Biodegradable polyurethane and preparation method thereof

A biodegradable polyurethane with a balanced soft segment composition of carboxyl polycaprolactone and polycarbonate oligomers, combined with lysine diisocyanate, addresses the issue of inadequate biodegradability by controlling pH during degradation, enhancing microbial activity and degradation rates.

CN119060290AActive Publication Date: 2024-12-03HUAFON MICROFIBER SHANGHAI
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411170499.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-12-03
Estimated Expiration
2044-08-26

AI Technical Summary

Technical Problem

Existing biodegradable polyurethanes suffer from inadequate biodegradability due to the production of intermediate substances that inhibit microbial activity during the degradation process, and the pH environment created by degradation products is often unsuitable for bacterial metabolism.

Method used

A biodegradable polyurethane composition comprising a soft segment made of carboxyl polycaprolactone oligomer diol and polycarbonate oligomer diol residues, with a balanced molar ratio, and a hard segment formed by lysine diisocyanate, to control the pH environment during degradation by producing acidic and alkaline metabolites, enhancing microbial activity.

Benefits of technology

The polyurethane exhibits improved biodegradability by regulating the pH environment, allowing for faster degradation and higher degradation rates, while maintaining mechanical strength.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to biodegradable polyurethane and a preparation method thereof. The biodegradable polyurethane comprises a first structural unit, a second structural unit, a third structural unit and a fourth structural unit, the first structural unit is a polyester oligomer diol residue, the second structural unit is a micromolecular diol residue, the third structural unit is a micromolecular monohydric alcohol residue, and the fourth structural unit is a diisocyanate residue; the first structural unit serves as a polyurethane soft segment, the first structural unit and the fourth structural unit are connected through carbamate, the second structural unit and the fourth structural unit are connected through carbamate to form a polyurethane hard segment, and the third structural unit and the fourth structural unit are connected through carbamate to form an end group of polyurethane; during preparation, polyester oligomer dihydric alcohol, a catalyst, lysine diisocyanate and a part of solvent are put into a reactor for reaction, then the chain extender and the remaining solvent are added, and finally the terminator is added for reaction. The method is simple; the product degradation performance is excellent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polyurethane materials and relates to a biodegradable polyurethane and a preparation method thereof. Background Art

[0002] Amino acid oligomers have good biocompatibility and degradability, and are often used in the field of synthetic materials to prepare drug carriers, bionic materials, cosmetics and other applications.

[0003] In terms of biodegradable polyurethane, amino acid is a class of compounds with terminal amino group and terminal carboxyl group. The prior art CN114539505A discloses an amino acid modified waterborne polyurethane acrylate and its preparation method, S1, polyol and diisocyanate react to obtain polyurethane soft satin, then add alcohol small molecule chain extender with carboxylic acid group to obtain polyurethane hard segment, and then obtain waterborne polyurethane prepolymer; S2, add acrylate to introduce photocurable group; S3, add neutralizer to neutralize carboxylic acid group; S4, add amino acid small molecule chain extender to extend the chain, and obtain waterborne polyurethane dispersion with solid content of 25-45%; S5, add photoinitiator, stir evenly, and remove organic solvent and triethylamine by rotary evaporation to obtain the material. The material has excellent anti-hydrolysis performance, biocompatibility and mechanical properties, but general biodegradability.

[0004] Patent CN108059706A discloses a biodegradable polyurethane, which is composed of a soft segment and a hard segment, wherein the soft segment is polycaprolactone, and the hard segment is a non-toxic amino acid diisocyanate, wherein the amino acid diisocyanate is lysine diisocyanate and / or L-lysine diisocyanate. The polyurethane has good biosafety and biocompatibility, which is improved compared to the introduction of polyurethane as a small molecule chain extender, but the biodegradability is still not good enough.

[0005] Therefore, it is of great significance to study a biodegradable polyurethane and a preparation method thereof to solve the problems existing in the prior art. Summary of the invention

[0006] The purpose of the present invention is to solve the problems of biodegradable polyurethane and its preparation method in the prior art, and to provide a biodegradable polyurethane and its preparation method.

[0007] To achieve the above object, the technical solution adopted by the present invention is as follows:

[0008] A biodegradable polyurethane comprises a first structural unit, a second structural unit, a third structural unit and a fourth structural unit;

[0009] The first structural unit is a polyester oligomer diol residue, the second structural unit is a small molecule diol residue, the third structural unit is a small molecule monool residue, and the fourth structural unit is a diisocyanate residue;

[0010] The first structural unit serves as a soft segment of the biodegradable polyurethane, the first structural unit is connected to the fourth structural unit via carbamate, the second structural unit is connected to the fourth structural unit via carbamate to form a hard segment of the biodegradable polyurethane, and the third structural unit is connected to the fourth structural unit via carbamate to form an end group of the biodegradable polyurethane;

[0011] The molar ratio of the first structural unit to the second structural unit is 7-9:1-3;

[0012] The polyester oligomer diol residues are composed of carboxyl polycaprolactone oligomer diol residues and polycarbonate oligomer diol residues, the molar ratio of the carboxyl polycaprolactone oligomer diol residues to the polycarbonate oligomer diol residues is 2 to 5:1, and the distribution of the two is random in the polyurethane soft segment molecular structure formed during prepolymerization;

[0013] The polycarbonate oligomer diol residue is a polypropylene carbonate diol residue or a polyethylene carbonate diol residue;

[0014] The diisocyanate residue is a lysine diisocyanate residue;

[0015] The molar ratio of the total amount of the first structural unit and the second structural unit to the fourth structural unit is 1:1.0-1.1;

[0016] The third structural unit is the end group that plays a capping role. It accounts for a very small proportion and its effect on degradation can be ignored.

