Bitype piperidine cation and anion exchange membrane as well as preparation method and application thereof
By introducing non-rotating aromatic hydrocarbons with brominated alkyl side chains into the anion exchange membrane, the grafted piperidine cation is solved, and the problem of taking into account both mechanical stability and conductivity of the anion exchange membrane is achieved, and high conductivity and resistance are achieved Alkaline stability, suitable for applications in hydrogen energy technology.
Patent Information
- Application Number
- CN202411382172.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-09-30
AI Technical Summary
When pursuing high mechanical stability, existing anion exchange membranes are difficult to take into account both high conductivity and chemical stability, which limits their application in hydrogen energy technology.
The preparation method of a bitype piperidine cation anion exchange membrane is adopted. By introducing non-rotating aromatic hydrocarbons containing bromine alkyl side chains, grafted piperidine cations are formed, increasing the width of the ion channel and improving chemical stability, combining with a stable ring shaped structure to enhance conductivity and mechanical strength.
It achieves high conductivity, low water absorption swelling rate and excellent alkali resistance stability, and has a peak power density of 1.38W/cm2, which is suitable for alkaline fuel cells and alkaline electrolytic water materials.
Smart Images

Figure CN119060280A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer materials, and in particular relates to a bi-piperidinium cation anion exchange membrane and a preparation method and application thereof. Background Art
[0002] In response to the urgent need for global energy transformation and climate change, hydrogen energy, as a clean and efficient alternative energy source, is increasingly becoming a research hotspot in the international energy field; hydrogen energy is not only seen as a key way to reduce dependence on fossil fuels and reduce greenhouse gas emissions, but also carries the important mission of promoting the transformation of the global energy structure towards a low-carbon and sustainable direction. The rise of the hydrogen economy depends on the synchronous development and breakthroughs of upstream and downstream technologies in the hydrogen energy industry chain. Among them, hydrogen fuel cells and water electrolysis hydrogen production technologies are the two core links in the utilization and production of hydrogen energy, and their performance optimization and technological innovation are particularly critical.
[0003] As the core component of alkaline hydrogen fuel cells and alkaline water electrolysis systems, the performance of anion exchange membranes directly affects the energy conversion efficiency and long-term operating stability of the entire system. An ideal anion exchange membrane should have high ionic conductivity, excellent chemical stability (to resist degradation in a strong alkaline environment) and excellent mechanical stability to ensure that the equipment operates under high efficiency and long life conditions. However, the major challenge facing current technology is that improving a certain performance is often accompanied by the sacrifice of other performances. In particular, it is difficult to take into account the simultaneous optimization of conductivity and chemical stability while pursuing high mechanical stability. This seriously restricts the widespread promotion and performance improvement of anion exchange membranes in practical applications.
[0004] Therefore, developing an innovative anion exchange membrane material that has high electrical conductivity and chemical stability while also having excellent mechanical strength has become the key to pushing hydrogen energy technology to new heights and accelerating the arrival of the hydrogen economy era. Summary of the invention
[0005] In view of the above-mentioned prior art, the present invention discloses a bi-type piperidine cation anion exchange membrane and a preparation method and application thereof, so as to solve the technical problems of the anion exchange membrane in the prior art, such as poor conductivity, poor chemical stability, poor mechanical stability, etc.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is: to provide a method for preparing a bi-type piperidinium cation anion exchange membrane, which comprises the following steps:
[0007] S1: Reaction precursor 1, reaction precursor 2 and N-methyl-4-piperidone are dissolved in a solvent, stirred evenly, and trifluoroacetic acid and trifluoromethanesulfonic acid are added to the resulting solution at -5 to 5°C, and the mixture is kept warm for reaction, and then the reaction solution is precipitated in a neutral solution, washed and dried to obtain a polymer solid; Reaction precursor 1 is one of the compounds represented by formula (I), wherein n is an integer of 1 to 15,
[0008]
[0009] Reaction precursor 2 is one of the compounds represented by formula (II),
[0010]
[0011] S2: dissolving the polymer solid with a polar solvent to obtain a polymer solution with a concentration of 3 to 20 wt%, adding methyl iodide and an alkaline substance to the polymer solution, reacting at 20 to 50° C. for 12 to 48 hours, dropping the reaction solution into the solvent for precipitation, and then filtering, washing and drying to obtain a main chain piperidine cationic polyelectrolyte resin;
[0012] S3: dissolving the main chain piperidinium cationic polyelectrolyte resin with a polar solvent to obtain a polyelectrolyte resin solution with a concentration of 3 to 20 wt%, adding N-methylpiperidine to the polyelectrolyte resin solution, reacting at 20 to 50° C. for 12 to 48 hours, dropping the reaction solution into the solvent for precipitation, and then filtering, washing and drying to obtain a bi-piperidinium cationic anion exchange resin;
[0013] S4: dissolving the bipiperidinium cationic anion exchange resin in a polar solvent to obtain a bipiperidinium cationic anion exchange resin solution having a concentration of 3 to 30 wt%, casting the bipiperidinium cationic anion exchange resin solution on a glass plate, drying it, and then soaking it in an alkaline solution, washing it, and drying it to obtain the product.
[0014] Based on the above technical solution, the present invention can also be improved as follows.
[0015] Furthermore, in step S1, the usage ratio of reaction precursor 1, reaction precursor 2, N-methyl-4-piperidone, solvent, trifluoroacetic acid and trifluoromethanesulfonic acid is 2-50 mmol: 50-95 mmol: 100-130 mmol: 5-10 ml: 1-5 ml: 5-10 ml; and the solvent in step S1 is dichloromethane.
[0016] Furthermore, the reaction time in step S1 is 5 to 24 hours; the neutral solution is at least one of NaCl, KCl and Na2SO4 aqueous solutions; and the drying temperature in steps S1, S2 and S3 is 55 to 65°C.
[0017] Furthermore, in step S2, the alkaline substance is at least one of KOH, NaOH, NH3·H2O and Ca(OH)2, and the mass ratio of the polymer solid, the alkaline substance and methyl iodide is 1:0.5-5:1-5; in steps S2, S3 and S4, the polar solvent is at least one of tetrahydrofuran, acetonitrile, N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide and dimethyl sulfoxide.
