Polyurethane elastomer with multiple dynamic hard segments and preparation method thereof
By designing polyurethane elastomers with multiple dynamic hard chain segments, the problems of damping and internal dissipation of polyurethane materials in vibration isolation applications are solved, and high tensile strength and stable damping effects are achieved, which enhances its construction materials application potential in the field.
Patent Information
- Application Number
- CN202411180562.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-03
AI Technical Summary
Polyurethane elastomers have problems with damping and internal disposal in vibration isolation materials, which limits their application range.
By designing polyurethane elastomers with multiple dynamic hard chain segments, a regular and tight structure is formed in alternating arrangements. The hard chain segment contains high-density urea-based hydrogen bonds, a large number of asymmetric alicycles and benzene rings, which improves the stretching rate and stretching of the material. The strength is maintained and the stable damping factor is maintained within the temperature range of -10~70℃ to enhance its vibration isolation and damping and vibration damping performance.
It achieves the high tensile ratio and tensile strength of polyurethane elastomer, while maintaining a stable damping effect over a wide temperature range, and has good water and oil resistance, which enhances its application potential in the field of building materials.
Smart Images

Figure CN119060302A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a polyurethane elastomer with multiple dynamic hard segments and a preparation method thereof, belonging to the technical field of polyurethane. The prepared polyurethane elastomer has excellent mechanical properties and damping properties, can play a stable damping and vibration isolation role in a wide temperature range, and has potential application prospects in the field of building materials. Background Art
[0002] Polyurethane is a polymer compound with many repeated carbamate groups on the polymer main chain. From the perspective of molecular structure, polyurethane elastomer is a block polymer, generally composed of soft segments of flexible long chains of oligomer polyols, and hard segments of diisocyanates and chain extenders. The soft segments and hard segments can produce microscopic phase separation, and a large number of hydrogen bonds can be formed within and between polyurethane molecules. These structural characteristics make polyurethane have excellent performance and are widely used in many fields such as industrial manufacturing, transportation and construction, oil and gas industry, and biomedicine.
[0003] In the field of vibration isolation materials, polyurethane materials have the advantages of good mechanical properties, light weight, small size, corrosion resistance, good vibration reduction effect, and excellent impact resistance compared to traditional rubber materials. However, the molecular structure of polyurethane elastomers determines that this type of material has large damping and internal friction heat generation, which limits its application as vibration isolation materials. Therefore, providing a polyurethane elastomer material with excellent mechanical properties and low internal friction has become a long-term technical demand of technicians in this field. Summary of the invention
[0004] In view of this, the purpose of the present invention is to provide a polyurethane elastomer with multiple dynamic hard segments and a preparation method thereof. Through structural design, the polyurethane hard segments form a regular and compact structure with alternating arrangement. At the same time, the hard segments contain high-density urea hydrogen bonds, a large number of asymmetric alicyclic rings and benzene rings, so that the elongation of the polyurethane elastomer material can reach 1400%-1600%, and the tensile strength can reach 35-42MPa. The damping factor is maintained at 0.12-0.18 in the temperature range of -10 to 70°C, and a stable damping effect can be exerted in the temperature range of -10 to 70°C. It can not only isolate vibration but also has a certain damping and vibration reduction effect. At the same time, it has certain water resistance and oil resistance, and has a good comprehensive effect in practical applications.
[0005] The objectives of the present invention are achieved through the following technical solutions.
[0006] A polyurethane elastomer with multiple dynamic hard segments, the structural formula of the polyurethane elastomer with multiple hard segments is:
[0007]
[0008] The value range of n is 24 to 28.