[0017] As the preferred technical solution:

[0018] In the biodegradable polyurethane as described above, the carboxyl polycaprolactone oligomer diol residue refers to a segment structure that enters into the polymer segment after the reaction of carboxyl polycaprolactone oligomer diol having an acid value of 28 mg to 85 KOH / g.

[0019] In the biodegradable polyurethane as described above, the small molecule diol residue is one or more of a 3-methyl-1,5-pentanediol residue, a dipropylene glycol residue, a 1,3-propanediol residue, a methylpropanediol residue and a neopentyl glycol residue, and the metabolites of these small molecule diol residues have been verified in experiments to be non-toxic to microorganisms.

[0020] In the biodegradable polyurethane as described above, the small molecule monohydric alcohol residue is an isopropanol residue.

[0021] The present invention also provides a method for preparing a biodegradable polyurethane as described in any one of the above items, comprising the following steps:

[0022] (1) putting polyester oligomer diol, catalyst, lysine diisocyanate and a portion of solvent into a reactor, stirring and reacting at 40-60° C. for 0.5-1 h;

[0023] (2) raising the temperature of the system after the reaction in step (1) to 70-100° C., then adding a chain extender and the remaining solvent, and reacting until the system viscosity is 69.9-129.9 Pa·s / 25° C.; the chain extender is a small molecule diol;

[0024] (3) After the reaction in step (2) is completed, the temperature is lowered to below 60° C., a terminator is added, and the reaction is carried out for 0.5 to 1 hour to obtain a biodegradable polyurethane with a viscosity of 70 to 130 Pa·s / 25° C. The terminator is a small molecule monohydric alcohol.

[0025] As the preferred technical solution:

[0026] In the above-mentioned method for preparing a biodegradable polyurethane, the catalyst in step (1) is tetrabutyl titanate or tetraisopropyl titanate. The catalyst used in the preparation process of the invention is a green and environmentally friendly titanate catalyst, which is easily decomposed into titanium dioxide and isopropanol or n-butanol after absorbing water, and will not have an adverse effect on the biodegradation of the invention. Such catalysts will hydrolyze into small molecular alcohols and titanium dioxide when exposed to water, and such degradation products will not affect the metabolic activity of microorganisms;

[0027] In step (2), the small molecular diol is one or more of 3-methyl-1,5-pentanediol, dipropylene glycol, 1,3-propanediol, methyl propanediol and neopentyl glycol;

[0028] In step (3), the small molecule monohydric alcohol is isopropanol, which has been verified to be non-toxic to microorganisms.

[0029] In the method for preparing a biodegradable polyurethane as described above, the mass ratio of the amount of solvent added in step (1) to that in step (2) is 3:7;

[0030] The solvent is one or more of ethyl acetate, butyl acetate and dimethyl sulfoxide;

[0031] Based on the total amount of polyester oligomer diol, small molecule diol, catalyst, lysine diisocyanate and solvent, the added amount of solvent is 70wt%.

[0032] In the method for preparing biodegradable polyurethane as described above, the amount of catalyst used is 0.3% to 3% relative to the total mass of reactants excluding solvent; the molar ratio of the total amount of polyester oligomer diol and small molecule diol to lysine diisocyanate is 1:1.0 to 1.1.

[0033] In the above-mentioned method for preparing a biodegradable polyurethane, based on the total amount of polyester oligomer diol, small molecule diol, catalyst, lysine diisocyanate and solvent, the amount of the terminator added is 0.1-0.2wt%.

[0034] Invention mechanism:

[0035] The development of degradable polyurethane usually needs to consider two points, one is the selection of polyester oligomer diols that are difficult to degrade, and the other is the selection of isocyanates. Usually, polyester oligomer diols are selected as polycaprolactone polyester oligomer diols, and isocyanates need to be selected from non-toxic categories to promote the degradability of the polyurethane structure. The present invention is a technical improvement based on the prior art CN108059706A. The inventors found that the main reason for the poor degradation ability of the prior art is that intermediate substances that inhibit the activity of microorganisms are produced during the degradation process. The degradation of polymers is not achieved overnight, but depends on the metabolic rate of microorganisms, and the metabolic activity of microorganisms is closely related to the environment.

[0036] Polycaprolactone has a certain degree of biodegradability. In nature, polycaprolactone will be degraded by species of Penicillium and Clostridium (such as Clostridium butyricum), and its degradation products contain small molecule carboxylic acids. Lysine isocyanate is a non-toxic isocyanate currently found to be suitable for polyurethane degradation. The degradation products of polyurethane containing this type of isocyanate structure contain lysine. However, the activity of bacteria in nature is closely related to the pH of the environment. During the polyurethane degradation experiment, it was found that the pH value suitable for the growth, metabolism and reproduction of Penicillium and Clostridium butyricum was 6.2-7.5.

[0037] The aqueous solution of small molecule carboxylic acid is acidic, while the aqueous solution of lysine is alkaline, and the pH value of saturated lysine solution is as high as 9.75. Since the degradation rate of polycaprolactone chain segments is slower than that of isocyanate, the degradation environment in the early stage of degradation is usually alkaline. The pH value environment created by the lysine solution formed by degradation will make the activity of bacteria that decompose polycaprolactone in an unsuitable state, thus affecting the degradation effect.

[0038] The innovation of the present invention lies in the discovery of the relationship between isocyanate degradation products and bacterial metabolism. By selecting a polyurethane molecular chain composition that is more suitable for bacterial metabolism, wherein the polyurethane molecular chain contains a structure that can be metabolized into acidic small molecules and a structure that can be metabolized into alkaline small molecules, and by coordinating the content of the two types of structures and the degradation rates of different structures in the degradation process, the pH value of the environment is controlled, thereby improving the degradability of the polyurethane.