[0018] Furthermore, in steps S2 and S3, the solvent is ethyl acetate.
[0019] Furthermore, in step S3, the mass ratio of N-methylpiperidine to the main chain piperidine cationic polyelectrolyte resin is 1 to 5:1.
[0020] Furthermore, in step S4, the drying temperature is 50-80° C., and the drying time is 8-24 hours; the alkaline solution is a KOH aqueous solution with a concentration of 1 wt%; the soaking temperature is 55-65° C.; and the soaking time is 12-48 hours.
[0021] Furthermore, in step S4, the drying temperature is 45-55°C.
[0022] The invention also discloses the use of the bi-piperidinium cation anion exchange membrane in the preparation of alkaline fuel cell materials, carbon dioxide reduction electrolyte materials or alkaline water electrolysis materials.
[0023] The beneficial effects of the present invention are:
[0024] 1. The present invention introduces a non-rotatable aromatic hydrocarbon containing a brominated alkyl side chain into the main chain piperidinium cation polymer structure. The rigid structure of the non-rotatable aromatic hydrocarbon helps to maintain the stability of the polymer structure. Then, the bromine atom in the brominated alkyl side chain in the non-rotatable aromatic hydrocarbon reacts with a piperidinium cation precursor containing a reactive group to form a grafted piperidinium cation. The presence of the side chain can increase the distance between polymer chains to form a more spacious ion channel, thereby improving the conductivity. The piperidinium cation has a stable cyclic structure, and the dual-type piperidinium cation structure can improve the conductivity of the membrane and also enhance its chemical stability.
[0025] 2. The bi-type piperidinium cation anion exchange membrane prepared by the present invention has high conductivity, low water absorption and swelling rate, and good mechanical strength.
[0026] 3. The bi-piperidinium cationic anion exchange membrane prepared by the present invention has excellent alkali resistance and stability. When the membrane is immersed in a KOH solution at 80° C., the degradation rate of the cationic group can be as low as 7.6% after 1000 hours.
[0027] 4. The bi-piperidinium cation anion exchange membrane prepared by the present invention has excellent fuel cell performance, with a peak power density of up to 1.38 W / cm 2.
[0028] 5. The preparation method of the present invention is simple and efficient. The prepared bi-piperidinium cation anion exchange membrane can be used to prepare alkaline fuel cell materials or alkaline water electrolysis materials, and can also be used in the fields of electrodialysis, organic electrosynthesis or carbon dioxide catalytic reduction technology. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 The conductivity of the samples in Examples 1 to 3 and Comparative Example 1 varies with temperature;
[0030] Figure 2 It is the tensile strength curve diagram of the samples in Examples 1 to 3 and Comparative Example 1;
[0031] Figure 3 The alkali resistance stability test results of the samples in Examples 1 to 3 and Comparative Example 1 are shown;
[0032] Figure 4 The water absorption rate of the samples in Examples 1 to 3 and Comparative Example 1 varies with temperature;
[0033] Figure 5 The swelling ratio of the samples in Examples 1 to 3 and Comparative Example 1 varies with temperature;
[0034] Figure 6 This is the polarization curve of the sample fuel cell in Example 1. DETAILED DESCRIPTION
[0035] The specific implementation modes of the present invention are described in detail below with reference to the embodiments.
[0036] Example 1
[0037] A method for preparing a bi-piperidinium cation anion exchange membrane, the method comprising the following steps:
[0038] S1: Add 5 mmol of reaction precursor 1, 95 mmol of reaction precursor 2 and 100 mmol of N-methyl-4-piperidone to a 50 mL round-bottom flask. The structures of reaction precursor 1 and reaction precursor 2 are shown below:
[0039] Reaction Precursor 1
[0040] Reaction Precursor 2
[0041] The round-bottom flask was fixed on a magnetic stirrer device, and 5 mL of dichloromethane was added, and the reaction precursor was dissolved by stirring. Then, the round-bottom flask was placed in a basin filled with ice water, and the temperature of the solution in the round-bottom flask was monitored by a thermometer. At 0°C, 1 mL of trifluoroacetic acid and 5 mL of trifluoromethanesulfonic acid were sequentially added dropwise to the solution, and then the temperature was kept to react for 5 hours. Then, the reaction solution was added to a sodium chloride aqueous solution, and a polymer solid was obtained after precipitation and filtration. The polymer solid was washed with pure water until its pH was neutral, and then dried at 60°C.
[0042] S2: Add 1 g of the dried polymer solid and tetrahydrofuran to another round-bottom flask, stir and dissolve at 60°C to obtain a polymer solution with a concentration of 3 wt%. When the polymer solution is cooled to room temperature, add 2 g of methyl iodide and 1 g of sodium hydroxide to the polymer solution, keep stirring and react at 40°C for 12 hours. After the reaction is completed, add the reaction solution dropwise to ethyl acetate for precipitation, filter and wash the solid with pure water until the pH is neutral, and then dry it at 60°C to obtain a main chain piperidine cationic polyelectrolyte resin;
[0043] S3: Add 1 g of dried main-chain piperidinium cationic polyelectrolyte resin and tetrahydrofuran to another round-bottom flask, stir and dissolve at 60° C. to obtain a polyelectrolyte resin solution with a concentration of 3 wt%. When the polyelectrolyte resin solution is cooled to room temperature, add 2 g of N-methylpiperidine to the polyelectrolyte resin solution, and then stir and react at 40° C. for 12 h. After the reaction is completed, add the reaction solution dropwise to ethyl acetate for precipitation, filter and wash the solid with pure water until the pH is neutral, and then dry it at 60° C. to obtain a bi-type piperidinium cationic anion exchange resin;
[0044] S4: 1 g of the bipiperidinium cationic anion exchange resin obtained in step S3 is dissolved in N,N-dimethylformamide to obtain a bipiperidinium cationic anion exchange resin solution with a concentration of 4 wt%, and the bipiperidinium cationic anion exchange resin solution is cast on a glass plate, dried at 50° C. for 24 h to form a film, and then the dried film is placed in a 1 mol / L potassium hydroxide aqueous solution and soaked at 60° C. for 12 h. After taking out, the residual potassium hydroxide is washed with pure water, and then the film is placed in a vacuum drying oven for drying, the drying temperature is 50° C., the vacuum degree is -0.1 MPa, and the drying time is 10 h. After drying, a bipiperidinium cationic anion exchange membrane is obtained.
