parts of tert-butyl perbenzoate; and 1.6-1.8 parts of release agent.
[0014] Furthermore, the foaming agent is 4,4'-oxybisbenzenesulfonyl hydrazide, and the release agent is zinc stearate.
[0015] The beneficial effects of the present invention are that the glass fiber reinforced plastic antenna cover material prepared by the method of the present invention has good mechanical properties and heat resistance, is not easy to deform and crack during use, and has high thermal stability, is suitable for long-term outdoor high temperature service, and is also suitable for use in aviation, mining and other occasions with high requirements for antenna heat resistance. The present invention first uses hydrochloric acid to etch the glass fiber, on the one hand, to increase the specific surface area of the glass fiber, and on the other hand, to hydroxylate the surface of the glass fiber to form a large number of hydroxyl groups, in preparation for subsequent modification. Then, the glass fiber is treated with triethylamine, γ-methacryloxypropyltrimethoxysilane and diphenylmethane diisocyanate to isocyanate the glass fiber, change the physical and chemical morphology and active functional group type of the surface of the glass fiber, and improve the chemical bonding between the glass fiber and the resin, thereby improving the compatibility of the glass fiber and the resin matrix, and improving the interface bonding strength between the glass fiber and the matrix; at the same time, γ-methacryloxypropyltrimethoxysilane can graft silane groups on the surface of the glass fiber, and then bond with the silane groups through 3,5-diaminobenzoic acid, so that the dispersion of the glass fiber is improved and the agglomeration is reduced. Finally, by adding 3-isopropyl-dimethylbenzyl isocyanate and styrene, a polymer network structure is formed, thereby improving the heat resistance stability of the material. DETAILED DESCRIPTION
[0016] The present invention will be further described below in conjunction with the embodiments.
[0017] Example 1
[0018] A method for preparing a highly weather-resistant fiberglass antenna cover, the preparation steps comprising:
[0019] (1) preparing a hydrochloric acid solution, wherein the concentration of the solute in the hydrochloric acid solution is 0.5 mol / L; in an ultrasonic environment, soaking a glass fiber (chopped glass fiber SGF, Chongqing International Composites ECS407-3-K, diameter 13 μm, length 3 mm) in acetone for 10 min to clean and degrease, then performing solid-liquid separation, drying at 60° C. for 20 min, obtaining the cleaned glass fiber, and soaking the cleaned glass fiber in anhydrous ethanol for 10 h, wherein the mass ratio of the glass fiber soaked in anhydrous ethanol is glass fiber: anhydrous ethanol = 1:100; then performing solid-liquid separation, washing the solid phase with deionized water twice, and then soaking it in the hydrochloric acid solution, wherein the mass ratio of the solid phase after the deionized water washing with the hydrochloric acid solution is solid phase: hydrochloric acid solution = 1:100; heating the water bath to 80±5° C. for 6 h of heat preservation, then performing solid-liquid separation, and washing the solid phase with deionized water until the washed liquid is neutral, thereby obtaining the etched glass fiber;
[0020] (2) adding the etched glass fiber to toluene, wherein the mass ratio of the etched glass fiber to toluene is etched glass fiber: toluene = 1:20, and ultrasonic stirring and dispersing for 20 minutes to obtain a dispersion, placing the dispersion in a nitrogen protection environment, and then adding triethylamine, γ-methacryloxypropyl trimethoxysilane and diphenylmethane diisocyanate to the dispersion under stirring, wherein the mass ratio of the added triethylamine, γ-methacryloxypropyl trimethoxysilane and diphenylmethane diisocyanate to the mass ratio of the etched glass fiber in the dispersion is triethylamine: γ-methacryloxypropyl trimethoxysilane: diphenylmethane diisocyanate: etched glass fiber = 0.7:0.3:6:10; after the addition is completed, stirring is continued in a nitrogen atmosphere for 20 hours, after the stirring is completed, solid-liquid separation is performed, the solid phase is washed twice with toluene, and then washed twice with ethanol, and dried at 60° C. for 5 hours to obtain a once-treated glass fiber;
[0021] (3) preparing a 3,5-diaminobenzoic acid N-methylpyrrolidone solution, wherein the mass percentage of 3,5-diaminobenzoic acid in the 3,5-diaminobenzoic acid N-methylpyrrolidone solution is 3%, and the solvent is N-methylpyrrolidone; adding the once treated glass fiber to the 3,5-diaminobenzoic acid N-methylpyrrolidone solution, wherein the mass ratio of the once treated glass fiber to the 3,5-diaminobenzoic acid N-methylpyrrolidone solution is once treated glass fiber: 3,5-diaminobenzoic acid N-methylpyrrolidone solution = 1:80; then heating in a water bath to 85±5° C. for 6 hours, condensing and refluxing during the insulation process, and separating the solid and liquid after the insulation is completed, washing the solid phase with deionized water 3 times, and drying at 80° C. for 5 hours to obtain modified glass fiber;
[0022] (4) Weigh the following raw materials: unsaturated polyester resin (type 191A, the same in all examples and comparative examples), the modified glass fiber, blowing agent, 3-isopropyl-dimethylbenzyl isocyanate, styrene, tert-butyl perbenzoate and a release agent. The raw materials are calculated by weight as follows: 50 parts of unsaturated polyester resin; 4 parts of modified glass fiber; 0.8 parts of blowing agent; 1 part of 3-isopropyl-dimethylbenzyl isocyanate; 0.9 parts of styrene; 0.5 parts of tert-butyl perbenzoate; and 1.6 parts of a release agent. The blowing agent is 4,4'-oxybisbenzenesulfonyl hydrazide. The release agent is zinc stearate; the foaming agent is first placed in a mold, the mold is preheated at 100°C for 30 minutes, and then the unsaturated polyester resin, modified glass fiber, 3-isopropyl-dimethylbenzyl isocyanate, styrene and the release agent are evenly mixed to form a resin glue, the resin glue is poured into the preheated mold, stirred for 2 minutes to mix, and then heated to 116±2°C for insulation, and then the tert-butyl perbenzoate is added, and the mixture is stirred at 116±2°C for 20 seconds, and then allowed to stand and solidify, and naturally cooled to room temperature after solidification, and demolded to obtain the fiberglass antenna cover.