[0039] The degradation of polyurethane usually occurs preferentially in the more amorphous polyester polyol soft segment, and simultaneously triggers the degradation of the isocyanate structure connecting the soft segment. The products of the former include lysine, and the products of the latter include small molecule acids and small molecule alcohols.

[0040] Compared with conventional polyurethanes, the proportion of polyester oligomer diol residues in the present invention is relatively high, and the polyester oligomer diol residues should be controlled to account for 70-90 mol% of the total molar number of diol residues. When the polyester oligomer diol residues are less than 70 mol%, the proportion of small molecule diol residues is relatively high, the crystallization area increases, and the overall degradation ability of the polyurethane is seriously reduced; when the polyester oligomer diol residues are greater than 90 mol%, the small molecule diol residues are too few, which will lead to a small content of hard segments composed of them, a reduced crystallization area, and a low tensile strength of the polyurethane, which cannot meet conventional application requirements.

[0041] Among them, the chain segment of the polyester polyol soft segment is longer, so less small molecule acid is produced in the initial stage of decomposition. We found that if carboxyl polycaprolactone oligomer diol is used to replace the traditional polycaprolactone polyester oligomer diol to construct the polyurethane soft segment, the environmental pH value at the initial stage of decomposition decreases. This is because the carboxyl content of the decomposed small molecule acid is higher, and the acid value is higher than the traditional polycaprolactone decomposition acid value; further, when a suitable amount of polypropylene carbonate diol or polyethylene carbonate diol is introduced as the third monomer for copolymerization, the environmental pH value of the obtained polyurethane is further significantly reduced at the same decomposition time in the initial stage of the reaction. The general degradation performance of polycarbonate is not as good as that of the polycaprolactone structure. However, the copolymerization method can break the regularity of the soft segment. After introducing a proper amount of polypropylene carbonate diol or polyethylene carbonate diol as the third monomer for copolymerization, it can be more conducive to improving the degradation performance of the polycaprolactone structure, which in turn drives the degradation of polypropylene carbonate diol residues or polyethylene carbonate diol residues, thereby producing relatively more carboxylic acids in the initial stage of the reaction.

[0042] The degradation of polyester oligomers all starts with the degradation of ester groups, and the metabolites are alcohols and carboxylic acids. Therefore, as the metabolism proceeds, the environmental pH gradually becomes acidic. The metabolism of carboxyl polycaprolactone oligomer diol residues is more conducive to regulating the acidic growth of the metabolic environment than that of polycaprolactone polyester oligomer diol residues.

[0043] A certain amount of polycarbonate oligomer diol residue structure is added to the soft segment, which changes the regularity of polycaprolactone and reduces the crystallinity of polycaprolactone, which is beneficial to increase the biodegradation rate of the soft segment and metabolize more acidic metabolites. The molar ratio of carboxyl polycaprolactone oligomer diol residues to polycarbonate oligomer diol residues is at least 2:1. The introduction of too many polycarbonate oligomer diol residues leads to excessively long polycarbonate oligomer residue chains, which in turn leads to a serious decrease in the degradation ability of the material, resulting in slow degradation, and then leads to insufficient acidic metabolites formed by metabolism, which cannot eliminate the impact of alkaline metabolites on the pH value of the system, and cannot balance the pH value of the system at a level that is conducive to bacterial reproduction; the molar ratio of the two is at most 5:1. Too few polycarbonate oligomer diol residues are not enough to destroy the chain regularity of polycaprolactone, which will lead to an insignificant improvement in the biodegradability of polyurethane.

[0044] Beneficial effects:

[0045] (1) A biodegradable polyurethane of the present invention, wherein the polyurethane molecular chain contains a structure that can be metabolized into an acidic small molecule substance and a structure that can be metabolized into an alkaline small molecule substance, and the pH value of the environment is controlled by coordinating the content of the two types of structures and the degradation speed of different structures in the degradation process, thereby improving the degradability of the polyurethane;

[0046] (2) A method for preparing a biodegradable polyurethane of the present invention can break the regularity of the soft segment and improve the degradation performance of the polycaprolactone structure by introducing polypropylene carbonate or polyethylene carbonate and copolymerizing with carboxyl polycaprolactone oligomer diol, which in turn drives the degradation of polypropylene carbonate diol residues or polyethylene carbonate diol residues. DETAILED DESCRIPTION

[0047] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0048] Terms and Definitions:

[0049] (1) The polyester oligomer diol is a polyester diol having a number average molecular weight of 1000 to 3000.

[0050] (2) The residue refers to the part that enters the polymer chain after the raw materials are polymerized. For example, after the polymerization of HO-A-OH and NCO-B-NCO, the parts that enter the molecular chain are -A- and -B- respectively. After polymerization, the part of polyester oligomer diol that enters the polymer chain is called polyester oligomer diol residue, the part of small molecule diol that enters the polymer chain is called small molecule diol residue, and the part of diisocyanate that enters the polymer chain is called diisocyanate residue.

[0051] (3) The carboxyl polycaprolactone oligomer diol is a polycaprolactone polyester oligomer diol containing a carboxyl group, and is usually prepared by polymerization of caprolactone raw material as a monomer using DMPA as an initiator.

[0052] The test methods involved in the performance indicators in the embodiments and comparative examples of the present invention are as follows:

[0053] (1) Degradation rate: Determined according to ISO 20200:2023 Plastics - Determination of disintegration of plastic materials under simulated composting conditions in laboratory-scale tests, with a test period of 100 days.

[0054] (2) Tensile strength test method: The tensile strength value when the elongation of the sample reaches 100% is measured in accordance with GB / T13022-1991.

[0055] (3) Acid value: The acid value of the carboxyl polycaprolactone oligomer diol raw material is measured using HG / T 2708-1995;

[0056] (4) Viscosity: The viscosity of polyurethane was tested using a Brookfield LVT dial-type rotational viscometer, with a No. 4 rotor, a rotation speed of 3 rpm, and a test temperature of 25°C.