[0045] Example 2
[0046] A method for preparing a bi-piperidinium cation anion exchange membrane, the method comprising the following steps:
[0047] S1: 30 mmol of reaction precursor 1, 70 mmol of reaction precursor 2 and 120 mmol of N-methyl-4-piperidone were added to a 50 mL round-bottom flask. The structures of reaction precursor 1 and reaction precursor 2 are shown below:
[0048] Reaction Precursor 1
[0049] Reaction Precursor 2
[0050] The round-bottom flask was fixed on a magnetic stirrer device, and 10 mL of dichloromethane was added, and the reaction precursor was dissolved by stirring. Then, the round-bottom flask was placed in a basin filled with ice water, and the temperature of the solution in the round-bottom flask was monitored by a thermometer. At 0° C., 3 mL of trifluoroacetic acid and 10 mL of trifluoromethanesulfonic acid were sequentially added dropwise to the solution, and then the temperature was kept to react for 12 hours. Then, the reaction solution was added to a sodium sulfate aqueous solution, and a polymer solid was obtained after precipitation and filtration. The polymer solid was washed with pure water until its pH was neutral, and then dried at 55° C.;
[0051] S2: Add 1g of the dried polymer solid and N,N-dimethylformamide to another round-bottom flask, stir and dissolve at 40°C to obtain a polymer solution with a concentration of 10wt%. When the polymer solution is cooled to room temperature, add 4g of iodomethane and 3g of calcium hydroxide to the polymer solution, and then stir and keep warm at 40°C for 36h. After the reaction is completed, add the reaction solution dropwise to ethyl acetate for precipitation, filter and wash the solid with pure water until the pH is neutral, and then dry it at 60°C to obtain a main chain piperidine cationic polyelectrolyte resin;
[0052] S3: Add 1 g of dried main-chain piperidinium cationic polyelectrolyte resin and tetrahydrofuran to another round-bottom flask, stir and dissolve at 60° C. to obtain a polyelectrolyte resin solution with a concentration of 8 wt%. When the polyelectrolyte resin solution is cooled to room temperature, add 2 g of N-methylpiperidine to the polyelectrolyte resin solution, and then stir and react at 35° C. for 12 h. After the reaction is completed, add the reaction solution dropwise to ethyl acetate for precipitation, filter and wash the solid with pure water until the pH is neutral, and then dry it at 60° C. to obtain a bi-type piperidinium cationic anion exchange resin;
[0053] S4: 1 g of the bipiperidinium cationic anion exchange resin obtained in step S3 is dissolved in acetonitrile to obtain a bipiperidinium cationic anion exchange resin solution with a concentration of 20 wt%, and the bipiperidinium cationic anion exchange resin solution is cast on a glass plate, dried at 70° C. for 20 h to form a film, and then the dried film is placed in a 1 mol / L potassium hydroxide aqueous solution and soaked at 62° C. for 36 h. After taking out, the residual potassium hydroxide is washed with pure water, and then the film is placed in a vacuum drying oven for drying, the drying temperature is 54° C., the vacuum degree is -0.1 MPa, and the drying time is 10 h. After drying, a bipiperidinium cationic anion exchange membrane is obtained.
[0054] Example 3
[0055] A method for preparing a bi-piperidinium cation anion exchange membrane, the method comprising the following steps:
[0056] S1: Add 10 mmol of reaction precursor 1, 90 mmol of reaction precursor 2 and 130 mmol of N-methyl-4-piperidone to a 50 mL round-bottom flask. The structures of reaction precursor 1 and reaction precursor 2 are shown below:
[0057] Reaction Precursor 1
[0058] Reaction Precursor 2
[0059] The round-bottom flask was fixed on a magnetic stirrer device, and 7 mL of dichloromethane was added, and the reaction precursor was dissolved by stirring. Then, the round-bottom flask was placed in a basin filled with ice water, and the temperature of the solution in the round-bottom flask was monitored by a thermometer. At 0°C, 2 mL of trifluoroacetic acid and 7 mL of trifluoromethanesulfonic acid were sequentially added dropwise to the solution, and then the temperature was kept to react for 10 hours. Then, the reaction solution was added to a potassium chloride aqueous solution, and a polymer solid was obtained after precipitation and filtration. The polymer solid was washed with pure water until its pH was neutral, and then dried at 65°C.
[0060] S2: Add 1g of the dried polymer solid and N-methylpyrrolidone to another round-bottom flask, stir and dissolve at 40°C to obtain a polymer solution with a concentration of 5wt%. When the polymer solution is cooled to room temperature, add 3g of iodomethane and 2g of potassium hydroxide to the polymer solution, and then stir and react at 50°C for 24h. After the reaction is completed, add the reaction solution dropwise to ethyl acetate for precipitation, filter and wash the solid with pure water until the pH is neutral, and then dry it at 60°C to obtain a main chain piperidine cationic polyelectrolyte resin;
[0061] S3: Add 1 g of dried main chain piperidine cationic polyelectrolyte resin and N-methylpyrrolidone to another round-bottom flask, stir and dissolve at 40° C. to obtain a polyelectrolyte resin solution with a concentration of 5 wt%. When the polyelectrolyte resin solution is cooled to room temperature, add 3 g of N-methylpiperidine to the polyelectrolyte resin solution, and then stir and react at 20° C. for 36 hours. After the reaction is completed, add the reaction solution dropwise to ethyl acetate for precipitation, filter and wash the solid with pure water until the pH is neutral, and then dry it at 60° C. to obtain a bi-type piperidine cationic anion exchange resin;
[0062] S4: 1 g of the bipiperidinium cationic anion exchange resin obtained in step S3 is dissolved in dimethyl sulfoxide to obtain a bipiperidinium cationic anion exchange resin solution with a concentration of 3 wt %, and the bipiperidinium cationic anion exchange resin solution is cast on a glass plate, dried at 60° C. for 12 h to form a film, and then the dried film is placed in a 1 mol / L potassium hydroxide aqueous solution and soaked at 60° C. for 24 h. After taking out, the residual potassium hydroxide is washed with pure water, and then the film is placed in a vacuum drying oven for drying, the drying temperature is 50° C., the vacuum degree is -0.1 MPa, and the drying time is 10 h. After drying, a bipiperidinium cationic anion exchange membrane is obtained.