[0023] Example 2
[0024] A method for preparing a highly weather-resistant fiberglass antenna cover, the preparation steps comprising:
[0025] (1) preparing a hydrochloric acid solution, wherein the concentration of the solute in the hydrochloric acid solution is 0.5 mol / L; in an ultrasonic environment, soaking a glass fiber (chopped glass fiber SGF, Chongqing International Composites ECS407-3-K, diameter 13 μm, length 3 mm) in acetone for 10 min to clean and degrease, then performing solid-liquid separation, drying at 60° C. for 20 min, obtaining the cleaned glass fiber, and soaking the cleaned glass fiber in anhydrous ethanol for 10 h, wherein the mass ratio of the glass fiber soaked in anhydrous ethanol is glass fiber: anhydrous ethanol = 1:100; then performing solid-liquid separation, washing the solid phase with deionized water twice, and then soaking it in the hydrochloric acid solution, wherein the mass ratio of the solid phase after the deionized water washing with the hydrochloric acid solution is solid phase: hydrochloric acid solution = 1:100; heating the water bath to 80±5° C. for 6 h of heat preservation, then performing solid-liquid separation, and washing the solid phase with deionized water until the washed liquid is neutral, thereby obtaining the etched glass fiber;
[0026] (2) adding the etched glass fiber to toluene, wherein the mass ratio of the etched glass fiber to toluene is etched glass fiber: toluene = 1:20, and ultrasonic stirring and dispersing for 20 minutes to obtain a dispersion, placing the dispersion in a nitrogen protection environment, and then adding triethylamine, γ-methacryloxypropyl trimethoxysilane and diphenylmethane diisocyanate to the dispersion under stirring, wherein the mass ratio of the added triethylamine, γ-methacryloxypropyl trimethoxysilane and diphenylmethane diisocyanate to the mass ratio of the etched glass fiber in the dispersion is triethylamine: γ-methacryloxypropyl trimethoxysilane: diphenylmethane diisocyanate: etched glass fiber = 0.7:0.4:7:10; after the addition is completed, stirring is continued in a nitrogen atmosphere for 20 hours, after the stirring is completed, solid-liquid separation is performed, the solid phase is washed twice with toluene, and then washed twice with ethanol, and dried at 60° C. for 5 hours to obtain a once-treated glass fiber;
[0027] (3) preparing a 3,5-diaminobenzoic acid N-methylpyrrolidone solution, wherein the mass percentage of 3,5-diaminobenzoic acid in the 3,5-diaminobenzoic acid N-methylpyrrolidone solution is 3%, and the solvent is N-methylpyrrolidone; adding the once treated glass fiber to the 3,5-diaminobenzoic acid N-methylpyrrolidone solution, wherein the mass ratio of the once treated glass fiber to the 3,5-diaminobenzoic acid N-methylpyrrolidone solution is once treated glass fiber: 3,5-diaminobenzoic acid N-methylpyrrolidone solution = 1:80; then heating in a water bath to 85±5° C. for 6 hours, condensing and refluxing during the insulation process, and separating the solid and liquid after the insulation is completed, washing the solid phase with deionized water 3 times, and drying at 80° C. for 5 hours to obtain modified glass fiber;
[0028] (4) Weigh the raw materials: unsaturated polyester resin, the modified glass fiber, blowing agent, 3-isopropyl-dimethylbenzyl isocyanate, styrene, tert-butyl perbenzoate and release agent respectively, wherein the raw materials are calculated in parts by weight as follows: 50 parts of unsaturated polyester resin; 4 parts of modified glass fiber; 0.9 parts of blowing agent; 1 part of 3-isopropyl-dimethylbenzyl isocyanate; 0.9 parts of styrene; 0.5 parts of tert-butyl perbenzoate; and 1.7 parts of release agent; wherein the blowing agent is 4,4'-oxybisbenzenesulfonyl hydrazide, and the release agent is zinc stearate; First, the foaming agent is placed in a mold, and the mold is preheated at 100° C. for 30 minutes. Then, the unsaturated polyester resin, modified glass fiber, 3-isopropyl-dimethylbenzyl isocyanate, styrene and a release agent are mixed evenly to form a resin glue solution. The resin glue solution is poured into the preheated mold, stirred for 2 minutes to mix evenly, and then heated to 116±2° C. for insulation. Then, tert-butyl perbenzoate is added, and the mixture is stirred at 116±2° C. for 20 seconds. Then, the mixture is allowed to stand and solidify. After solidification, the mixture is naturally cooled to room temperature, and the mold is demolded to obtain the fiberglass antenna cover.