[0009] A method for preparing a polyurethane elastomer with multiple dynamic hard segments, wherein the raw materials for preparing the polyurethane elastomer include component A, component B, component C, and component D, and the amounts of component A, component B, and component C are added according to the molar mass ratio of isocyanate groups to amine groups;
[0010] Taking the total mass of component A as 100%, the components in component A and their mass fractions are as follows:
[0011] Toluene diisocyanate 14% to 16%;
[0012] Polypropylene glycol 84% to 86%;
[0013] Component B is isophorone diamine;
[0014] Component C is toluene diisocyanate;
[0015] Component D includes an organic solvent, 0.1 mol / L dilute hydrochloric acid, isopropanol, bromocresol blue indicator and a toluene solution of di-n-butylamine, wherein the organic solvent is any one of N,N-dimethylformamide, anhydrous ethanol and tetrahydrofuran;
[0016] The molecular weight of the polypropylene glycol is 1860-2080;
[0017] The steps of the method include:
[0018] In the first step, the toluene diisocyanate and polypropylene glycol in component A are dehydrated and then mixed, and nitrogen environment protection is performed during the mixing, and then the temperature is raised to 80°C ± 2°C, and stirred for reaction for 2-3 hours to obtain a polyurethane prepolymer, and the stirring speed is 180-220r / min;
[0019] The second step is to mix part of the polyurethane prepolymer obtained in the first step with isopropanol in a water bath environment at 45-55° C., with a mixing volume of L and a mixing time of 10-15 min, and then add a toluene solution of bromocresol blue indicator and di-n-butylamine, and then titrate with 0.1 mol / L dilute hydrochloric acid until the solution no longer changes color within 30 seconds, and then terminate the titration. After the titration, calculate the isocyanate content a in the polyurethane prepolymer, a=3.6-3.8wt%;
[0020] The third step is to mix the polyurethane prepolymer obtained in the first step, component C and an organic solvent in a water bath environment at 0-10°C, and stir under a nitrogen atmosphere to obtain a mixture A with a concentration of 0.3-0.4 g / ml, a stirring speed of 180-220 r / min, and a stirring time of 20-25 min;
[0021] The fourth step is to mix component B with an organic solvent to obtain a mixture B with a concentration of 0.1-0.2 g / ml, and then slowly add it to the mixture A in the third step using a constant pressure separatory funnel, the mixing temperature is 0-10°C, and the mixture is stirred under a nitrogen atmosphere to obtain a mixture C at a stirring speed of 180-220 r / min for 12 hours;
[0022] The fifth step is to heat the mixture C obtained in the fourth step to 83-87°C, react at a speed of 180-220r / min for 12-14h, pour it into a polytetrafluoroethylene mold, cure it in a blast drying oven at 80-85°C for 36-48h, and then dry it in a vacuum oven at 80-90°C for 24-36h to remove the organic solvent, thereby obtaining a polyurethane elastomer with multiple dynamic hard segments.
[0023] The ratio of the polyurethane prepolymer, toluene diisocyanate and isophorone diamine satisfies:
[0024] (m1×a) / 42+(m2 / 174)×2=R×(m3 / 170)×2
[0025] Wherein, m1 is the mass of polyurethane prepolymer, m2 is the mass of toluene diisocyanate (TDI), and m3 is the mass of isophorone diamine (IPDA);
[0026] The sum of the isocyanate groups in the polyurethane prepolymer and toluene diisocyanate is defined as R1, and the value of the amine group in isophorone diamine is defined as R2, then R=R1 / R2, and R=1-1.05.
[0027] Beneficial Effects
[0028] (1) The present invention forms a regular and compact structure of alternating arrangement of polyurethane hard segments through structural design. At the same time, the hard segments contain high-density urea hydrogen bonds, a large number of asymmetric alicyclic rings and benzene rings, so that the elongation of the polyurethane elastomer material can reach 1400%-1600%, and the tensile strength can reach 35-42MPa. The damping factor is maintained at 0.12-0.18 in the temperature range of -10 to 70°C, and a stable damping effect can be exerted in the temperature range of -10 to 70°C. It can not only isolate vibrations but also have a certain damping and vibration reduction effect, and at the same time has certain water resistance and oil resistance, and has a good comprehensive effect in practical applications. It can not only isolate vibrations but also have a certain damping and vibration reduction effect, and at the same time has certain water resistance and oil resistance, and has a good comprehensive effect in practical applications. A large number of urea bonds are introduced into the polymer chain, transforming the loosely arranged urethane / urea bond hard domains into tightly arranged urea bond hard domains; at the same time, due to the alternating copolymerization of isophorone diamine and toluene diisocyanate, the hard chain segments form a unique structure with high density of urea hydrogen bonds, a large number of asymmetric alicyclic rings and benzene rings, so the material exhibits excellent mechanical properties.
[0029] (2) The present invention provides a method for preparing a polyurethane elastomer with multiple dynamic hard segments. In the method, a prepared polyurethane matrix of component A is mixed with reactants of components B and C in an organic solvent, and the mixture is fully mixed by stirring. After that, the finished product is obtained by evaporating the solvent. The method has simple steps, and the experimental formula can be changed according to production needs, so that industrial production can be carried out.
[0030] (3) The present invention provides a method for preparing a polyurethane elastomer with multiple dynamic hard segments. The method uses a specific organic solvent (such as N,N-dimethylformamide) for the following purposes: first, to reduce the viscosity of the reaction system; second, to dissolve the prepolymer and small molecule components to allow the reaction to proceed more completely.