[0063] Example 4
[0064] A method for preparing a bi-piperidinium cation anion exchange membrane, the method comprising the following steps:
[0065] S1: Add 2 mmol of reaction precursor 1, 50 mmol of reaction precursor 2 and 130 mmol of N-methyl-4-piperidone to a 50 mL round-bottom flask. The structures of reaction precursor 1 and reaction precursor 2 are shown below:
[0066] Reaction Precursor 1
[0067] Reaction Precursor 2:
[0068] The round-bottom flask was fixed on a magnetic stirrer device, and 5 mL of dichloromethane was added, and the reaction precursor was dissolved by stirring. Then, the round-bottom flask was placed in a basin filled with ice water, and the temperature of the solution in the round-bottom flask was monitored by a thermometer. At 5° C., 5 mL of trifluoroacetic acid and 5 mL of trifluoromethanesulfonic acid were sequentially added dropwise to the solution, and then the temperature was kept to react for 5 hours. Then, the reaction solution was added to a potassium chloride aqueous solution, and a polymer solid was obtained after precipitation and filtration. The polymer solid was washed with pure water until its pH was neutral, and then dried at 55° C.;
[0069] S2: Add 1g of dried polymer solid and N,N-dimethylacetamide to another round-bottom flask, stir and dissolve at 40°C to obtain a polymer solution with a concentration of 3wt%. When the polymer solution is cooled to room temperature, add 1g of iodomethane and 0.5g of potassium hydroxide to the polymer solution, and then stir and keep warm at 50°C for 12h. After the reaction is completed, add the reaction solution dropwise to ethyl acetate for precipitation, filter and wash the solid with pure water until its pH is neutral, and then dry it at 55°C to obtain a main chain piperidine cationic polyelectrolyte resin;
[0070] S3: Add 1 g of dried main-chain piperidine cationic polyelectrolyte resin and N-methylpyrrolidone to another round-bottom flask, stir and dissolve at 60° C. to obtain a polyelectrolyte resin solution with a concentration of 3 wt%. When the polyelectrolyte resin solution is cooled to room temperature, add 5 g of N-methylpiperidine to the polyelectrolyte resin solution, and then stir and react at 40° C. for 30 h. After the reaction is completed, add the reaction solution dropwise to ethyl acetate for precipitation, filter and wash the solid with pure water until the pH is neutral, and then dry it at 60° C. to obtain a bi-type piperidine cationic anion exchange resin;
[0071] S4: 1 g of the bipiperidinium cationic anion exchange resin obtained in step S3 is dissolved in tetrahydrofuran to obtain a bipiperidinium cationic anion exchange resin solution with a concentration of 10 wt%, and the bipiperidinium cationic anion exchange resin solution is cast on a glass plate, dried at 50° C. for 8 h to form a film, and then the dried film is placed in a 1 mol / L potassium hydroxide aqueous solution and soaked at 55° C. for 12 h. After taking out, the residual potassium hydroxide is washed with pure water, and then the film is placed in a vacuum drying oven for drying, the drying temperature is 45° C., the vacuum degree is -0.1 MPa, and the drying time is 10 h. After drying, a bipiperidinium cationic anion exchange membrane is obtained.
[0072] Example 5
[0073] A method for preparing a bi-piperidinium cation anion exchange membrane, the method comprising the following steps:
[0074] S1: Add 50 mmol of reaction precursor 1, 95 mmol of reaction precursor 2 and 100 mmol of N-methyl-4-piperidone to a 50 mL round-bottom flask. The structures of reaction precursor 1 and reaction precursor 2 are shown below:
[0075] Reaction Precursor 1
[0076] Reaction Precursor 2
[0077] The round-bottom flask was fixed on a magnetic stirrer device, and 10 mL of dichloromethane was added, and the reaction precursor was dissolved by stirring. At -5°C, 5 mL of trifluoroacetic acid and 10 mL of trifluoromethanesulfonic acid were sequentially added to the solution, and then the temperature was kept to react for 24 hours. The reaction solution was then added to a sodium chloride aqueous solution, and a polymer solid was obtained after precipitation and filtration. The polymer solid was washed with pure water until its pH was neutral, and then dried at 60°C.
[0078] S2: Add 1 g of the dried polymer solid and acetonitrile to another round-bottom flask, stir and dissolve at 60°C to obtain a polymer solution with a concentration of 20 wt%. When the polymer solution is cooled to room temperature, add 5 g of iodomethane and 5 g of sodium hydroxide to the polymer solution, and then stir and keep warm at 20°C for 48 hours. After the reaction is completed, add the reaction solution dropwise to ethyl acetate for precipitation, filter and wash the solid with pure water until the pH is neutral, and then dry it at 65°C to obtain a main chain piperidine cationic polyelectrolyte resin;
[0079] S3: Add 1 g of dried main-chain piperidinium cationic polyelectrolyte resin and dimethyl sulfoxide to another round-bottom flask, stir and dissolve at 60° C. to obtain a polyelectrolyte resin solution with a concentration of 12 wt%. When the polyelectrolyte resin solution is cooled to room temperature, add 1 g of N-methylpiperidine to the polyelectrolyte resin solution, and then stir and react at 40° C. for 12 h. After the reaction is completed, add the reaction solution dropwise to ethyl acetate for precipitation, filter and wash the solid with pure water until the pH is neutral, and then dry it at 60° C. to obtain a bi-type piperidinium cationic anion exchange resin;
[0080] S4: 1 g of the bipiperidinium cationic anion exchange resin obtained in step S3 is dissolved in dimethyl sulfoxide to obtain a bipiperidinium cationic anion exchange resin solution with a concentration of 3 wt%, and the polyelectrolyte resin solution is cast on a glass plate, dried at 80° C. for 24 h to form a film, and then the dried film is placed in a 1 mol / L potassium hydroxide aqueous solution and soaked at 65° C. for 48 h. After taking out, the residual potassium hydroxide is washed with pure water, and then the film is placed in a vacuum drying oven for drying at a drying temperature of 55° C., a vacuum degree of -0.1 MPa, and a drying time of 10 h. After drying, a bipiperidinium cationic anion exchange membrane is obtained.