[0029] Example 3
[0030] A method for preparing a highly weather-resistant fiberglass antenna cover, the preparation steps comprising:
[0031] (1) preparing a hydrochloric acid solution, wherein the concentration of the solute in the hydrochloric acid solution is 0.5 mol / L; in an ultrasonic environment, soaking a glass fiber (chopped glass fiber SGF, Chongqing International Composites ECS407-3-K, diameter 13 μm, length 3 mm) in acetone for 10 min to clean and degrease, then performing solid-liquid separation, drying at 60° C. for 20 min, obtaining the cleaned glass fiber, and soaking the cleaned glass fiber in anhydrous ethanol for 10 h, wherein the mass ratio of the glass fiber soaked in anhydrous ethanol is glass fiber: anhydrous ethanol = 1:100; then performing solid-liquid separation, washing the solid phase with deionized water twice, and then soaking it in the hydrochloric acid solution, wherein the mass ratio of the solid phase after the deionized water washing with the hydrochloric acid solution is solid phase: hydrochloric acid solution = 1:100; heating the water bath to 80±5° C. for 6 h of heat preservation, then performing solid-liquid separation, and washing the solid phase with deionized water until the washed liquid is neutral, thereby obtaining the etched glass fiber;
[0032] (2) adding the etched glass fiber to toluene, wherein the mass ratio of the etched glass fiber to toluene is etched glass fiber: toluene = 1:20, and ultrasonic stirring and dispersing for 20 minutes to obtain a dispersion, placing the dispersion in a nitrogen protection environment, and then adding triethylamine, γ-methacryloxypropyl trimethoxysilane and diphenylmethane diisocyanate to the dispersion under stirring, wherein the mass ratio of the added triethylamine, γ-methacryloxypropyl trimethoxysilane and diphenylmethane diisocyanate to the mass ratio of the etched glass fiber in the dispersion is triethylamine: γ-methacryloxypropyl trimethoxysilane: diphenylmethane diisocyanate: etched glass fiber = 0.8:0.4:7:10; after the addition is completed, stirring is continued in a nitrogen atmosphere for 20 hours, and after the stirring is completed, solid-liquid separation is performed, the solid phase is washed twice with toluene, and then washed twice with ethanol, and dried at 60° C. for 5 hours to obtain a once-treated glass fiber;
[0033] (3) preparing a 3,5-diaminobenzoic acid N-methylpyrrolidone solution, wherein the mass percentage of 3,5-diaminobenzoic acid in the 3,5-diaminobenzoic acid N-methylpyrrolidone solution is 4%, and the solvent is N-methylpyrrolidone; adding the once treated glass fiber to the 3,5-diaminobenzoic acid N-methylpyrrolidone solution, wherein the mass ratio of the once treated glass fiber to the 3,5-diaminobenzoic acid N-methylpyrrolidone solution is once treated glass fiber: 3,5-diaminobenzoic acid N-methylpyrrolidone solution = 1:80; then heating in a water bath to 85±5° C. for 6 hours, condensing and refluxing during the insulation process, separating the solid and the liquid after the insulation is completed, washing the solid phase with deionized water 3 times, and drying at 80° C. for 5 hours to obtain a modified glass fiber;
[0034] (4) Weigh the raw materials: unsaturated polyester resin, the modified glass fiber, blowing agent, 3-isopropyl-dimethylbenzyl isocyanate, styrene, tert-butyl perbenzoate and release agent respectively, wherein the raw materials are calculated in parts by weight as follows: 50 parts of unsaturated polyester resin; 5 parts of modified glass fiber; 0.9 parts of blowing agent; 2 parts of 3-isopropyl-dimethylbenzyl isocyanate; 1 part of styrene; 0.6 parts of tert-butyl perbenzoate; and 1.7 parts of release agent; wherein the blowing agent is 4,4'-oxybisbenzenesulfonyl hydrazide and the release agent is zinc stearate; first The foaming agent is placed in a mold, and the mold is preheated at 100°C for 30 minutes. Unsaturated polyester resin, modified glass fiber, 3-isopropyl-dimethylbenzyl isocyanate, styrene and a release agent are then mixed evenly to form a resin glue solution. The resin glue solution is poured into the preheated mold, stirred for 2 minutes to mix evenly, and then heated to 116±2°C for insulation. Tert-butyl perbenzoate is then added, and the mixture is stirred at 116±2°C for 20 seconds. The mixture is then allowed to stand and solidify. After solidification, the mixture is naturally cooled to room temperature, and the mold is demolded to obtain the fiberglass antenna cover.