[0031] (4) The polyurethane elastomer of the present invention is a new type of high-performance polyurethane elastomer. Through the design of the hard segment, a large number of urea hydrogen bonds, asymmetric alicyclic rings and benzene rings are introduced, the hydrogen bond density is increased, and the hard domain structure is compact and regular, so that the polyurethane elastomer has good mechanical properties, damping properties, and water and oil resistance. The present invention also provides a method for preparing a polyurethane elastomer. The method has simple steps, is relatively safe and environmentally friendly, and the experimental formula can be changed according to production needs, and can be industrially produced. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 is the infrared spectrum of polyurethane elastomer, among which, 3353 (ν-NH-), 2871 / 2972 (ν-CH3), 1537 (ν-C7H6-), 1373 (δ-CH3), 1223 (ν(-CC-)s), 10920 (ν-COC-), 929 / 825 (δ-C7H6-);
[0033] Figure 2 It is the infrared peak diagram of 1600-1800 of polyurethane elastomer; among them, 1752 (νC=O, amide carbonyl), 1712 (νC=O, hydrogen-bonded amide carbonyl), 1680 (νC=O, urea carbonyl), 1625 (νC=O, hydrogen-bonded urea carbonyl);
[0034] Figure 3 It is the mechanical properties diagram of polyurethane elastomer;
[0035] Figure 4 This is the DMA result of polyurethane elastomer. DETAILED DESCRIPTION
[0036] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments, but this is not intended to limit the present invention.
[0037] Example 1
[0038] A method for preparing a polyurethane elastomer with multiple dynamic hard segments, the method comprising the steps of:
[0039] The first step is to add 3.49g of TDI to a 100ml three-necked flask, and add 20.1g of PPG2000 to a constant pressure dropping funnel and add dropwise, and the addition should be completed within 15 minutes. Since both of them have high reaction activity and obvious heat release, the addition temperature is maintained at 60℃~70℃, and an ice-water mixture is prepared on the side to prevent the reaction temperature from being too high. The entire reaction process requires continuous flow of dry N2. After the addition of PPG2000 is completed, increase the temperature of the oil bath to 80℃±2℃, and keep the entire reaction at the set temperature for 2 hours to obtain a polyurethane prepolymer;
[0040] The second step is to mix 0.4147 g of the polyurethane prepolymer obtained in the first step with 25 mL of isopropanol in a 50° C. water bath environment for 10 min, then add 4 drops of bromocresol blue indicator and 50 mL of di-n-butylamine toluene solution, and then titrate with 0.1 mol / L dilute hydrochloric acid until the solution no longer changes color within 30 s, and then terminate the titration. After the titration, the isocyanate content a in the polyurethane prepolymer is calculated to be 3.6 wt%;
[0041] In the third step, 7.36g of polyurethane prepolymer and 0.84g of TDI were dissolved in 20ml of dimethylformamide, added to a 100ml three-necked flask, stirred for 20min under a 0℃ N2 atmosphere at a stirring speed of 180-220r / min, and 1.36g of IPDA dissolved in 10mL of DMF was slowly added using a constant pressure dropping funnel, and the dropping time exceeded 10min. The mixture was stirred for 12h under a 0℃ N2 atmosphere at a stirring speed of 180-220r / min, and then heated to 85℃±2℃ for 12h. After cooling to room temperature, 3mL of ethanol was added to remove the residual toluene diisocyanate, and the reaction mixture was poured into a polytetrafluoroethylene (PTFE) mold, dried in a 90℃ oven for 48h, and then dried in a 90℃ vacuum oven for 12h to remove the solvent and bubbles to obtain a polyurethane elastomer.
[0042] The obtained elastomer was analyzed by infrared spectroscopy. Figure 1 As shown, Figure 2 Infrared peak separation is performed in the wavelength range of 1600-1800.
[0043] The obtained elastomer was subjected to a tensile test, and the results are as follows: Figure 3 As shown by Figure 3 It can be seen that polyurethane elastomers have excellent mechanical properties, with an elongation of up to 1600% and a tensile strength of up to 42 MPa.
[0044] The obtained polyurethane elastomer was subjected to DMA test, and the results are as follows: Figure 4 As shown, the damping factor of the polyurethane elastomer is maintained at 0.12-0.18 in the temperature range of -10 to 70°C, and it can play a stable damping role in the temperature range of -10 to 70°C. It can not only isolate vibration but also has a certain damping and vibration reduction effect, and has a good comprehensive effect.