[0057] Some raw material information of the present invention:

[0058] (1) Carboxylic polycaprolactone oligomer diol I: HC1060 purchased from Perstorp Company, acid value 85 mgKOH / g, number average molecular weight 600.

[0059] (2) Carboxylic polycaprolactone oligomer diol II: HC1100 purchased from Perstorp Company, with an acid value of 53 mgKOH / g and a number average molecular weight of 1000.

[0060] (3) Carboxylic polycaprolactone oligomer diol III: HC1200 purchased from Perstorp Company, with an acid value of 28 mgKOH / g and a number average molecular weight of 2000.

[0061] (4) Polycaprolactone oligomer diol: 2100 purchased from Perstorp, acid value 0.3 mgKOH / g.

[0062] (5) Polypropylene carbonate diol: purchased from Huizhou Daya Bay Dazhi Fine Chemical Co., Ltd., brand PPCD222, number average molecular weight of 2000.

[0063] (6) Polypropylene carbonate diol: purchased from Huizhou Daya Bay Dazhi Fine Chemical Co., Ltd., brand PPCD 231, number average molecular weight of 3000.

[0064] (7) Polycarbonate oligomer diol: purchased from Shanghai Shuyu Chemical Co., Ltd., brand SYPC1000, number average molecular weight of 1000.

[0065] (8) 3-Methyl-1,5-pentanediol (CAS No.: 4457-71-0).

[0066] (9) Dipropylene glycol (CAS No.: 25265-71-8).

[0067] (10) 1,3-Propanediol (CAS No.: 504-63-2).

[0068] (11) Methylpropanediol (CAS No.: 2163-42-0).

[0069] (12) Neopentyl glycol (CAS No.: 126-30-7).

[0070] Example 1

[0071] A method for preparing biodegradable polyurethane, the specific steps are as follows:

[0072] (1) Raw material preparation:

[0073] Polyester oligomer diol: carboxyl polycaprolactone oligomer diol III (HC1200) and polycarbonate oligomer diol (PPCD 231) in a molar ratio of 2:1;

[0074] Catalyst: tetrabutyl titanate;

[0075] Lysine diisocyanate;

[0076] Solvent: ethyl acetate;

[0077] Small molecule diol: 3-methyl-1,5-pentanediol;

[0078] Terminator: isopropanol;

[0079] (2) putting polyester oligomer diol, catalyst, lysine diisocyanate and 30% solvent into a reactor and stirring at 40° C. for 1 hour;

[0080] The amount of catalyst used is 0.30% relative to the total mass of the reactants excluding the solvent;

[0081] (3) raising the temperature of the system after the reaction in step (1) to 70° C., then adding a small molecule diol and the remaining 70% of the solvent, and reacting until the system viscosity reaches 69.9 Pa·s / 25° C.;

[0082] The molar ratio of polyester oligomer diol to small molecule diol is 7:1; the molar ratio of the total amount of polyester oligomer diol and small molecule diol to lysine diisocyanate is 1:1.0; based on the total amount of polyester oligomer diol, small molecule diol, catalyst, lysine diisocyanate and solvent, the total amount of solvent added in step (1) and step (2) is 70wt%;

[0083] (4) After the reaction in step (2) is completed, the temperature is lowered to below 60° C., a terminator is added, and the reaction is carried out for 0.5 hours to obtain a biodegradable polyurethane with a viscosity of 70 Pa·s / 25° C.;

[0084] Wherein, based on the total amount of polyester oligomer diol, small molecule diol, catalyst, lysine diisocyanate and solvent, the added amount of the terminator is 0.1wt%.

[0085] The biodegradable polyurethane finally prepared comprises a first structural unit, a second structural unit, a third structural unit and a fourth structural unit; the first structural unit is a polyester oligomer diol residue, the second structural unit is a small molecule diol residue, the third structural unit is an isopropanol residue, and the fourth structural unit is a lysine diisocyanate residue; the first structural unit serves as a soft segment of the biodegradable polyurethane, the first structural unit and the fourth structural unit are connected via carbamate, the second structural unit and the fourth structural unit are connected via carbamate to form a hard segment of the biodegradable polyurethane, and the third structural unit and the fourth structural unit are connected via carbamate to form an end group of the biodegradable polyurethane; the polyester oligomer diol residue is composed of a carboxyl polycaprolactone oligomer diol residue and a polycarbonate oligomer diol residue; the polyurethane end group of the biodegradable polyurethane The tensile strength is 1.5MPa; during the composting process of biodegradable polyurethane, the pH of the composting system on the first day was 7.5, and the degradation rate of biodegradable polyurethane was 0.01%; the pH of the composting system on the third day was 7.4, and the degradation rate of biodegradable polyurethane was 0.07%; the pH of the composting system on the tenth day was 7.3, and the degradation rate of biodegradable polyurethane was 0.14%; the pH of the composting system on the 30th day was 7.1, and the degradation rate of biodegradable polyurethane was 0.93%; the pH of the composting system on the 60th day was 6.8, and the degradation rate of biodegradable polyurethane was 10.8%; the pH of the composting system on the 90th day was 6.5, and the degradation rate of biodegradable polyurethane was 37.8%; the pH of the composting system on the 100th day was 6.3, and the degradation rate of biodegradable polyurethane was 43.8%.

[0086] Comparative Example 1

[0087] A method for preparing a biodegradable polyurethane is basically the same as that of Example 1, except that the polyester oligomer diol is polycaprolactone oligomer diol (2100).