[0035] Example 4
[0036] A method for preparing a highly weather-resistant fiberglass antenna cover, the preparation steps comprising:
[0037] (1) preparing a hydrochloric acid solution, wherein the concentration of the solute in the hydrochloric acid solution is 0.5 mol / L; in an ultrasonic environment, soaking a glass fiber (chopped glass fiber SGF, Chongqing International Composites ECS407-3-K, diameter 13 μm, length 3 mm) in acetone for 10 min to clean and degrease, then performing solid-liquid separation, drying at 60° C. for 20 min, obtaining the cleaned glass fiber, and soaking the cleaned glass fiber in anhydrous ethanol for 10 h, wherein the mass ratio of the glass fiber soaked in anhydrous ethanol is glass fiber: anhydrous ethanol = 1:100; then performing solid-liquid separation, washing the solid phase with deionized water twice, and then soaking it in the hydrochloric acid solution, wherein the mass ratio of the solid phase after the deionized water washing with the hydrochloric acid solution is solid phase: hydrochloric acid solution = 1:100; heating the water bath to 80±5° C. for 6 h of heat preservation, then performing solid-liquid separation, and washing the solid phase with deionized water until the washed liquid is neutral, thereby obtaining the etched glass fiber;
[0038] (2) adding the etched glass fiber to toluene, wherein the mass ratio of the etched glass fiber to toluene is etched glass fiber: toluene = 1:20, and ultrasonic stirring and dispersing for 20 minutes to obtain a dispersion, placing the dispersion in a nitrogen protection environment, and then adding triethylamine, γ-methacryloxypropyl trimethoxysilane and diphenylmethane diisocyanate to the dispersion under stirring, wherein the mass ratio of the added triethylamine, γ-methacryloxypropyl trimethoxysilane and diphenylmethane diisocyanate to the mass ratio of the etched glass fiber in the dispersion is triethylamine: γ-methacryloxypropyl trimethoxysilane: diphenylmethane diisocyanate: etched glass fiber = 0.8:0.5:8:10; after the addition is completed, stirring is continued in a nitrogen atmosphere for 20 hours, after the stirring is completed, solid-liquid separation is performed, the solid phase is washed twice with toluene, and then washed twice with ethanol, and dried at 60° C. for 5 hours to obtain a treated glass fiber;
[0039] (3) preparing a 3,5-diaminobenzoic acid N-methylpyrrolidone solution, wherein the mass percentage of 3,5-diaminobenzoic acid in the 3,5-diaminobenzoic acid N-methylpyrrolidone solution is 4%, and the solvent is N-methylpyrrolidone; adding the once treated glass fiber to the 3,5-diaminobenzoic acid N-methylpyrrolidone solution, wherein the mass ratio of the once treated glass fiber to the 3,5-diaminobenzoic acid N-methylpyrrolidone solution is once treated glass fiber: 3,5-diaminobenzoic acid N-methylpyrrolidone solution = 1:80; then heating in a water bath to 85±5° C. for 6 hours, condensing and refluxing during the insulation process, separating the solid and the liquid after the insulation is completed, washing the solid phase with deionized water 3 times, and drying at 80° C. for 5 hours to obtain a modified glass fiber;
[0040] (4) Weigh the raw materials: unsaturated polyester resin, the modified glass fiber, blowing agent, 3-isopropyl-dimethylbenzyl isocyanate, styrene, tert-butyl perbenzoate and release agent respectively, wherein the raw materials are calculated in parts by weight as follows: 50 parts of unsaturated polyester resin; 5 parts of modified glass fiber; 1 part of blowing agent; 2 parts of 3-isopropyl-dimethylbenzyl isocyanate; 1 part of styrene; 0.6 parts of tert-butyl perbenzoate; and 1.8 parts of release agent; wherein the blowing agent is 4,4'-oxybisbenzenesulfonyl hydrazide and the release agent is zinc stearate; first The foaming agent is placed in a mold, and the mold is preheated at 100° C. for 30 minutes. Then, unsaturated polyester resin, modified glass fiber, 3-isopropyl-dimethylbenzyl isocyanate, styrene and a release agent are mixed evenly to form a resin glue. The resin glue is poured into the preheated mold, stirred for 2 minutes to mix evenly, and then heated to 116±2° C. for insulation. Then, tert-butyl perbenzoate is added, and the mixture is stirred at 116±2° C. for 20 seconds. Then, the mixture is allowed to stand and solidify. After solidification, the mixture is naturally cooled to room temperature, and the mold is demolded to obtain the fiberglass antenna cover.
