Bio-based spandex fiber and preparation method thereof

By designing a two-block structure spandex fiber preparation method, the application of spandex fiber in high-end textiles and medical and health fields is solved, and high value-added bio-based spandex fiber is achieved, with excellent mechanical properties and biocompatibility , suitable for medical and health care fields.

CN119060293AActive Publication Date: 2024-12-03ZHONGYUAN ENGINEERING COLLEGE
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411199741.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-03
Estimated Expiration
2044-08-29

AI Technical Summary

Technical Problem

The preparation of existing spandex fibers consumes petrochemical resources, has uncontrollable elongation of breaks, low strength, and poor biological activity, which limits its application in high-end textiles and medical and health fields.

Method used

By designing a spandex fiber preparation method that has excellent properties of biological activity and conventional spandex, diisocyanate and bio-based polydiol are used for prepolymerization, natural products are added for chain expansion and end capping, forming a two-block structure fiber, improving its mechanical properties and biocompatibility.

Benefits of technology

The obtained bio-based spandex fiber has excellent mechanical properties, biocompatibility and antibacterial properties. It can be used in the medical field and imparts excellent health care functions to textiles and sanitary products, increasing the added value of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060293A_ABST
    Figure CN119060293A_ABST
Patent Text Reader

Abstract

The invention provides a bio-based spandex fiber and a preparation method thereof, belongs to the technical field of polymer fiber materials, and aims to solve the technical problems that petrochemical resources are consumed during preparation of spandex fibers and bio-based spandex is uncontrollable in breaking elongation, low in breaking strength and poor in biological activity. The preparation method comprises the following steps: dissolving diisocyanate I and bio-based poly dihydric alcohol in a polar amine solution I, and then carrying out prepolymerization reaction I to prepare a prepolymer solution A; dissolving poly dihydric alcohol and diisocyanate II in a polar amine solution II, and then carrying out a prepolymerization reaction II to prepare an isocyanato-terminated prepolymer solution B; mixing and reacting the prepolymer solution A and the prepolymer solution B, then adding a natural product, continuously reacting, and curing to obtain a spinning solution; and spinning the spinning solution to obtain the bio-based spandex fiber. The fineness of the bio-based spandex fiber is 5-40D, the breaking strength is 1.5-2.1 cN / detx, the breaking elongation is 100-600%, and the bio-based spandex fiber has excellent biocompatibility, antibacterial property and cell regeneration promoting capacity, can be used in the medical fields of artificial blood vessels, skeleton repair, wound dressings and the like, can endow textiles and hygienic products with excellent health-care functions, and has wide application prospects. And the added value of the product is greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer fiber materials, and in particular relates to a bio-based spandex fiber and a preparation method thereof. Background Art

[0002] Spandex has an elasticity that is unmatched by other synthetic fibers. Its elongation at break is as high as 800%, and its elastic recovery rate is over 95%. It is widely used in textiles and clothing, medical and health care, sports, national defense and military industries, etc. A small amount of addition can give textiles excellent elasticity, comfort and shape retention, and it is an indispensable fiber material for high-end textiles. At the same time, it is also widely used in the field of disposable sanitary products such as diapers, protective clothing, and nursing products, as well as in the field of sports and leisure.

[0003] Conventional spandex is prepared by polymerization and spinning of petroleum-based polyether polyols and diisocyanates. Its molecular chain also lacks degradable elements and bioactive components, which is not conducive to reducing carbon emissions and does not meet the requirements of green development of the spandex industry. At the same time, it limits the application of spandex fibers in the field of medical and sanitary materials. Patent CN117127276A prepares bio-based spandex fibers by prepolymerization, chain extension, and spinning of polyether polyols containing bio-based 1,3-propylene glycol structure and conventional diisocyanates. Since the polyether polyols with 1,3-propylene glycol structure are less flexible and have a single structure than polytetramethylene ether glycol (PTMEG), the prepared spandex fibers have relatively low elongation and strength at break and cannot be adjusted. They are also not biologically active and have a single application field. Summary of the invention

[0004] In view of the technical problems of spandex fiber preparation consuming petrochemical resources, uncontrollable elongation at break, low strength and poor biological activity, the present invention proposes a bio-based spandex fiber and a preparation method thereof, and develops spandex fiber with both biological activity and excellent properties of conventional spandex through molecular structure design, which meets the application needs of high-end textiles and medical and sanitary products and greatly improves the added value of the product.