[0088] The tensile strength of the prepared biodegradable polyurethane is 1.4MPa. During the composting process of the biodegradable polyurethane, it is measured that the pH of the composting system on the first day is 8, and the degradation rate of the biodegradable polyurethane is 0; the pH of the composting system on the third day is 7.9, and the degradation rate of the biodegradable polyurethane is 0.001%; ​​the pH of the composting system on the tenth day is 7.9, and the degradation rate of the biodegradable polyurethane is 0.002%; the pH of the composting system on the 30th day is 7.8, and the degradation rate of the biodegradable polyurethane is 0.003%; the pH of the composting system on the 60th day is 7.8, and the degradation rate of the biodegradable polyurethane is 0.09%; the pH of the composting system on the 90th day is 7.7, and the degradation rate of the biodegradable polyurethane is 0.15%; the pH of the composting system on the 100th day is 7.8, and the degradation rate of the biodegradable polyurethane is 0.21%.

[0089] Comparative Example 2

[0090] A method for preparing a biodegradable polyurethane is basically the same as that of Example 1, except that the polyester oligomer diol is carboxyl polycaprolactone oligomer diol III (HC1200).

[0091] The tensile strength of the prepared biodegradable polyurethane is 1.4MPa. During the composting process of the biodegradable polyurethane, the pH of the composting system on the first day was measured to be 7.9, and the degradation rate of the biodegradable polyurethane was 0.003%; the pH of the composting system on the third day was 7.9, and the degradation rate of the biodegradable polyurethane was 0.005%; the pH of the composting system on the tenth day was 7.8, and the degradation rate of the biodegradable polyurethane was 0.01%; the pH of the composting system on the 30th day was 7.7, and the degradation rate of the biodegradable polyurethane was 0.04%; the pH of the composting system on the 60th day was 7.7, and the degradation rate of the biodegradable polyurethane was 0.21%; the pH of the composting system on the 90th day was 7.6, and the degradation rate of the biodegradable polyurethane was 1.01%; the pH of the composting system on the 100th day was 7.6, and the degradation rate of the biodegradable polyurethane was 1.37%.

[0092] Comparative Example 3

[0093] A method for preparing a biodegradable polyurethane is basically the same as Example 1, except that carboxyl polycaprolactone oligomer diol III (HC1200) is replaced by polycaprolactone oligomer diol (2100).

[0094] The tensile strength of the prepared biodegradable polyurethane is 1.5MPa. During the composting process of the biodegradable polyurethane, the pH value of the composting system on the first day is measured to be 7.8, and the degradation rate of the biodegradable polyurethane is 0.001%; ​​the pH value of the composting system on the third day is 7.8, and the degradation rate of the biodegradable polyurethane is 0.002%; the pH value of the composting system on the tenth day is 7.8, and the degradation rate of the biodegradable polyurethane is 0.006%; the pH value of the composting system on the 30th day is 7.7, and the degradation rate of the biodegradable polyurethane is 0.009%; the pH value of the composting system on the 60th day is 7.7, and the degradation rate of the biodegradable polyurethane is 0.11%; the pH value of the composting system on the 90th day is 7.6, and the degradation rate of the biodegradable polyurethane is 0.78%; the pH value of the composting system on the 100th day is 7.6, and the degradation rate of the biodegradable polyurethane is 0.82%.

[0095] Comparing Comparative Examples 1 to 3 with Example 1, it can be found that the degradation rate of the biodegradable polyurethane of Comparative Examples 1 to 3 is low. If carboxyl polycaprolactone oligomer diol is used to replace the traditional polycaprolactone polyester oligomer diol to construct the polyurethane soft segment, the environmental pH value at the initial stage of decomposition decreases. This is because the carboxyl content of the decomposed small molecule acid is higher, and the acid value is higher than that of the traditional polycaprolactone polyester oligomer diol. Further, when a suitable amount of polypropylene carbonate diol or polyethylene carbonate diol is introduced as the third monomer for copolymerization, the environmental pH value of the obtained polyurethane is further significantly reduced under the same decomposition time. In addition, it was found through experiments that controlling the initial pH value within 7.5 is more conducive to bacterial reproduction.

[0096] In Example 1, by adding different types of soft segment structures into the polyurethane structure, the regularity of the polyurethane can be reduced, the proportion of the crystalline segments of the polyurethane can be reduced, and water can enter the interior of the polyurethane molecules more easily, thereby making it easier for the polyurethane to be hydrolyzed from large molecules into small molecules. The hydrolyzed small molecules are more easily decomposed into water and carbon dioxide by bacteria. Therefore, Example 1 has good biodegradability.

[0097] Comparative Example 4

[0098] A method for preparing a biodegradable polyurethane is basically the same as that of Example 1, except that the molar ratio of carboxyl polycaprolactone oligomer diol III to polycarbonate oligomer diol is 1:1.

[0099] The tensile strength of the prepared biodegradable polyurethane is 1.7MPa. During the composting process of the biodegradable polyurethane, the pH of the composting system on the first day was measured to be 7.8, and the degradation rate of the biodegradable polyurethane was 0.002%; the pH of the composting system on the third day was 7.8, and the degradation rate of the biodegradable polyurethane was 0.005%; the pH of the composting system on the tenth day was 7.8, and the degradation rate of the biodegradable polyurethane was 0.003%; the pH of the composting system on the 30th day was 7.7, and the degradation rate of the biodegradable polyurethane was 0.008%; the pH of the composting system on the 60th day was 7.7, and the degradation rate of the biodegradable polyurethane was 0.13%; the pH of the composting system on the 90th day was 7.6, and the degradation rate of the biodegradable polyurethane was 0.94%; the pH of the composting system on the 100th day was 7.7, and the degradation rate of the biodegradable polyurethane was 1%.