[0041] Comparative Example 1
[0042] A method for preparing a fiberglass antenna cover for comparison, the preparation steps comprising:
[0043] (1) preparing a hydrochloric acid solution, wherein the concentration of the solute in the hydrochloric acid solution is 0.5 mol / L; in an ultrasonic environment, soaking a glass fiber (chopped glass fiber SGF, Chongqing International Composites ECS407-3-K, diameter 13 μm, length 3 mm) in acetone for 10 min to clean and degrease, then performing solid-liquid separation, drying at 60° C. for 20 min, obtaining the cleaned glass fiber, and soaking the cleaned glass fiber in anhydrous ethanol for 10 h, wherein the mass ratio of the glass fiber soaked in anhydrous ethanol is glass fiber: anhydrous ethanol = 1:100; then performing solid-liquid separation, washing the solid phase with deionized water twice, and then soaking it in the hydrochloric acid solution, wherein the mass ratio of the solid phase after the deionized water washing with the hydrochloric acid solution is solid phase: hydrochloric acid solution = 1:100; heating the water bath to 80±5° C. for 6 h of heat preservation, then performing solid-liquid separation, and washing the solid phase with deionized water until the washed liquid is neutral, thereby obtaining the etched glass fiber;
[0044] (2) adding the etched glass fiber to toluene, the mass ratio of the etched glass fiber to toluene is etched glass fiber: toluene = 1:20, ultrasonic stirring and dispersing for 20 minutes to obtain a dispersion, placing the dispersion in a nitrogen protection environment, and then adding triethylamine and γ-methacryloxypropyltrimethoxysilane to the dispersion under stirring, the mass ratio of the added triethylamine and γ-methacryloxypropyltrimethoxysilane to the etched glass fiber in the dispersion is triethylamine: γ-methacryloxypropyltrimethoxysilane: etched glass fiber = 0.8:0.4:10; continuing to stir in a nitrogen atmosphere for 20 hours after the addition is completed, after the stirring is completed, the solid-liquid separation is carried out, the solid phase is washed twice with toluene, and then washed twice with ethanol, and dried at 60°C for 5 hours to obtain a once-treated glass fiber of this comparative example;
[0045] (3) preparing a 3,5-diaminobenzoic acid N-methylpyrrolidone solution, wherein the mass percentage of 3,5-diaminobenzoic acid in the 3,5-diaminobenzoic acid N-methylpyrrolidone solution is 4%, and the solvent is N-methylpyrrolidone; adding the once treated glass fiber to the 3,5-diaminobenzoic acid N-methylpyrrolidone solution, wherein the mass ratio of the once treated glass fiber to the 3,5-diaminobenzoic acid N-methylpyrrolidone solution is once treated glass fiber: 3,5-diaminobenzoic acid N-methylpyrrolidone solution = 1:80; then heating in a water bath to 85±5° C. for 6 hours, condensing and refluxing during the insulation process, separating the solid and the liquid after the insulation is completed, washing the solid phase with deionized water 3 times, and drying at 80° C. for 5 hours to obtain a modified glass fiber;
[0046] (4) Weigh the raw materials: unsaturated polyester resin, the modified glass fiber, blowing agent, 3-isopropyl-dimethylbenzyl isocyanate, styrene, tert-butyl perbenzoate and release agent respectively, and the raw materials are calculated by weight as follows: 50 parts of unsaturated polyester resin; 5 parts of modified glass fiber; 0.9 parts of blowing agent; 2 parts of 3-isopropyl-dimethylbenzyl isocyanate; 1 part of styrene; 0.6 parts of tert-butyl perbenzoate; 1.7 parts of release agent; wherein the blowing agent is 4,4'-oxybisbenzenesulfonyl hydrazide, and the release agent is zinc stearate; first, The foaming agent is placed in a mold, and the mold is preheated at 100°C for 30 minutes. Then, the unsaturated polyester resin, modified glass fiber, 3-isopropyl-dimethylbenzyl isocyanate, styrene and a release agent are mixed evenly to form a resin glue. The resin glue is poured into the preheated mold, stirred for 2 minutes to mix, and then heated to 116±2°C for insulation. Then, tert-butyl perbenzoate is added, and the mixture is stirred at 116±2°C for 20 seconds. Then, the mixture is allowed to stand and solidify. After solidification, it is naturally cooled to room temperature and demolded to obtain the fiberglass antenna cover described in this comparative example.