[0005] In order to achieve the above object, the technical solution of the present invention is achieved as follows:

[0006] A method for preparing bio-based spandex fiber, comprising the following steps:

[0007] (1) dissolving diisocyanate I and bio-based polydiol in polar amine solution I, and then performing prepolymerization reaction I to prepare prepolymer solution A;

[0008] (2) dissolving the polydiol and diisocyanate II in a polar amine solution II, and then performing a prepolymerization reaction II to obtain an isocyanate-terminated prepolymer solution B;

[0009] (3) Prepolymer solutions A and B are mixed in a mass ratio of 1:9-9:1 at 60-80° C. for reaction for 60-90 min, and then the natural product is added, followed by chain extension reaction for 30-60 min, and a spinning solution is obtained after aging; (4) The spinning solution is spun to obtain bio-based spandex fiber.

[0010] The diisocyanates I and II are independently selected from one of 4,4'-methylenebis(phenyl isocyanate), dicyclohexylmethane 4,4'-diisocyanate, toluene diisocyanate, and 4,4'-diisocyanato-3,3'-dimethylbiphenyl.

[0011] In the step (1), the molar ratio of diisocyanate I to bio-based polydiol is 1: (1.5-1.8); the conditions of the prepolymerization reaction I are: temperature 80-100°C, time 80-120min, and a solution A with a prepolymer ratio of 20-35wt% is obtained.

[0012] The molar ratio of the polyglycol to diisocyanate II in step (2) is 1:(1.8-2.5); the conditions of the prepolymerization reaction II are: temperature 80-100°C, time 80-120min, and a B solution with a prepolymer ratio of 20-35wt% is obtained.

[0013] The polar amine solutions I and II are independently selected from N,N-dimethylformamide or N,N-dimethylacetamide.

[0014] The bio-based diol is polyether polyol, polylactic acid diol or polyhydroxyacetic acid diol, and the molecular weight of the bio-based diol is 1000-3000; the polyether polyol is prepared by using 1,3-propylene glycol, 1,5-pentanediol and 1,4-butanediol.

[0015] The polyglycol is one of polycaprolactone glycol, polyethylene glycol, polycarbonate glycol and polytetramethylene glycol.

[0016] The spinning solution in step (3) is further added with an auxiliary agent, the amount of which is 0.1-3wt% of the total mass of the spinning solution; the auxiliary agent includes any one or more of an antioxidant, a nanoparticle, a stabilizer, and a flame retardant. The antioxidant is antioxidant 1010, 168, 1135, the nanoparticle is titanium dioxide, zinc oxide, silver, the light stabilizer is light stabilizer 770, 531, 329, and the flame retardant is zinc borate, melamine urate, and aluminum polyphosphate.

[0017] The natural product is one or more of tea polyphenols, anthocyanidins, malic acid, amino acids, alginic acid, and triterpenoid compounds, and the amount used is 1-10wt% of the total amount of prepolymer solutions A and B. The chain extension reaction requires the addition of a diamine chain extender.

[0018] The spinning step in step (4) is as follows: the spinning solution is transported to the spinning box through a metering pump for extrusion, the filaments are solidified and wound in the spinning tunnel to obtain bio-based spandex fibers. The spinning conditions are as follows: the number of filament holes is 30-200 holes, the spinning tunnel is filled with hot air or hot nitrogen at 230-280°C, the gas flow rate is 0.1-3m / s, and the winding speed is 600-1500m / min.