[0081] Example 6
[0082] A method for preparing a bi-piperidinium cation anion exchange membrane, the method comprising the following steps:
[0083] S1: Add 40 mmol of reaction precursor 1, 80 mmol of reaction precursor 2 and 130 mmol of N-methyl-4-piperidone to a 50 mL round-bottom flask. The structures of reaction precursor 1 and reaction precursor 2 are shown below:
[0084] Reaction Precursor 1
[0085] Reaction Precursor 2
[0086] The round-bottom flask was fixed on a magnetic stirrer device, and 10 mL of dichloromethane was added, and the reaction precursor was dissolved by stirring. Then, the round-bottom flask was placed in a basin filled with ice water, and the temperature of the solution in the round-bottom flask was monitored by a thermometer. At 2° C., 5 mL of trifluoroacetic acid and 10 mL of trifluoromethanesulfonic acid were sequentially added dropwise to the solution, and then the temperature was kept to react for 22 hours. Then, the reaction solution was added to a sodium chloride aqueous solution, and a polymer solid was obtained after precipitation and filtration. The polymer solid was washed with pure water until its pH was neutral, and then dried at 60° C.;
[0087] S2: Add 1g of the dried polymer solid and dimethyl sulfoxide to another round-bottom flask, stir and dissolve at 70°C to obtain a polymer solution with a concentration of 15wt%. When the polymer solution is cooled to room temperature, add 4g of iodomethane and 4g of calcium hydroxide to the polymer solution, and then stir and keep warm at 30°C for 40h. After the reaction is completed, add the reaction solution dropwise to ethyl acetate for precipitation, filter and wash the solid with pure water until the pH is neutral, and then dry it at 60°C to obtain a main chain piperidine cationic polyelectrolyte resin;
[0088] S3: Add 1 g of dried main-chain piperidine cationic polyelectrolyte resin and N,N-dimethylformamide to another round-bottom flask, stir and dissolve at 65° C. to obtain a polyelectrolyte resin solution with a concentration of 15 wt%. When the polyelectrolyte resin solution is cooled to room temperature, add 4 g of N-methylpiperidine to the polyelectrolyte resin solution, and then stir and react at 40° C. for 36 hours. After the reaction is completed, add the reaction solution dropwise to ethyl acetate for precipitation, filter and wash the solid with pure water until the pH is neutral, and then dry it at 60° C. to obtain a bi-type piperidine cationic anion exchange resin;
[0089] S4: 1 g of the bipiperidinium cationic anion exchange resin obtained in step S3 is dissolved in N,N-dimethylacetamide to obtain a bipiperidinium cationic anion exchange resin solution with a concentration of 15 wt%, and the bipiperidinium cationic anion exchange resin solution is cast on a glass plate, dried at 75° C. for 12 h to form a film, and then the dried film is placed in a 1 mol / L potassium hydroxide aqueous solution and soaked at 60° C. for 30 h. After taking out, the residual potassium hydroxide is washed with pure water, and then the film is placed in a vacuum drying oven for drying, the drying temperature is 50° C., the vacuum degree is -0.1 MPa, and the drying time is 10 h. After drying, a bipiperidinium cationic anion exchange membrane is obtained.
[0090] Example 7
[0091] A method for preparing a bi-piperidinium cation anion exchange membrane, the method comprising the following steps:
[0092] S1: Add 20 mmol of reaction precursor 1, 80 mmol of reaction precursor 2 and 130 mmol of N-methyl-4-piperidone to a 50 mL round-bottom flask. The structures of reaction precursor 1 and reaction precursor 2 are shown below:
[0093] Reaction Precursor 1
[0094] Reaction Precursor 2
[0095] The round-bottom flask was fixed on a magnetic stirrer device, and 10 mL of dichloromethane was added, and the reaction precursor was dissolved by stirring. Then, the round-bottom flask was placed in a basin filled with ice water, and the temperature of the solution in the round-bottom flask was monitored by a thermometer. At 3° C., 3 mL of trifluoroacetic acid and 8 mL of trifluoromethanesulfonic acid were sequentially added dropwise to the solution, and then the temperature was kept to react for 24 hours. Then, the reaction solution was added to a sodium sulfate aqueous solution, and a polymer solid was obtained after precipitation and filtration. The polymer solid was washed with pure water until its pH was neutral, and then dried at 60° C.;
[0096] S2: Add 1 g of the dried polymer solid and dimethyl sulfoxide to another round-bottom flask, stir and dissolve at 80°C to obtain a polymer solution with a concentration of 20 wt%. When the polymer solution is cooled to room temperature, add 4 g of iodomethane and 4 g of potassium hydroxide to the polymer solution, keep stirring and react at 50°C for 12 hours. After the reaction is completed, add the reaction solution dropwise to ethyl acetate for precipitation, filter and wash the solid with pure water until the pH is neutral, and then dry it at 60°C to obtain a main chain piperidine cationic polyelectrolyte resin;
[0097] S3: Add 1 g of dried main-chain piperidinium cationic polyelectrolyte resin and tetrahydrofuran to another round-bottom flask, stir and dissolve at 60° C. to obtain a polyelectrolyte resin solution with a concentration of 20 wt%. When the polyelectrolyte resin solution is cooled to room temperature, add 4 g of N-methylpiperidine to the polyelectrolyte resin solution, and then stir and react at 50° C. for 48 h. After the reaction is completed, add the reaction solution dropwise to ethyl acetate for precipitation, filter and wash the solid with pure water until the pH is neutral, and then dry it at 60° C. to obtain a bi-type piperidinium cationic anion exchange resin;
[0098] S4: 1 g of the bipiperidinium cationic anion exchange resin obtained in step S3 is dissolved in N,N-dimethylformamide to obtain a bipiperidinium cationic anion exchange resin solution with a concentration of 27 wt%, and the bipiperidinium cationic anion exchange resin solution is cast on a glass plate, dried at 80° C. for 24 h to form a film, and then the dried film is placed in a 1 mol / L potassium hydroxide aqueous solution and soaked at 60° C. for 48 h. After taking out, the residual potassium hydroxide is washed with pure water, and then the film is placed in a vacuum drying oven for drying, the drying temperature is 50° C., the vacuum degree is -0.1 MPa, and the drying time is 10 h. After drying, a bipiperidinium cationic anion exchange membrane is obtained.