[0047] Comparative Example 2
[0048] A method for preparing a fiberglass antenna cover for comparison, the preparation steps comprising:
[0049] (1) preparing a hydrochloric acid solution, wherein the concentration of the solute in the hydrochloric acid solution is 0.5 mol / L; in an ultrasonic environment, soaking a glass fiber (chopped glass fiber SGF, Chongqing International Composites ECS407-3-K, diameter 13 μm, length 3 mm) in acetone for 10 min to clean and degrease, then performing solid-liquid separation, drying at 60° C. for 20 min, obtaining the cleaned glass fiber, and soaking the cleaned glass fiber in anhydrous ethanol for 10 h, wherein the mass ratio of the glass fiber soaked in anhydrous ethanol is glass fiber: anhydrous ethanol = 1:100; then performing solid-liquid separation, washing the solid phase with deionized water twice, and then soaking it in the hydrochloric acid solution, wherein the mass ratio of the solid phase after the deionized water washing with the hydrochloric acid solution is solid phase: hydrochloric acid solution = 1:100; heating the water bath to 80±5° C. for 6 h of heat preservation, then performing solid-liquid separation, and washing the solid phase with deionized water until the washed liquid is neutral, thereby obtaining the etched glass fiber;
[0050] (2) adding the etched glass fiber to toluene, wherein the mass ratio of the etched glass fiber to toluene is etched glass fiber: toluene = 1:20, and ultrasonic stirring and dispersing for 20 minutes to obtain a dispersion, placing the dispersion in a nitrogen protection environment, and then adding triethylamine, γ-methacryloxypropyl trimethoxysilane and diphenylmethane diisocyanate to the dispersion under stirring, wherein the mass ratio of the added triethylamine, γ-methacryloxypropyl trimethoxysilane and diphenylmethane diisocyanate to the mass ratio of the etched glass fiber in the dispersion is triethylamine: γ-methacryloxypropyl trimethoxysilane: diphenylmethane diisocyanate: etched glass fiber = 0.8:0.4:7:10; after the addition is completed, stirring is continued in a nitrogen atmosphere for 20 hours, and after the stirring is completed, solid-liquid separation is performed, the solid phase is washed twice with toluene, and then washed twice with ethanol, and dried at 60° C. for 5 hours to obtain the modified glass fiber of this comparative example;
[0051] (3) Weigh the raw materials: unsaturated polyester resin, the modified glass fiber, blowing agent, 3-isopropyl-dimethylbenzyl isocyanate, styrene, tert-butyl perbenzoate and release agent respectively, and the raw materials are calculated in parts by weight: 50 parts of unsaturated polyester resin; 5 parts of modified glass fiber; 0.9 parts of blowing agent; 2 parts of 3-isopropyl-dimethylbenzyl isocyanate; 1 part of styrene; 0.6 parts of tert-butyl perbenzoate; 1.7 parts of release agent; wherein the blowing agent is 4,4'-oxybisbenzenesulfonyl hydrazide, and the release agent is zinc stearate; first, The foaming agent is placed in a mold, and the mold is preheated at 100°C for 30 minutes. Then, the unsaturated polyester resin, modified glass fiber, 3-isopropyl-dimethylbenzyl isocyanate, styrene and a release agent are mixed evenly to form a resin glue. The resin glue is poured into the preheated mold, stirred for 2 minutes to mix, and then heated to 116±2°C for insulation. Then, tert-butyl perbenzoate is added, and the mixture is stirred at 116±2°C for 20 seconds. Then, the mixture is allowed to stand and solidify. After solidification, it is naturally cooled to room temperature and demolded to obtain the fiberglass antenna cover described in this comparative example.
[0052] Comparative Example 3
[0053] A method for preparing a fiberglass antenna cover for comparison, the preparation steps comprising:
[0054] (1) preparing a hydrochloric acid solution, wherein the concentration of the solute in the hydrochloric acid solution is 0.5 mol / L; in an ultrasonic environment, soaking a glass fiber (chopped glass fiber SGF, Chongqing International Composites ECS407-3-K, diameter 13 μm, length 3 mm) in acetone for 10 min to clean and degrease, then performing solid-liquid separation, drying at 60° C. for 20 min, obtaining the cleaned glass fiber, and soaking the cleaned glass fiber in anhydrous ethanol for 10 h, wherein the mass ratio of the glass fiber soaked in anhydrous ethanol is glass fiber: anhydrous ethanol = 1:100; then performing solid-liquid separation, washing the solid phase with deionized water twice, and then soaking it in the hydrochloric acid solution, wherein the mass ratio of the solid phase after the deionized water washing with the hydrochloric acid solution is solid phase: hydrochloric acid solution = 1:100; heating the water bath to 80±5° C. for 6 h of heat preservation, then performing solid-liquid separation, and washing the solid phase with deionized water until the washed liquid is neutral, thereby obtaining the etched glass fiber;
[0055] (2) adding the etched glass fiber to toluene, wherein the mass ratio of the etched glass fiber to toluene is etched glass fiber: toluene = 1:20, and ultrasonic stirring and dispersing for 20 minutes to obtain a dispersion, placing the dispersion in a nitrogen protection environment, and then adding triethylamine, γ-methacryloxypropyl trimethoxysilane and diphenylmethane diisocyanate to the dispersion under stirring, wherein the mass ratio of the added triethylamine, γ-methacryloxypropyl trimethoxysilane and diphenylmethane diisocyanate to the mass ratio of the etched glass fiber in the dispersion is triethylamine: γ-methacryloxypropyl trimethoxysilane: diphenylmethane diisocyanate: etched glass fiber = 0.8:0.4:7:10; after the addition is completed, stirring is continued in a nitrogen atmosphere for 20 hours, and after the stirring is completed, solid-liquid separation is performed, the solid phase is washed twice with toluene, and then washed twice with ethanol, and dried at 60° C. for 5 hours to obtain a once-treated glass fiber;