[0019] A bio-based spandex fiber has a fineness of 5-40D, a breaking strength of 1.5-2.1 cN / detx, and a breaking elongation of 100-600%.

[0020] Beneficial effects of the present invention:

[0021] The invention firstly reacts bio-based polydiol with diisocyanate to prepare a hydroxyl-terminated prepolymer solution A; then conventional polydiol and diisocyanate are reacted to prepare an isocyanate-terminated prepolymer solution B; by adjusting the ratio of the two, the two are mixed and chain-extended to give the spandex fiber a two-block structure, and then natural products are added for secondary chain extension and end-capping, so that the molecular chain is further extended and micro-cross-linked, the intermolecular force and biological activity can be enhanced, and the bio-based spandex spinning stock solution with a weight average molecular weight of more than 100,000 is obtained, and the spandex fiber is given excellent mechanical properties that are adjustable and controllable within a certain range. The fineness of the bio-based spandex fiber is 5-40D, the breaking strength is 1.5-2.1cN / detx, and the breaking elongation is 100-600%.

[0022] The spandex fiber involved in the present invention has excellent biocompatibility, antibacterial properties and the ability to promote cell regeneration, and can be used in medical fields such as artificial blood vessels, bone repair, wound dressings, etc. It can also give textiles and sanitary products excellent health functions, greatly improving the added value of the products. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0024] Figure 1 This is the stress-strain curve of the bio-based spandex fiber in Example 1.

[0025] Figure 2 This is a confocal microscopic image of the cytotoxicity of the spandex fiber in Example 1 (green: living cells; red: dead cells) and an apparent morphology microscopic image (magnification 500x).

[0026] Figure 3 This is a confocal microscopic image of the cytotoxicity of spandex fibers in the comparative example (green: living cells; red: dead cells) and an apparent morphology microscopic image (magnification 500x).

[0027] Figure 4 This is the infrared spectrum of the bio-based spandex fiber in Example 2.

[0028] Figure 5 is the chemical structural formula of the bio-based spandex in Example 2. DETAILED DESCRIPTION

[0029] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] Example 1

[0031] A method for preparing bio-based spandex fiber, comprising the following steps: dissolving 4,4'-methylenebis(phenyl isocyanate) and bio-based poly 1,3-propylene glycol with a molecular weight of 1000 in an N,N-dimethylacetamide solution at a molar ratio of 1:1.5, and reacting at 80°C for 80 minutes to prepare a hydroxyl-terminated prepolymer solution A with a concentration of 30wt%; dissolving polyethylene glycol and diisocyanate in an N,N-dimethylacetamide solution at a molar ratio of 1:1.8, and reacting at 80°C for 80 minutes to prepare an isocyanate-terminated prepolymer solution B with a concentration of 30wt%; and mixing the prepolymer solutions A and B in a mass ratio of 1:9 and 1:1. After wt% of antioxidant 1010, nano diatomaceous earth particles, light stabilizer 770, and flame retardant melamine urate are reacted at 60°C for 90 minutes, 8wt% of natural product tea polyphenols and chain extender ethylenediamine are added, and the reaction is continued for 60 minutes. After aging, the spinning solution is obtained; finally, the spinning solution is transported to the spinning box through a metering pump for extrusion, the number of spinnerets is 60, and the filaments are solidified in a spinning channel filled with 250°C hot air, the gas flow rate is 0.1m / s, and the winding speed is 1000m / min, to obtain a bio-based spandex fiber with a fineness of 10D, a breaking strength of 1.6cN / detx, and a breaking elongation of 190%.