[0099] Example 8
[0100] A method for preparing a bi-piperidinium cation anion exchange membrane, the method comprising the following steps:
[0101] S1: Add 5 mmol of reaction precursor 1, 60 mmol of reaction precursor 2 and 110 mmol of N-methyl-4-piperidone to a 50 mL round-bottom flask. The structures of reaction precursor 1 and reaction precursor 2 are shown below:
[0102] Reaction Precursor 1:
[0103] Reaction Precursor 2
[0104] The round-bottom flask was fixed on a magnetic stirrer device, and 7 mL of dichloromethane was added, and the reaction precursor was dissolved by stirring. At -3°C, 1 mL of trifluoroacetic acid and 7 mL of trifluoromethanesulfonic acid were sequentially added to the solution, and then the temperature was kept to react for 7 hours. The reaction solution was then added to a sodium sulfate aqueous solution, and a polymer solid was obtained after precipitation and filtration; the polymer solid was washed with pure water until its pH was neutral, and then dried at 60°C;
[0105] S2: Add 1 g of the dried polymer solid and tetrahydrofuran to another round-bottom flask, stir and dissolve at 80°C to obtain a polymer solution with a concentration of 7 wt%. When the polymer solution is cooled to room temperature, add 2 g of iodomethane and 2 g of ammonia water to the polymer solution, and then stir and keep warm at 50°C for 17 hours. After the reaction is completed, add the reaction solution dropwise to ethyl acetate for precipitation, filter and wash the solid with pure water until the pH is neutral, and then dry it at 58°C to obtain a main chain piperidine cationic polyelectrolyte resin;
[0106] S3: Add 1 g of dried main-chain piperidinium cationic polyelectrolyte resin and tetrahydrofuran to another round-bottom flask, stir and dissolve at 60° C. to obtain a polyelectrolyte resin solution with a concentration of 5 wt%. When the polyelectrolyte resin solution is cooled to room temperature, add 3 g of N-methylpiperidine to the polyelectrolyte resin solution, and then stir and react at 40° C. for 12 h. After the reaction is completed, add the reaction solution dropwise to ethyl acetate for precipitation, filter and wash the solid with pure water until the pH is neutral, and then dry it at 60° C. to obtain a bi-type piperidinium cationic anion exchange resin;
[0107] S4: Take 1g of the bipiperidinium cationic anion exchange resin obtained in step S3 and dissolve it in N,N-dimethylformamide to obtain a bipiperidinium cationic anion exchange resin solution with a concentration of 5wt%, and cast the polyelectrolyte resin solution on a glass plate, dry it at 55°C for 10h to form a film, then place the dried film in a 1mol / L potassium hydroxide aqueous solution and soak it at 58°C for 16h, take it out and wash the residual potassium hydroxide with pure water, then place the film in a vacuum drying oven for drying, the drying temperature is 48°C, the vacuum degree is -0.1MPa, and the drying time is 10h. After drying, the bipiperidinium cationic anion exchange membrane is obtained.
[0108] Example 9
[0109] A method for preparing a bi-piperidinium cation anion exchange membrane, the method comprising the following steps:
[0110] S1: Add 20 mmol of reaction precursor 1, 60 mmol of reaction precursor 2 and 105 mmol of N-methyl-4-piperidone to a 50 mL round-bottom flask. The structures of reaction precursor 1 and reaction precursor 2 are shown below:
[0111] Reaction Precursor 1
[0112] Reaction Precursor 2
[0113] The round-bottom flask was fixed on a magnetic stirrer device, and 10 mL of dichloromethane was added, and the reaction precursor was dissolved by stirring. Then, the round-bottom flask was placed in a basin filled with ice water, and the temperature of the solution in the round-bottom flask was monitored by a thermometer. At 4° C., 5 mL of trifluoroacetic acid and 10 mL of trifluoromethanesulfonic acid were sequentially added dropwise to the solution, and then the temperature was kept to react for 15 hours. Then, the reaction solution was added to a potassium chloride aqueous solution, and a polymer solid was obtained after precipitation and filtration. The polymer solid was washed with pure water until its pH was neutral, and then dried at 65° C.;
[0114] S2: Add 1g of the dried polymer solid and N-methylpyrrolidone to another round-bottom flask, stir and dissolve at 50°C to obtain a polymer solution with a concentration of 8wt%. When the polymer solution is cooled to room temperature, add 2g of iodomethane and 1g of calcium hydroxide to the polymer solution, and then stir and keep warm at 30°C for 20h. After the reaction is completed, add the reaction solution dropwise to ethyl acetate for precipitation, filter and wash the solid with pure water until the pH is neutral, and then dry it at 60°C to obtain a main chain piperidine cationic polyelectrolyte resin;
[0115] S3: Add 1 g of dried main-chain piperidinium cationic polyelectrolyte resin and tetrahydrofuran to another round-bottom flask, stir and dissolve at 50° C. to obtain a polyelectrolyte resin solution with a concentration of 3 wt%. When the polyelectrolyte resin solution is cooled to room temperature, add 2 g of N-methylpiperidine to the polyelectrolyte resin solution, and then stir and react at 40° C. for 25 h. After the reaction is completed, add the reaction solution dropwise to ethyl acetate for precipitation, filter and wash the solid with pure water until the pH is neutral, and then dry it at 60° C. to obtain a bi-type piperidinium cationic anion exchange resin;
[0116] S4: 1 g of the bipiperidinium cationic anion exchange resin obtained in step S3 is dissolved in N-methylpyrrolidone to obtain a bipiperidinium cationic anion exchange resin solution with a concentration of 30 wt%, and the bipiperidinium cationic anion exchange resin solution is cast on a glass plate, dried at 65° C. for 18 h to form a film, and then the dried film is placed in a 1 mol / L potassium hydroxide aqueous solution and soaked at 60° C. for 22 h. After taking out, the residual potassium hydroxide is washed with pure water, and then the film is placed in a vacuum drying oven for drying, the drying temperature is 55° C., the vacuum degree is -0.1 MPa, and the drying time is 10 h. After drying, a bipiperidinium cationic anion exchange membrane is obtained.