[0100] By comparing Comparative Example 4 with Example 1, it can be found that the degradation rate of the biodegradable polyurethane of Comparative Example 4 is lower. This is because the introduction of too many polycarbonate oligomer diol residues leads to excessively long polycarbonate oligomer residue chains, which in turn leads to a serious decrease in the degradation ability of the material, resulting in slow degradation, and further leading to insufficient acidic metabolites formed by metabolism, unable to eliminate the impact of alkaline metabolites on the pH value of the system, and unable to balance the pH value of the system at a level that is conducive to bacterial reproduction.

[0101] Comparative Example 5

[0102] A method for preparing a biodegradable polyurethane is basically the same as Example 1, except that the molar ratio of carboxyl polycaprolactone oligomer diol III to polycarbonate oligomer diol is 6:1.

[0103] The tensile strength of biodegradable polyurethane is 1.3MPa; during the composting process of biodegradable polyurethane, the pH of the composting system on the first day was measured to be 7.7, and the degradation rate of biodegradable polyurethane was 0.004%; the pH of the composting system on the third day was 7.7, and the degradation rate of biodegradable polyurethane was 0.01%; the pH of the composting system on the tenth day was 7.7, and the degradation rate of biodegradable polyurethane was 0.04%; the pH of the composting system on the 30th day was 7.6, and the degradation rate of biodegradable polyurethane was 0.07%; the pH of the composting system on the 60th day was 7.6, and the degradation rate of biodegradable polyurethane was 0.44%; the pH of the composting system on the 90th day was 7.5, and the degradation rate of biodegradable polyurethane was 5.59%; the pH of the composting system on the 100th day was 7.3, and the degradation rate of biodegradable polyurethane was 10.62%.

[0104] By comparing Comparative Example 5 with Example 1, it can be found that the degradation rate of the biodegradable polyurethane in Comparative Example 5 is lower. This is because too few polycarbonate oligomer diol residues are not enough to destroy the chain regularity of polycaprolactone, resulting in no obvious improvement in the biodegradability of the polyurethane.

[0105] Example 2

[0106] A method for preparing biodegradable polyurethane, the specific steps are as follows:

[0107] (1) Raw material preparation:

[0108] Polyester oligomer diol: carboxyl polycaprolactone oligomer diol II (HC1100) and polycarbonate oligomer diol (PPCD222) in a molar ratio of 3:1;

[0109] Catalyst: tetraisopropyl titanate;

[0110] Lysine diisocyanate;

[0111] Solvent: Butyl acetate;

[0112] Small molecule diol: dipropylene glycol;

[0113] Terminator: isopropanol;

[0114] (2) adding polyester oligomer diol, catalyst, lysine diisocyanate and 30% solvent into a reactor and stirring the reaction at 45° C. for 0.8 h;

[0115] The amount of catalyst used is 2% relative to the total mass of the reactants excluding the solvent;

[0116] (3) raising the temperature of the system after the reaction in step (1) to 80° C., then adding a small molecule diol and the remaining 70% of the solvent, and reacting until the system viscosity reaches 92.9 Pa·s / 25° C.;

[0117] The molar ratio of polyester oligomer diol to small molecule diol is 7:3; the molar ratio of the total amount of polyester oligomer diol and small molecule diol to lysine diisocyanate is 1:1.02; based on the total amount of polyester oligomer diol, small molecule diol, catalyst, lysine diisocyanate and solvent, the total amount of solvent added in step (1) and step (2) is 70wt%;

[0118] (4) After the reaction in step (2) is completed, the temperature is lowered to below 60° C., a terminator is added, and the reaction is carried out for 0.7 hours to obtain a biodegradable polyurethane with a viscosity of 93 Pa·s / 25° C.;

[0119] Wherein, based on the total amount of polyester oligomer diol, small molecule diol, catalyst, lysine diisocyanate and solvent, the added amount of the terminator is 0.15wt%.

[0120] The biodegradable polyurethane finally prepared comprises a first structural unit, a second structural unit, a third structural unit and a fourth structural unit; the first structural unit is a polyester oligomer diol residue, the second structural unit is a small molecule diol residue, the third structural unit is an isopropanol residue, and the fourth structural unit is a lysine diisocyanate residue; the first structural unit serves as a soft segment of the biodegradable polyurethane, the first structural unit and the fourth structural unit are connected via carbamate, the second structural unit and the fourth structural unit are connected via carbamate to form a hard segment of the biodegradable polyurethane, and the third structural unit and the fourth structural unit are connected via carbamate to form an end group of the biodegradable polyurethane; the polyester oligomer diol residue is composed of a carboxyl polycaprolactone oligomer diol residue and a polycarbonate oligomer diol residue; the polyurethane end group of the biodegradable polyurethane The tensile strength is 1.9MPa; during the composting process of biodegradable polyurethane, the pH of the composting system on the first day was 7.4, and the degradation rate of biodegradable polyurethane was 0.02%; the pH of the composting system on the third day was 7.3, and the degradation rate of biodegradable polyurethane was 0.09%; the pH of the composting system on the tenth day was 7.0, and the degradation rate of biodegradable polyurethane was 0.23%; the pH of the composting system on the 30th day was 6.8, and the degradation rate of biodegradable polyurethane was 1.76%; the pH of the composting system on the 60th day was 6.8, and the degradation rate of biodegradable polyurethane was 18.9%; the pH of the composting system on the 90th day was 6.7, and the degradation rate of biodegradable polyurethane was 44.5%; the pH of the composting system on the 100th day was 6.2, and the degradation rate of biodegradable polyurethane was 55.4%.