[0032] Example 2

[0033] A method for preparing bio-based spandex fiber, comprising the following steps: dissolving 4,4'-methylenebis(phenyl isocyanate) and bio-based poly-1,5-pentanediol with a molecular weight of 2000 in an N,N-dimethylacetamide solution at a molar ratio of 1:1.8, reacting at 90°C for 100 minutes to prepare a hydroxyl-terminated prepolymer solution A with a concentration of 30wt%; dissolving polyethylene glycol and dicyclohexylmethane 4,4'-diisocyanate in an N,N-dimethylacetamide solution at a molar ratio of 1:2.5, reacting at 100°C for 120 minutes to prepare an isocyanate-terminated prepolymer solution B with a concentration of 30wt%; and mixing the prepolymer solutions A and B at a molar ratio of 1:2.5. After reacting at 60°C for 60 minutes with 2 wt% of antioxidant 168, nanoparticle silver, stabilizer 531 and flame retardant zinc borate in a mass ratio of 1:9, 1 wt% of natural product malic acid and chain extender diamine were added, and the reaction was continued for 50 minutes. After aging, the spinning solution was obtained; finally, the spinning solution was transported to the spinning manifold through a metering pump for extrusion, with 60 spinneret holes, and the filaments were solidified in a spinning tunnel filled with 230°C hot air, with a gas flow rate of 0.15 m / s and a winding speed of 600 m / min, to obtain a bio-based spandex fiber with a fineness of 40D, a breaking strength of 1.75 cN / detx, and a breaking elongation of 600%. The bio-based spandex prepared in this example was characterized by infrared, as shown in FIG. Figure 4 As shown, 1750cm -1 It is the characteristic absorption peak of C=O, 3430cm -1 The characteristic absorption peaks of NH are 1510 and 1600 cm -1 It is the characteristic absorption peak of benzene ring, 1470cm -1 = is the characteristic absorption peak of CH2, and it can be determined that the prepared spandex fiber is the target product. The structural formula of the preparation of bio-based ammonia is as follows Figure 5 shown.

[0034] Example 3

[0035] A method for preparing bio-based spandex fiber comprises the following steps: dissolving 4,4'-diisocyanato-3,3'-dimethylbiphenyl and bio-based poly-1,3-propylene glycol with a molecular weight of 1500 in an N,N-dimethylacetamide solution at a molar ratio of 1:1.8, reacting at 100°C for 120 minutes to prepare a hydroxyl-terminated prepolymer solution A with a concentration of 30wt%; dissolving polyethylene glycol and toluene diisocyanate in an N,N-dimethylacetamide solution at a molar ratio of 1:1.5, reacting at 100°C for 120 minutes to prepare an isocyanate-terminated prepolymer solution B with a concentration of 30wt%; mixing the prepolymer solutions A and B in a mass ratio of 9: 1 and 2.5wt% of antioxidant 1135, nanoparticle titanium dioxide, stabilizer 531, and flame retardant melamine urate are reacted at 80°C for 50 minutes, and then 5wt% of natural product amino acid, alginate and chain extender ethylenediamine are added, and the reaction is continued for 60 minutes. After aging, the spinning solution is obtained; finally, the spinning solution is transported to the spinning box through a metering pump for extrusion, the number of spinnerets is 60, and the filaments are solidified in a spinning channel filled with 280°C hot air, the gas flow rate is 1m / s, and the winding speed is 700m / min, to obtain a bio-based spandex fiber with a fineness of 25D, a breaking strength of 1.7cN / detx, and a breaking elongation of 185%.

[0036] Example 4

[0037] A method for preparing bio-based spandex fiber, comprising the following steps: dissolving toluene diisocyanate and bio-based poly 1,4-butanediol with a molecular weight of 1000 in an N,N-dimethylacetamide solution at a molar ratio of 1:1.5, reacting at 80°C for 100 minutes to prepare a hydroxyl-terminated prepolymer solution A with a concentration of 30wt%; dissolving polycarbonate diol and toluene diisocyanate in an N,N-dimethylacetamide solution at a molar ratio of 1:1.8, reacting at 100°C for 120 minutes to prepare an isocyanate-terminated prepolymer solution B with a concentration of 30wt%; mixing the prepolymer solutions A and B at a mass ratio of 4:5 and 2:5, respectively. After wt% of antioxidant 1010, nanoparticle zinc oxide, stabilizer 770, and flame retardant polyaluminum phosphate are reacted at 80°C for 60 minutes, 7wt% of natural product tea polyphenols, amino acids and chain extender propylenediamine are added, and the reaction is continued for 60 minutes. After aging, the spinning solution is obtained; finally, the spinning solution is transported to the spinning box through a metering pump for extrusion, the number of spinnerets is 65, and the filaments are solidified in a spinning channel filled with 240°C hot air, the gas flow rate is 0.5m / s, and the winding speed is 600m / min, to obtain a bio-based spandex fiber with a fineness of 40D, a breaking strength of 1.5cN / detx, and a breaking elongation of 280%.