[0117] Comparative Example 1
[0118] A method for preparing an anion exchange membrane, the method comprising the following steps:
[0119] S1: Add 5 mmol of reaction precursor 1, 95 mmol of reaction precursor 2 and 100 mmol of N-methyl-4-piperidone to a 50 mL round-bottom flask. The structures of reaction precursor 1 and reaction precursor 2 are shown below:
[0120] Reaction Precursor 1
[0121] Reaction Precursor 2
[0122] The round-bottom flask was fixed on a magnetic stirrer device, and 5 mL of dichloromethane was added, and the reaction precursor was dissolved by stirring. Then, the round-bottom flask was placed in a basin filled with ice water, and the temperature of the solution in the round-bottom flask was monitored by a thermometer. At 0°C, 1 mL of trifluoroacetic acid and 5 mL of trifluoromethanesulfonic acid were sequentially added dropwise to the solution, and then the temperature was kept to react for 5 hours. Then, the reaction solution was added to a sodium chloride aqueous solution, and a polymer solid was obtained after precipitation and filtration. The polymer solid was washed with pure water until its pH was neutral, and then dried at 60°C.
[0123] S2: Add 1g of the dried polymer solid and tetrahydrofuran to another round-bottom flask, stir and dissolve at 60°C to obtain a polymer solution with a concentration of 3wt%. When the polymer solution is cooled to room temperature, add 2g of iodomethane and 1g of sodium hydroxide to the polymer solution, keep warm and stir at 40°C for 12h, after the reaction is completed, add the reaction solution dropwise to ethyl acetate for precipitation, filter and wash the solid with pure water until its pH is neutral, and then dry it at 60°C to obtain a polyelectrolyte resin;
[0124] S3: Take 1g of the polyelectrolyte resin obtained in step S2 and dissolve it in N,N-dimethylformamide to obtain a polyelectrolyte resin solution with a concentration of 4wt%, and cast the polyelectrolyte resin solution on a glass plate, dry it at 50°C for 24h to form a film, then place the dried film in a 1mol / L potassium hydroxide aqueous solution and soak it at 60°C for 12h. After taking it out, wash the residual potassium hydroxide with pure water, and then place the film in a vacuum drying oven for drying. The drying temperature is 50°C, the vacuum degree is -0.1MPa, and the drying time is 10h. After drying, it is obtained.
[0125] Test example
[0126] The bi-piperidinium cation anion exchange membranes prepared in the embodiments of the present invention have similar performances. Examples 1 to 3 are used as examples to illustrate the performances of related products.
[0127] 1. Conductivity test
[0128] The samples prepared in Examples 1 to 3 and Comparative Example 1 were cut into rectangular film strips of 4 cm × 1 cm and immersed in a solution of 1 mol L -1 The sample was then placed in an aqueous solution of NaOH for 48 h, during which the solution was replaced twice to convert the sample into OH - The sample was quickly clamped in the test fixture, immersed in ultrapure water, and tested using an AC impedance meter (Solartron 1287 & 1260, with a test frequency range of 1 to 10 6 Hz. Then, the conductivity is calculated based on the Nyquist plot of the test results. The results are as follows: Figure 1 As shown in the figure, it can be seen that the conductivity of the bi-piperidinium cation anion exchange membrane in the embodiment is significantly greater than the conductivity of the sample in Comparative Example 1, and its conductivity can be as high as 167.3mS / cm at 30°C, and its conductivity increases with the increase of temperature, and can reach 180-240mS / cm at 60°C and 90°C.
[0129] 2. Mechanical properties test
[0130] The samples prepared in Examples 1 to 3 and Comparative Example 1 were cut into rectangular film strips of 4 cm × 1 cm and tested by an MTS tensile testing machine (E44.104) at room temperature and a tensile speed of 5 mm min. -1 , the results are as follows Figure 2 As shown in the figure, it can be seen that the yield stage and the strengthening stage of the stress-strain curve of the bi-piperidinium cationic anion exchange membrane in the embodiment are later than those in the comparative example, and it can be concluded that the mechanical properties of the bi-piperidinium cationic anion exchange membrane in the embodiment are better.
[0131] 3. Alkali resistance stability test
[0132] The samples prepared in Examples 1 to 3 and Comparative Example 1 were immersed in a 1 mol / L KOH solution at 80°C for 1000 hours to test the degradation rate of the cationic groups. Figure 3 As shown in the figure, it can be seen that the degradation rate of the cationic group of the bi-piperidinium cationic anion exchange membrane in the embodiment after immersion for 1000 hours is significantly lower than that of the comparative example sample, indicating that the bi-piperidinium cationic anion exchange membrane in the embodiment has better alkali resistance and stability.
[0133] 4. Water absorption and swelling test
[0134] The samples prepared in Examples 1 to 3 and Comparative Example 1 were subjected to water absorption and swelling tests, and the dry film and the wet film at different temperatures were tested for mass and length changes. The results are shown in FIG. Figure 4 and Figure 5As shown in the figure, it can be seen that the water absorption and swelling ratio of the bi-piperidinium cation anion exchange membrane in the embodiment are significantly smaller than those in the comparative example.