[0121] Example 3

[0122] A method for preparing biodegradable polyurethane, the specific steps are as follows:

[0123] (1) Raw material preparation:

[0124] Polyester oligomer diol: carboxyl polycaprolactone oligomer diol I (HC1060) and polycarbonate oligomer diol (PPCD222) in a molar ratio of 5:1;

[0125] Catalyst: tetrabutyl titanate;

[0126] Lysine diisocyanate;

[0127] Solvent: dimethyl sulfoxide;

[0128] Small molecule diols: 1,3-propylene glycol;

[0129] Terminator: isopropanol;

[0130] (2) adding polyester oligomer diol, catalyst, lysine diisocyanate and 30% solvent into a reactor and stirring the reaction at 50° C. for 0.75 h;

[0131] The amount of catalyst used is 3% relative to the total mass of the reactants excluding the solvent;

[0132] (3) raising the temperature of the system after the reaction in step (1) to 90° C., then adding a small molecule diol and the remaining 70% of the solvent, and reacting until the system viscosity reaches 129.9 Pa·s / 25° C.;

[0133] The molar ratio of polyester oligomer diol to small molecule diol is 8:2; the molar ratio of the total amount of polyester oligomer diol and small molecule diol to lysine diisocyanate is 1:1.05; based on the total amount of polyester oligomer diol, small molecule diol, catalyst, lysine diisocyanate and solvent, the total amount of solvent added in step (1) and step (2) is 70wt%;

[0134] (4) After the reaction in step (2) is completed, the temperature is lowered to below 60° C., a terminator is added, and the reaction is carried out for 1 hour to obtain a biodegradable polyurethane with a viscosity of 130 Pa·s / 25° C.;

[0135] Wherein, based on the total amount of polyester oligomer diol, small molecule diol, catalyst, lysine diisocyanate and solvent, the added amount of the terminator is 0.2wt%.

[0136] The finally prepared biodegradable polyurethane comprises a first structural unit, a second structural unit, a third structural unit and a fourth structural unit; the first structural unit is a polyester oligomer diol residue, the second structural unit is a small molecule diol residue, the third structural unit is an isopropanol residue, and the fourth structural unit is a lysine diisocyanate residue; the first structural unit serves as a soft segment of the biodegradable polyurethane, the first structural unit and the fourth structural unit are connected via carbamate, the second structural unit and the fourth structural unit are connected via carbamate to form a hard segment of the biodegradable polyurethane, and the third structural unit and the fourth structural unit are connected via carbamate to form an end group of the biodegradable polyurethane; the polyester oligomer diol residue is composed of a carboxyl polycaprolactone oligomer diol residue and a polycarbonate oligomer diol residue; the biodegradable polyurethane The tensile strength of the biodegradable polyurethane is 2.2MPa; during the composting process of biodegradable polyurethane, the pH of the composting system on the first day was 7.3, and the degradation rate of the biodegradable polyurethane was 0.05%; the pH of the composting system on the third day was 7.1, and the degradation rate of the biodegradable polyurethane was 0.17%; the pH of the composting system on the tenth day was 6.9, and the degradation rate of the biodegradable polyurethane was 1.1%; the pH of the composting system on the 30th day was 6.5, and the degradation rate of the biodegradable polyurethane was 8.9%; the pH of the composting system on the 60th day was 6.3, and the degradation rate of the biodegradable polyurethane was 47.9%; the pH of the composting system on the 90th day was 6.5, and the degradation rate of the biodegradable polyurethane was 93.2%; the pH of the composting system on the 100th day was 6.6, and the degradation rate of the biodegradable polyurethane was 100%.

[0137] Example 4

[0138] A method for preparing biodegradable polyurethane, the specific steps are as follows:

[0139] (1) Raw material preparation:

[0140] Polyester oligomer diol: carboxyl polycaprolactone oligomer diol II (HC1100) and polycarbonate oligomer diol (SYPC1000) in a molar ratio of 4:1;

[0141] Catalyst: tetraisopropyl titanate;

[0142] Lysine diisocyanate;

[0143] Solvent: a mixed solution of ethyl acetate and butyl acetate in a mass ratio of 1:1;

[0144] Small molecule diols: methyl propanediol and neopentyl glycol in a mass ratio of 1:1;

[0145] Terminator: isopropanol;

[0146] (2) putting polyester oligomer diol, catalyst, lysine diisocyanate and 30% solvent into a reactor and stirring the reaction at 60° C. for 0.5 h;

[0147] The amount of catalyst used is 2% relative to the total mass of the reactants excluding the solvent;

[0148] (3) raising the temperature of the system after the reaction in step (1) to 100° C., then adding a small molecule diol and the remaining 70% of the solvent, and reacting until the system viscosity reaches 109.9 Pa·s / 25° C.;

[0149] The molar ratio of polyester oligomer diol to small molecule diol is 9:3; the molar ratio of the total amount of polyester oligomer diol and small molecule diol to lysine diisocyanate is 1:1.1; based on the total amount of polyester oligomer diol, small molecule diol, catalyst, lysine diisocyanate and solvent, the total amount of solvent added in step (1) and step (2) is 70wt%;

[0150] (4) After the reaction in step (2) is completed, the temperature is lowered to below 60° C., a terminator is added, and the reaction is carried out for 0.8 hours to obtain a biodegradable polyurethane with a viscosity of 110 Pa·s / 25° C.;

[0151] Wherein, based on the total amount of polyester oligomer diol, small molecule diol, catalyst, lysine diisocyanate and solvent, the added amount of the terminator is 0.17wt%.