[0038] Example 5

[0039] A method for preparing bio-based spandex fiber, comprising the following steps: dissolving 4,4'-diisocyanato-3,3'-dimethylbiphenyl and bio-based poly-1,5-pentanediol with a molecular weight of 2000 in an N,N-dimethylacetamide solution at a molar ratio of 1:1.6, and reacting at 95°C for 110 minutes to prepare a hydroxyl-terminated prepolymer solution A with a concentration of 30wt%; dissolving polytetrahydrofuran ether diol and 4,4'-diisocyanato-3,3'-dimethylbiphenyl in an N,N-dimethylacetamide solution at a molar ratio of 1:2.5, and reacting at 80°C for 100 minutes to prepare an isocyanate-terminated prepolymer solution B with a concentration of 30wt%; and mixing the prepolymer solution. A and B are reacted at a mass ratio of 7:3 and 0.1wt% of antioxidant 1010, nanoparticle silver, stabilizer 770, and flame retardant zinc borate at 60°C for 30 minutes, then 10wt% of natural product alginate, triterpenoid compounds and chain extender phenylenediamine are added, and the reaction is continued for 60 minutes. After aging, the spinning solution is obtained; finally, the spinning solution is transported to the spinning box through a metering pump for extrusion, the number of spinnerets is 30, and the filaments are solidified in a spinning channel filled with 250°C hot air, the gas flow rate is 1m / s, and the winding speed is 1500m / min, to obtain a bio-based spandex fiber with a fineness of 5D, a breaking strength of 1.9cN / detx, and a breaking elongation of 310%.

[0040] Example 6

[0041] A method for preparing bio-based spandex fiber comprises the following steps: dissolving 4,4'-methylenebis(phenyl isocyanate) and bio-based polylactic acid diol with a molecular weight of 1500 in an N,N-dimethylacetamide solution at a molar ratio of 1:1.5, and reacting at 90°C for 110 minutes to prepare a hydroxyl-terminated prepolymer solution A with a concentration of 30wt%; dissolving polyethylene glycol and 4,4'-methylenebis(phenyl isocyanate) in an N,N-dimethylacetamide solution at a molar ratio of 1:1.5, and reacting at 100°C for 120 minutes to prepare a 30wt% isocyanate-terminated prepolymer solution B; mixing the prepolymer solutions A and B at a mass ratio of 3:7 and 8:1. 3wt% of antioxidant 1135, nano-particle titanium dioxide, stabilizer 770, and flame retardant melamine urate are reacted at 80°C for 60 minutes, and then 5wt% of natural product alginate, triterpenoid compounds, amino acids and chain extender ethylenediamine are added, and the reaction is continued for 30 minutes. After aging, the spinning solution is obtained; finally, the spinning solution is transported to the spinning box through a metering pump for extrusion, the number of spinnerets is 65, and the filaments are solidified in a spinning channel filled with 260°C hot air, the gas flow rate is 0.5m / s, and the winding speed is 800m / min, to obtain a bio-based spandex fiber with a fineness of 20D, a breaking strength of 1.7cN / detx, and a breaking elongation of 160%.