[0045] The obtained polyurethane elastomer was immersed in water, seawater and edible oil respectively at room temperature (25°C) for 72 hours. The mass change rate of the polyurethane elastomer before and after immersion is shown in Table 1. According to Table 1, the prepared polyurethane has excellent medium resistance.
[0046] Table 1 Test results of media resistance of polyurethane elastomer
[0047] project Example 1 Example 2 Example 3 Water resistance (25℃, immersion for 72h), mass change rate (%) 3.90 3.45 4.11 Seawater resistance (25℃, immersion for 72h), mass change rate (%) 4.81 4.42 4.93 Oil resistance (25℃, immersion for 72h), mass change rate (%) 5.56 5.28 6.15
[0048] Example 2
[0049] A method for preparing a polyurethane elastomer with multiple dynamic hard segments, the method comprising the steps of:
[0050] In the first step, add 3.52g of TDI to a 100ml three-necked flask, add 19.9g of PPG2000 to a constant pressure dropping funnel and add dropwise, and complete the addition within 15 minutes. Since both have high reaction activity and obvious heat release, the dropping temperature is maintained at 60℃~70℃, and an ice-water mixture is prepared on the side to prevent the reaction temperature from being too high. The entire reaction process requires continuous flow of dry N2. After the addition of PPG2000 is completed, increase the temperature of the oil bath to 80℃±2℃, and keep the entire reaction at the set temperature for about 2 hours to obtain a polyurethane prepolymer;
[0051] The second step is to mix 0.4231 g of the polyurethane prepolymer obtained in the first step with 25 mL of isopropanol in a 50° C. water bath environment for 10 min, then add 4 drops of bromocresol blue indicator and 50 mL of a toluene solution of di-n-butylamine, and then titrate with 0.1 mol / L dilute hydrochloric acid until the solution no longer changes color within 30 s, and then terminate the titration. After the titration, the isocyanate content a in the polyurethane prepolymer is calculated to be 3.6 wt%;
[0052] In the third step, 7.42g of polyurethane prepolymer and 0.85g of TDI were dissolved in 20ml of dimethylformamide (DMF), added to a 100ml three-necked flask, stirred for 20min under a 0℃ N2 atmosphere at a stirring speed of 180-220r / min, and 1.37g of IPDA dissolved in 10mL of DMF was slowly added using a constant pressure dropping funnel, and the dropping time exceeded 10min. The mixture was stirred for 12h under a 0℃ N2 atmosphere at a stirring speed of 180-220r / min, and then heated to 85℃±2℃ for 12h. After cooling to room temperature, 3mL of ethanol was added to remove residual isocyanate, and the reaction mixture was poured into a polytetrafluoroethylene (PTFE) mold, dried in a 90℃ oven for 48h, and then dried in a 90℃ vacuum oven for 12h to remove solvents and bubbles to obtain a polyurethane elastomer.
[0053] The obtained polyurethane elastomer was immersed in water, seawater and oil respectively at room temperature (25°C) for 72 hours. The mass change rate of the polyurethane elastomer before and after immersion is shown in Table 1. According to Table 1, the prepared polyurethane has excellent medium resistance.
[0054] Example 3
[0055] A method for preparing a polyurethane elastomer with multiple dynamic hard segments, the method comprising the steps of:
[0056] In the first step, add 3.48g of TDI to a 100ml three-necked flask, add 20.2g of PPG2000 to a constant pressure dropping funnel and add dropwise, and complete the addition within 15 minutes. Since both have high reaction activity and obvious heat release, the dropping temperature is maintained at 60℃~70℃, and an ice-water mixture is prepared on the side to prevent the reaction temperature from being too high. The entire reaction process requires continuous flow of dry N2. After the addition of PPG2000 is completed, increase the temperature of the oil bath to 80℃±2℃, and keep the entire reaction at the set temperature for about 2 hours to obtain a polyurethane prepolymer;
[0057] The second step is to mix 0.4157 g of the polyurethane prepolymer obtained in the first step with 25 mL of isopropanol in a 50° C. water bath environment for 10 min, then add 4 drops of bromocresol blue indicator and 50 mL of di-n-butylamine toluene solution, and then titrate with 0.1 mol / L dilute hydrochloric acid until the solution no longer changes color within 30 s, and then terminate the titration. After the titration, the isocyanate content a in the polyurethane prepolymer is calculated to be 3.7 wt%;
[0058] In the third step, 7.38g of polyurethane prepolymer and 0.83g of TDI were dissolved in 20ml of dimethylformamide (DMF), added to a 100ml three-necked flask, stirred for 20min under a 0℃ N2 atmosphere at a stirring speed of 180-220r / min, and 1.36g of IPDA dissolved in 10mL of DMF was slowly added using a constant pressure dropping funnel, and the dropping time exceeded 10min. The mixture was stirred for 12h under a 0℃ N2 atmosphere at a stirring speed of 180-220r / min, and then heated to 85℃±2℃ for 12h. After cooling to room temperature, 3mL of ethanol was added to remove residual isocyanate, and the reaction mixture was poured into a polytetrafluoroethylene (PTFE) mold, dried in a 90℃ oven for 48h, and then dried in a 90℃ vacuum oven for 12h to remove solvents and bubbles to obtain a polyurethane elastomer.