[0135] 5. Battery performance test
[0136] First, weigh an appropriate amount of commercially available Pt / C and PtRu / C catalysts with a concentration of 60wt% and isopropanol and add them to a sample tube, then add 20μL of a 5wt% bipiperidinium cationic anion exchange resin solution prepared by the bipiperidinium cationic anion exchange resin in Example 1, the solvent is DMSO, the sample tube is ultrasonicated in a water bath for 1h to form a catalyst ink, and the ultrasonically prepared 60wt% Pt / C and PtRu / C catalyst inks are sprayed on both sides of the bipiperidinium cationic anion exchange membrane prepared in Example 1 to form a cathode catalyst layer and an anode catalyst layer, thereby preparing a fuel cell chip (catalyst-coated membrane, CCM) with a loading of 0.4mg / cm 2 ; Finally, the prepared CCM was assembled in a fuel cell testing system (850e Multi Range, Scribner Associates Co) for battery performance testing.
[0137] The test conditions are: battery temperature 80℃, pure hydrogen as fuel, pure oxygen as oxidant, the results are as follows Figure 6 As shown in the figure, it can be seen that the bi-piperidinium cation anion exchange membrane in Example 1 exhibits excellent battery performance, with a peak power density of up to 1.38 W / cm 2 .
[0138] Although the specific implementation of the present invention is described in detail in conjunction with the embodiments, it should not be understood as limiting the scope of protection of this patent. Within the scope described in the claims, various modifications and variations that can be made by those skilled in the art without creative work still fall within the scope of protection of this patent.
Claims
1. A method for preparing a bi-type piperidinium cationic anion exchange membrane, characterized in that: The following steps are involved: S1: Dissolve the reaction precursor 1, the reaction precursor 2 and N-methyl-4-piperidone in a solvent, stir evenly, and add trifluoroacetic acid and trifluoromethanesulfonic acid to the resulting solution at -5 to 5°C, keep the temperature for reaction, then precipitate the reaction solution in a neutral solution, wash and dry to obtain a polymer solid; the reaction precursor 1 is one of the compounds represented by formula (I), wherein n is an integer of 1 to 15, The reaction precursor 2 is one of the compounds represented by formula (II), S2: dissolving the polymer solid with a polar solvent to obtain a polymer solution with a concentration of 3 to 20 wt%, adding methyl iodide and an alkaline substance to the polymer solution, reacting at 20 to 50° C. for 12 to 48 hours, dropping the reaction solution into the solvent for precipitation, filtering, washing and drying to obtain a main chain piperidine cationic polyelectrolyte resin; S3: dissolving the main chain piperidinium cationic polyelectrolyte resin with a polar solvent to obtain a polyelectrolyte resin solution with a concentration of 3 to 20 wt%, adding N-methylpiperidine to the polyelectrolyte resin solution, reacting at 20 to 50° C. for 12 to 48 hours, adding the reaction solution dropwise to the solvent for precipitation, and then filtering, washing and drying to obtain a bi-type piperidinium cationic anion exchange resin; S4: dissolving the bi-piperidinium cationic anion exchange resin in a polar solvent to obtain a bi-piperidinium cationic anion exchange resin solution with a concentration of 3 to 30 wt%, casting the bi-piperidinium cationic anion exchange resin solution on a glass plate, drying it, and then soaking it in an alkaline solution, washing and drying it to obtain the bi-piperidinium cationic anion exchange resin solution.
2. The method for preparing a bi-type piperidinium cationic anion exchange membrane according to claim 1, wherein: In step S1, the amount ratio of reaction precursor 1, reaction precursor 2, N-methyl-4-piperidone, solvent, trifluoroacetic acid and trifluoromethanesulfonic acid is 2-50 mmol: 50-95 mmol: 100-130 mmol: 5-10 ml: 1-5 ml: 5-10 ml; the solvent in step S1 is dichloromethane.
3. The method for preparing a bi-type piperidinium cationic anion exchange membrane according to claim 1, wherein: The reaction time in step S1 is 5 to 24 hours; the neutral solution is at least one of NaCl, KCl and Na2SO4 aqueous solutions; the drying temperature in steps S1, S2 and S3 is 55 to 65°C.
4. The method for preparing a bi-type piperidinium cationic anion exchange membrane according to claim 1, wherein: The alkaline substance in step S2 is at least one of KOH, NaOH, NH3·H2O and Ca(OH)2, and the mass ratio of the polymer solid, the alkaline substance and methyl iodide is 1:0.5-5:1-5; the polar solvent in steps S2, S3 and S4 is at least one of tetrahydrofuran, acetonitrile, N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide and dimethyl sulfoxide.
5. The method for preparing a bi-type piperidinium cationic anion exchange membrane according to claim 1, wherein: The solvent in steps S2 and S3 is ethyl acetate.
6. The method for preparing a bi-type piperidinium cationic anion exchange membrane according to claim 1, wherein: In the step S3, the mass ratio of N-methylpiperidine to the main chain piperidine cationic polyelectrolyte resin is 1 to 5:
1.
7. The method for preparing a bi-piperidinium cationic anion exchange membrane according to claim 1, wherein: In step S4, the drying temperature is 50-80° C., and the drying time is 8-24 hours; the alkaline solution is a KOH aqueous solution with a concentration of 1wt%; the soaking temperature is 55-65° C.; and the soaking time is 12-48 hours.
8. The bi-piperidinium cationic anion exchange membrane according to claim 1, characterized in that: The drying temperature in step S4 is 45-55°C.
9. A bi-piperidinium cationic anion exchange membrane prepared by the method for preparing a bi-piperidinium cationic anion exchange membrane according to any one of claims 1 to 8.
10. Use of the bi-piperidinium cationic anion exchange membrane according to claim 9 in the preparation of alkaline fuel cell materials, carbon dioxide reduction electrolyte materials or alkaline water electrolysis materials.
Citation Information
Patent Citations
Cardo structure-containing isatin aromatic hydrocarbon copolymer, preparation method and application thereof
CN110862516A
Low-swelling ordered branched polyaromatic piperidine alkaline membrane for fuel cell and preparation method of low-swelling ordered branched polyaromatic piperidine alkaline membrane
CN114560997A
Piperidine functionalized ether-bond-free polyarylindole anion exchange membrane as well as preparation method and application thereof
CN115466422A
Polymer, anion exchange membrane and preparation method and application thereof
CN116948153A
Anion exchange membrane based on high free volume main chain and preparation method thereof
CN117986651A