[0042] Example 7

[0043] A method for preparing bio-based spandex fiber comprises the following steps: dissolving dicyclohexylmethane 4,4'-diisocyanate and bio-based poly(glycolic acid) diol with a molecular weight of 1500 in an N,N-dimethylacetamide solution at a molar ratio of 1:1.6, and reacting at 80°C for 80 minutes to prepare a hydroxyl-terminated prepolymer solution A with a concentration of 30wt%; dissolving polycaprolactone diol and dicyclohexylmethane 4,4'-diisocyanate in an N,N-dimethylacetamide solution at a molar ratio of 1:1.8, and reacting at 105°C for 100 minutes to prepare an isocyanate-terminated prepolymer solution B with a concentration of 30wt%; and mixing the prepolymer solutions A and B at a mass ratio of 1:1.6. 9 and 3wt% of antioxidant 1010, nanoparticle zinc oxide, stabilizer 770, and flame retardant polyaluminum phosphate are reacted at 60°C for 60 minutes, and then 8wt% of natural product alginate, triterpenoid compounds, amino acids and chain extender propylenediamine are added, and the reaction is continued for 45 minutes. After aging, the spinning solution is obtained; finally, the spinning solution is transported to the spinning box through a metering pump for extrusion, the number of spinnerets is 65, and the filaments are solidified in a spinning tunnel filled with 230°C hot air, the gas flow rate is 0.5m / s, and the winding speed is 700m / min, to obtain a bio-based spandex fiber with a fineness of 35D, a breaking strength of 1.55cN / detx, and a breaking elongation of 220%.

[0044] Example 8

[0045] A method for preparing bio-based spandex fiber comprises the following steps: dissolving toluene diisocyanate and bio-based polylactic acid diol with a molecular weight of 1000 in an N,N-dimethylacetamide solution at a molar ratio of 1:1.5, and reacting at 100°C for 120 minutes to prepare a hydroxyl-terminated prepolymer solution A with a concentration of 35wt%; dissolving polycarbonate diol and toluene diisocyanate in an N,N-dimethylacetamide solution at a molar ratio of 1:2.5, and reacting at 80°C for 120 minutes to prepare an isocyanate-terminated prepolymer solution B with a concentration of 20wt%; mixing the prepolymer solutions A and B at a mass ratio of 1:9 and 0.1wt%; After t% of antioxidant 1010, nanoparticle silver, stabilizer 531, and flame retardant zinc borate are fully reacted, 5wt% of natural products malic acid, alginic acid, amino acids, anthocyanins and chain extender ethylenediamine are added, and the reaction is continued for 60 minutes. After aging, the spinning solution is obtained; finally, the spinning solution is transported to the spinning box through a metering pump for extrusion, the number of spinnerets is 65, and the filaments are solidified in a spinning channel filled with 260°C hot nitrogen, the gas flow rate is 0.5m / s, and the winding speed is 1200m / min, to obtain a bio-based spandex fiber with a fineness of 7D, a breaking strength of 1.95cN / detx, and a breaking elongation of 210%.

[0046] Example 9

[0047] A method for preparing bio-based spandex fiber, comprising the following steps: dissolving 4,4'-methylenebis(phenyl isocyanate) and bio-based poly 1,4-butanediol with a molecular weight of 1000 in an N,N-dimethylacetamide solution at a molar ratio of 1:1.8, and reacting at 80°C for 80 minutes to prepare a hydroxyl-terminated prepolymer solution A with a concentration of 20wt%; dissolving polyethylene glycol and 4,4'-methylenebis(phenyl isocyanate) in an N,N-dimethylacetamide solution at a molar ratio of 1:2, and reacting at 120°C for 120 minutes to prepare an isocyanate-terminated prepolymer solution B with a concentration of 35wt%; and mixing the prepolymer solutions A and B at a mass ratio of 1:9. and 3wt% of antioxidant 1135, nanoparticle silver, stabilizer 531, flame retardant melamine urate, and aluminum polyphosphate are reacted at 75°C for 60 minutes, and then 8wt% of natural products malic acid, alginate and chain extender ethylenediamine are added, and the reaction is continued for 60 minutes. After aging, the spinning solution is obtained; finally, the spinning solution is transported to the spinning box through a metering pump for extrusion, the number of spinnerets is 60, and the filaments are solidified in a spinning channel filled with 230°C hot air, the gas flow rate is 0.5m / s, and the winding speed is 600m / min, to obtain a bio-based spandex fiber with a fineness of 25D, a breaking strength of 1.5cN / detx, and a breaking elongation of 495%.