[0056] (3) preparing a 3,5-diaminobenzoic acid N-methylpyrrolidone solution, wherein the mass percentage of 3,5-diaminobenzoic acid in the 3,5-diaminobenzoic acid N-methylpyrrolidone solution is 4%, and the solvent is N-methylpyrrolidone; adding the once treated glass fiber to the 3,5-diaminobenzoic acid N-methylpyrrolidone solution, wherein the mass ratio of the once treated glass fiber to the 3,5-diaminobenzoic acid N-methylpyrrolidone solution is once treated glass fiber: 3,5-diaminobenzoic acid N-methylpyrrolidone solution = 1:80; then heating in a water bath to 85±5° C. for 6 hours, condensing and refluxing during the insulation process, separating the solid and the liquid after the insulation is completed, washing the solid phase with deionized water 3 times, and drying at 80° C. for 5 hours to obtain a modified glass fiber;
[0057] (4) Weigh the raw materials: unsaturated polyester resin, modified glass fiber, foaming agent, styrene, tert-butyl perbenzoate and release agent respectively, and the raw materials are calculated by weight as follows: 50 parts of unsaturated polyester resin; 5 parts of modified glass fiber; 0.9 parts of foaming agent; 1 part of styrene; 0.6 parts of tert-butyl perbenzoate; 1.7 parts of release agent; wherein the foaming agent is 4,4'-oxybisbenzenesulfonyl hydrazide, and the release agent is zinc stearate; first place the foaming agent in a mold. The mold is preheated at 100°C for 30 minutes, and then the unsaturated polyester resin, modified glass fiber, styrene and release agent are mixed evenly to form a resin glue solution, and the resin glue solution is poured into the preheated mold, stirred for 2 minutes to mix, and then heated to 116±2°C for insulation, and then the tert-butyl peroxybenzoate is added, and the mixture is stirred at 116±2°C for 20 seconds, and then allowed to stand and solidify. After solidification, it is naturally cooled to room temperature and demolded to obtain the fiberglass antenna cover described in this comparative example.
[0058] Example 5
[0059] The antenna covers prepared by the methods described in the above embodiments and comparative examples were cut into 100mm×10mm×2mm strip samples, and the tensile strength of the samples was tested on a universal testing machine, and the tensile speed was set to 50mm / min; in addition, 5 mg of the antenna covers prepared by the methods described in the above embodiments and comparative examples were cut respectively, and thermogravimetric analysis tests were performed in a nitrogen atmosphere, the test temperature range was 0-500°C, the heating rate was set to 5°C / min, and the temperature value corresponding to 5% weight loss was calculated. The results are shown in Table 1.
[0060] As can be seen from Table 1, the FRP antenna cover material prepared by the method of the present invention has good mechanical properties and heat resistance, is not easy to deform and crack during use, and has high thermal stability. It is suitable for long-term service in outdoor high-temperature environments, and is also suitable for use in aviation, mining and other occasions that require high antenna heat resistance. By comparing Example 3 and the comparative examples, it can be seen that the tensile strength and thermal stability of the composite material obtained by the preparation method of Example 3 are higher than those of the comparative examples. This is mainly due to the effect obtained by the present invention by modifying the glass fiber to improve the dispersibility and bonding force of the glass fiber in the resin matrix. The present invention first uses hydrochloric acid to etch the glass fiber, on the one hand to increase the specific surface area of the glass fiber, and on the other hand to hydroxylate the surface of the glass fiber to form a large number of hydroxyl groups to prepare for subsequent modification. Then, the glass fiber is treated with triethylamine, γ-methacryloxypropyl trimethoxysilane and diphenylmethane diisocyanate to isocyanate the glass fiber, change the physical and chemical morphology and active functional group type of the glass fiber surface, and improve the chemical bonding between the glass fiber and the resin, thereby improving the compatibility between the glass fiber and the resin matrix and the interfacial bonding strength between the glass fiber and the matrix; at the same time, γ-methacryloxypropyl trimethoxysilane can graft silane groups on the surface of the glass fiber, and then bond with the silane groups through 3,5-diaminobenzoic acid, so that the dispersion of the glass fiber is improved and agglomeration is reduced. Finally, by adding 3-isopropyl-dimethylbenzyl isocyanate and styrene, a polymer network structure is formed, thereby improving the heat resistance and stability of the material.
[0061] Table 1
[0062] Experimental Group Tensile strength(MPa) 5% weight loss temperature (℃) Example 1 37.7 271 Example 2 38.2 276 Example 3 38.5 278 Example 4 38.0 275 Comparative Example 1 33.3 267 Comparative Example 2 32.9 263 Comparative Example 3 32.4 260
[0063] The technical solution provided by the present invention is introduced in detail above. For those skilled in the art, according to the concept of the embodiments of the present invention, there may be changes in the specific implementation method and application scope. In summary, the content of this specification should not be understood as limiting the present invention.