[0152] The finally prepared biodegradable polyurethane comprises a first structural unit, a second structural unit, a third structural unit and a fourth structural unit; the first structural unit is a polyester oligomer diol residue, the second structural unit is a small molecule diol residue, the third structural unit is an isopropanol residue, and the fourth structural unit is a lysine diisocyanate residue; the first structural unit serves as a soft segment of the biodegradable polyurethane, the first structural unit and the fourth structural unit are connected via carbamate, the second structural unit and the fourth structural unit are connected via carbamate to form a hard segment of the biodegradable polyurethane, and the third structural unit and the fourth structural unit are connected via carbamate to form an end group of the biodegradable polyurethane; the polyester oligomer diol residue is composed of a carboxyl polycaprolactone oligomer diol residue and a polycarbonate oligomer diol residue; the biodegradable polyurethane The tensile strength of biodegradable polyurethane is 4.2MPa; during the composting process of biodegradable polyurethane, the pH of the composting system on the first day was 7.4, and the degradation rate of biodegradable polyurethane was 0.035%; the pH of the composting system on the third day was 7.2, and the degradation rate of biodegradable polyurethane was 0.1%; the pH of the composting system on the tenth day was 6.8, and the degradation rate of biodegradable polyurethane was 0.87%; the pH of the composting system on the 30th day was 6.7, and the degradation rate of biodegradable polyurethane was 3.3%; the pH of the composting system on the 60th day was 6.6, and the degradation rate of biodegradable polyurethane was 23%; the pH of the composting system on the 90th day was 6.4, and the degradation rate of biodegradable polyurethane was 69.1%; the pH of the composting system on the 100th day was 6.5, and the degradation rate of biodegradable polyurethane was 81.1%.

Claims

1. A biodegradable polyurethane, characterized in that: comprising a first structural unit, a second structural unit, a third structural unit and a fourth structural unit; The first structural unit is a polyester oligomer diol residue, the second structural unit is a small molecule diol residue, the third structural unit is a small molecule monool residue, and the fourth structural unit is a diisocyanate residue; The first structural unit serves as a soft segment of the biodegradable polyurethane, the first structural unit is connected to the fourth structural unit via carbamate, the second structural unit is connected to the fourth structural unit via carbamate to form a hard segment of the biodegradable polyurethane, and the third structural unit is connected to the fourth structural unit via carbamate to form an end group of the biodegradable polyurethane; The molar ratio of the first structural unit to the second structural unit is 7-9:1-3; The polyester oligomer diol residue is composed of a carboxyl polycaprolactone oligomer diol residue and a polycarbonate oligomer diol residue, and the molar ratio of the carboxyl polycaprolactone oligomer diol residue to the polycarbonate oligomer diol residue is 2 to 5:1; The polycarbonate oligomer diol residue is a polypropylene carbonate diol residue or a polyethylene carbonate diol residue; The diisocyanate residue is a lysine diisocyanate residue; The molar ratio of the total amount of the first structural unit and the second structural unit to the fourth structural unit is 1:1.0-1.

1.

2. A biodegradable polyurethane according to claim 1, characterized in that: The carboxyl polycaprolactone oligomer diol residue refers to a segment structure that is introduced into a polymer segment after a carboxyl polycaprolactone oligomer diol having an acid value of 28 to 85 mgKOH / g is reacted.

3. The biodegradable polyurethane according to claim 1, characterized in that: The small molecule diol residue is one or more of a 3-methyl-1,5-pentanediol residue, a dipropylene glycol residue, a 1,3-propanediol residue, a methylpropanediol residue and a neopentyl glycol residue.

4. The biodegradable polyurethane according to claim 1, characterized in that: The small molecule monohydric alcohol residue is an isopropanol residue.

5. A method for preparing a biodegradable polyurethane according to any one of claims 1 to 4, characterized in that The steps include: (1) putting polyester oligomer diol, catalyst, lysine diisocyanate and a portion of solvent into a reactor, stirring and reacting at 40-60° C. for 0.5-1 h; (2) raising the temperature of the system after the reaction in step (1) to 70-100° C., then adding a chain extender and the remaining solvent, and reacting until the system viscosity is 69.9-129.9 Pa·s / 25° C.; the chain extender is a small molecule diol; (3) After the reaction in step (2) is completed, the temperature is lowered to below 60° C., a terminator is added, and the reaction is carried out for 0.5 to 1 hour to obtain a biodegradable polyurethane with a viscosity of 70 to 130 Pa·s / 25° C. The terminator is a small molecule monohydric alcohol.

6. The method for preparing a biodegradable polyurethane according to claim 5, characterized in that: In step (1), the catalyst is tetrabutyl titanate or tetraisopropyl titanate; In step (2), the small molecular diol is one or more of 3-methyl-1,5-pentanediol, dipropylene glycol, 1,3-propanediol, methyl propanediol and neopentyl glycol; In step (3), the small molecule monohydric alcohol is isopropanol.

7. The method for preparing a biodegradable polyurethane according to claim 5, characterized in that: The mass ratio of the amount of solvent added in step (1) to that in step (2) is 3:7; The solvent is one or more of ethyl acetate, butyl acetate and dimethyl sulfoxide; Based on the total amount of polyester oligomer diol, small molecule diol, catalyst, lysine diisocyanate and solvent, the added amount of solvent is 70wt%.

8. The method for preparing a biodegradable polyurethane according to claim 5, characterized in that: The molar ratio of the total amount of polyester oligomer diol and small molecule diol to lysine diisocyanate is 1:1.0-1.

1.

9. The method for preparing a biodegradable polyurethane according to claim 5, characterized in that: Based on the total amount of polyester oligomer diol, small molecule diol, catalyst, lysine diisocyanate and solvent, the added amount of the terminator is 0.1-0.2wt%.

Citation Information

Patent Citations

  • Degradable and nontoxic medical polyurethane material and preparation method thereof

    CN101654508A

  • Biodegradable thermoplastic polyamide elastomer and preparation method thereof

    CN114644754A

  • Highly elastic aqueous adhesive composition and method for surface treatment of a molded article using the same

    DE102015226480A1

  • Vehicle composition for coating agent, method for printing plastic film and plastic film printed article

    JP2004083664A

  • High-strength polyurethane adhesive

    US20090266482A1