[0048] Example 10

[0049] A method for preparing bio-based spandex fiber comprises the following steps: dissolving 4,4'-diisocyanato-3,3'-dimethylbiphenyl and bio-based poly 1,4-butanediol with a molecular weight of 1000 in an N,N-dimethylacetamide solution at a molar ratio of 1:1.5, and reacting at 80°C for 80 minutes to prepare a hydroxyl-terminated prepolymer solution A with a concentration of 30wt%; dissolving polyethylene glycol and 4,4'-diisocyanato-3,3'-dimethylbiphenyl in an N,N-dimethylacetamide solution at a molar ratio of 1:1.8, and reacting at 120°C for 120 minutes to prepare an isocyanate-terminated prepolymer solution B with a concentration of 20wt%; and reacting the prepolymer solution A with B is prepared by reacting antioxidant 1010, nano-particle titanium dioxide, stabilizer 770 and flame retardant zinc borate at a ratio of 9:1 and 0.5wt% at 80°C for 40min, then adding 10wt% of natural products malic acid, alginic acid and chain extender diamine, and continuing the reaction for 30min. After aging, the spinning solution is obtained. Finally, the spinning solution is transported to the spinning box through a metering pump for extrusion, the number of spinnerets is 60, and the filaments are solidified in a spinning tunnel filled with 280°C hot nitrogen, the gas flow rate is 0.5m / s, and the winding speed is 800m / min, to obtain a bio-based spandex fiber with a fineness of 25D, a breaking strength of 2.1cN / detx, and a breaking elongation of 100%.

[0050] Comparative Example 1

[0051] A spandex fiber, the preparation method of which comprises the following steps: dissolving 4,4'-methylenebis(phenyl isocyanate) and polytetramethylene ether with a molecular weight of 1000 in an N,N-dimethylacetamide solution at a molar ratio of 1:1.5, reacting at 80°C for 80 minutes to prepare a hydroxyl-terminated prepolymer solution A with a concentration of 30wt%; dissolving polyethylene glycol and 4,4'-methylenebis(phenyl isocyanate) in an N,N-dimethylacetamide solution at a molar ratio of 1:1.5, reacting at 80°C for 80 minutes to prepare an isocyanate-terminated prepolymer solution with a concentration of 30wt% B; prepolymer solution A and B are reacted at a mass ratio of 1:9 and 1wt% of antioxidant 1010, nano diatomaceous earth particles, light stabilizer 770, flame retardant melamine urate and chain extender ethylenediamine at 60°C for 90 minutes. Finally, the spinning solution is transported to the spinning box through a metering pump for extrusion, the number of spinnerets is 60, and the filaments are solidified in a spinning tunnel filled with 230°C hot air, the gas flow rate is 0.1m / s, and the winding speed is 600m / min to obtain a spandex fiber with a fineness of 20D, a breaking strength of 1.1cN / detx, and a breaking elongation of 520%.

[0052] The biocompatibility of the spandex fibers prepared in Example 1 and Comparative Example 1 was tested, and the results were as follows: Figure 2 and 3 As shown, it can be clearly seen that after the cell culture, the comparative fiber has more red dead cells in its fluorescence microscope photo, while no dead cells are obviously observed in the fiber of Example 1, indicating that the fiber of Example 1 has excellent biocompatibility.

[0053] Biocompatibility test conditions: The sterilized fibers were cultured with HUVEC cells for 72 h, washed with PBS buffer, stained with staining solution, and then the cell morphology was observed under a fluorescence microscope.