Claims
1. A method for preparing a highly weather-resistant fiberglass antenna cover, characterized in that: The preparation steps include: (1) preparing a hydrochloric acid solution; in an ultrasonic environment, soaking the glass fiber in acetone for more than 10 minutes to clean and degrease, then performing solid-liquid separation, drying at 60° C. for more than 20 minutes to obtain the cleaned glass fiber, soaking the cleaned glass fiber in anhydrous ethanol for more than 10 hours, then performing solid-liquid separation, washing the solid phase with deionized water for more than 2 times, then soaking it in the hydrochloric acid solution, heating it in a water bath to 80±5° C. and etching it for more than 6 hours, then performing solid-liquid separation, washing the solid phase with deionized water until the washed liquid is neutral, and obtaining the etched glass fiber; (2) adding the etched glass fiber to toluene, stirring and dispersing with ultrasonic wave for more than 20 minutes to obtain a dispersion, placing the dispersion in a nitrogen protection environment, and then adding triethylamine, γ-methacryloxypropyltrimethoxysilane and diphenylmethane diisocyanate to the dispersion under stirring, and continuing to stir in a nitrogen atmosphere for more than 20 hours after the addition is completed. After the stirring is completed, the solid-liquid separation is carried out, the solid phase is washed with toluene for more than 2 times, and then washed with ethanol for more than 2 times, and dried at 60° C. for more than 5 hours to obtain a treated glass fiber; (3) preparing a 3,5-diaminobenzoic acid N-methylpyrrolidone solution; adding the once treated glass fiber to the 3,5-diaminobenzoic acid N-methylpyrrolidone solution, and then heating the glass fiber in a water bath to 85±5° C. and keeping the temperature for more than 6 hours, condensing and refluxing during the insulation process, separating the solid and the liquid after the insulation is completed, washing the solid phase with deionized water for more than 3 times, and drying at 80° C. for more than 5 hours to obtain a modified glass fiber; (4) Weigh the raw materials respectively: unsaturated polyester resin, the modified glass fiber, foaming agent, 3-isopropyl-dimethylbenzyl isocyanate, styrene, tert-butyl perbenzoate and a release agent, first place the foaming agent in a mold, and preheat the mold at 100° C. for 30 to 40 minutes, then mix the unsaturated polyester resin, modified glass fiber, 3-isopropyl-dimethylbenzyl isocyanate, styrene and the release agent to form a resin glue, pour the resin glue into the preheated mold, stir for 2 to 3 minutes to mix, then heat to 116±2° C. and keep warm, then add the tert-butyl perbenzoate, keep warm at 116±2° C. and stir for 20 to 30 seconds, then let it stand and cure, naturally cool to room temperature after curing, and demold to obtain the fiberglass antenna cover.
2. The method for preparing a highly weather-resistant fiberglass antenna cover according to claim 1, characterized in that: In the step (1), the concentration of the solute in the hydrochloric acid solution is 0.5 mol / L, the mass ratio of the glass fiber immersed in the anhydrous ethanol is glass fiber: anhydrous ethanol = 1:100; the mass ratio of the solid phase after washing with deionized water immersed in the hydrochloric acid solution is solid phase: hydrochloric acid solution = 1:
100.
3. The method for preparing a highly weather-resistant fiberglass antenna cover according to claim 1, characterized in that: In the step (2), the mass ratio of toluene added to the etched glass fiber is etched glass fiber: toluene = 1:20, and the mass ratio of triethylamine, γ-methacryloxypropyltrimethoxysilane and diphenylmethane diisocyanate added to the mass ratio of the etched glass fiber in the dispersion is triethylamine:γ-methacryloxypropyltrimethoxysilane:diphenylmethane diisocyanate:etched glass fiber = 0.7-0.8:0.3-0.5:6-8:
10.
4. The method for preparing a highly weather-resistant fiberglass antenna cover according to claim 1, characterized in that: In the step (3), in the N-methylpyrrolidone solution of 3,5-diaminobenzoic acid, the mass percentage of 3,5-diaminobenzoic acid is 3% to 4%, the solvent is N-methylpyrrolidone, and the mass ratio of the once-treated glass fiber added to the N-methylpyrrolidone solution of 3,5-diaminobenzoic acid is once-treated glass fiber: 3,5-diaminobenzoic acid N-methylpyrrolidone solution = 1:
80.
5. The method for preparing a highly weather-resistant fiberglass antenna cover according to claim 1, characterized in that: In the step (4), the raw materials are calculated by weight as follows: 50 parts of unsaturated polyester resin; 4-5 parts of modified glass fiber; 0.8-1 part of foaming agent; 1-2 parts of 3-isopropyl-dimethylbenzyl isocyanate; 0.9-1 part of styrene; 0.5-0.6 parts of tert-butyl perbenzoate; and 1.6-1.8 parts of release agent.
6. The method for preparing a highly weather-resistant fiberglass antenna cover according to claim 5, characterized in that: The foaming agent is 4,4'-oxybisbenzenesulfonyl hydrazide, and the release agent is zinc stearate.