[0054] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing bio-based spandex fiber, It is characterized in that Here are the steps: (1) dissolving diisocyanate I and bio-based polydiol in polar amine solution I, and then performing prepolymerization reaction I to prepare prepolymer solution A; (2) dissolving the polydiol and diisocyanate II in a polar amine solution II, and then performing a prepolymerization reaction II to obtain an isocyanate-terminated prepolymer solution B; (3) mixing prepolymer solutions A and B to react, then adding the natural product, continuing the reaction, and obtaining a spinning solution after aging; (4) Spinning the spinning solution to obtain bio-based spandex fibers.

2. The method for preparing the bio-based spandex fiber according to claim 1, It is characterized in that The diisocyanates I and II are independently selected from one of 4,4'-methylenebis(phenyl isocyanate), dicyclohexylmethane 4,4'-diisocyanate, toluene diisocyanate, and 4,4'-diisocyanato-3,3'-dimethylbiphenyl.

3. The method for preparing the bio-based spandex fiber according to claim 1, It is characterized in that In the step (1), the molar ratio of diisocyanate I to bio-based polydiol is 1: (1.5-1.8); the conditions of the prepolymerization reaction I are: temperature 80-100°C, time 80-120min, and a solution A with a prepolymer ratio of 20-35wt% is obtained.

4. The method for preparing the bio-based spandex fiber according to claim 1, It is characterized in that The molar ratio of the polyglycol to diisocyanate II in step (2) is 1:(1.8-2.5); the conditions of the prepolymerization reaction II are: temperature 80-100°C, time 80-120min, and a B solution with a prepolymer ratio of 20-35wt% is obtained.

5. The method for preparing the bio-based spandex fiber according to claim 1, It is characterized in that The polar amine solutions I and II are independently selected from N,N-dimethylformamide or N,N-dimethylacetamide; in the step (3), the mass ratio of the prepolymer solution A to B is (1:9)-(9:1), the temperature of the mixing reaction is 60-80°C, the time is 60-90 minutes, and after adding the natural product, the chain extension reaction is carried out for 30-60 minutes.

6. The method for preparing the bio-based spandex fiber according to claim 1, It is characterized in that The bio-based diol is polyether polyol, polylactic acid diol or polyhydroxyacetic acid diol, and the molecular weight of the bio-based diol is 1000-3000; the polyether polyol is prepared by using 1,3-propylene glycol, 1,5-pentanediol and 1,4-butanediol.

7. The method for preparing the bio-based spandex fiber according to claim 6, It is characterized in that The polyglycol is one of polycaprolactone glycol, polyethylene glycol, polycarbonate glycol and polytetramethylene glycol.

8. The method for preparing the bio-based spandex fiber according to claim 1, It is characterized in that The natural product is one or more of tea polyphenols, anthocyanidins, malic acid, amino acids, alginic acid and triterpenoid compounds, and the amount used is 1-10wt% of the total amount of prepolymer solutions A and B.

9. The method for preparing the bio-based spandex fiber according to any one of claims 1 to 8, It is characterized in that The spinning solution in step (3) is further added with an auxiliary agent, the amount of which is 0.1-3wt% of the total mass of the spinning solution; the auxiliary agent includes any one or more of antioxidants, nanoparticles, stabilizers, and flame retardants.

10. The bio-based spandex fiber prepared by the method according to any one of claims 1 to 9, It is characterized in that The bio-based spandex fiber has a fineness of 5-40D, a breaking strength of 1.5-2.1 cN / detx, and a breaking elongation of 100-600%.

Citation Information

Patent Citations

  • Bio-based spandex fiber and preparation method thereof

    CN115233331A

  • Melt-spun spandex slice with high elongation at break and high bio-based content as well as preparation and application of melt-spun spandex slice

    CN115926100A

  • Bio-based elastic spandex fiber and preparation method thereof

    CN117127276A

  • Process for producing polyurethane elastomer and elastic filament

    CN1261930A

  • Improved spandex compositions

    SG101789A1