[0059] The obtained polyurethane elastomer was immersed in water, seawater and oil respectively at room temperature (25°C) for 72 hours. The mass change rate of the polyurethane elastomer before and after immersion is shown in Table 1. According to Table 1, the prepared polyurethane has excellent medium resistance.
[0060] Example 4
[0061] A method for preparing a polyurethane elastomer with multiple dynamic hard segments, the method comprising the steps of:
[0062] In the first step, add 3.51g of TDI to a 100ml three-necked flask, add 20.1g of PPG2000 to a constant pressure dropping funnel and add dropwise, and complete the addition within 15 minutes. Since both have high reaction activity and obvious heat release, the dropping temperature is maintained at 60℃~70℃, and an ice-water mixture is prepared on the side to prevent the reaction temperature from being too high. The entire reaction process requires continuous flow of dry N2. After the addition of PPG2000 is completed, increase the temperature of the oil bath to 80℃±2℃, and keep the entire reaction at the set temperature for about 2 hours to obtain a polyurethane prepolymer;
[0063] The second step is to mix 0.4156 g of the polyurethane prepolymer obtained in the first step with 25 mL of isopropanol in a 50° C. water bath environment for 10 min, then add 4 drops of bromocresol blue indicator and 50 mL of di-n-butylamine toluene solution, and then titrate with 0.1 mol / L dilute hydrochloric acid until the solution no longer changes color within 30 s, and then terminate the titration. After the titration, the isocyanate content a in the polyurethane prepolymer is calculated to be 3.6 wt%;
[0064] In the third step, 7.37g of polyurethane prepolymer and 0.84g of TDI were dissolved in 20ml of dimethylformamide (DMF), added to a 100ml three-necked flask, stirred for 20min under a 0℃ N2 atmosphere at a stirring speed of 180-220r / min, and 1.35g of IPDA dissolved in 10mL of DMF was slowly added using a constant pressure dropping funnel, and the dropping time exceeded 10min. The mixture was stirred for 12h under a 0℃ N2 atmosphere at a stirring speed of 180-220r / min, and then heated to 85℃±2℃ for 12h. After cooling to room temperature, 3mL of ethanol was added to remove residual isocyanate, and the reaction mixture was poured into a polytetrafluoroethylene (PTFE) mold, dried in a 90℃ oven for 48h, and then dried in a 90℃ vacuum oven for 12h to remove solvents and bubbles to obtain a polyurethane elastomer.
[0065] Example 5
[0066] A method for preparing a polyurethane elastomer with multiple dynamic hard segments, the method comprising the steps of:
[0067] In the first step, add 3.53g of TDI to a 100ml three-necked flask, add 19.9g of PPG2000 to a constant pressure dropping funnel and add dropwise, and complete the addition within 15 minutes. Since both have high reaction activity and obvious heat release, the dropping temperature is maintained at 60℃~70℃, and an ice-water mixture is prepared on the side to prevent the reaction temperature from being too high. The entire reaction process requires continuous flow of dry N2. After the addition of PPG2000 is completed, increase the temperature of the oil bath to 80℃±2℃, and keep the entire reaction at the set temperature for about 2 hours to obtain a polyurethane prepolymer;
[0068] The second step is to mix 0.4152 g of the polyurethane prepolymer obtained in the first step with 25 mL of isopropanol in a 50° C. water bath environment for 10 min, then add 4 drops of bromocresol blue indicator and 50 mL of di-n-butylamine toluene solution, and then titrate with 0.1 mol / L dilute hydrochloric acid until the solution no longer changes color within 30 s, and then terminate the titration. After the titration, the isocyanate content a in the polyurethane prepolymer is calculated to be 3.7 wt%;
[0069] In the third step, 7.42g of polyurethane prepolymer and 0.85g of TDI were dissolved in 20ml of dimethylformamide (DMF), added to a 100ml three-necked flask, stirred for 20min under a 0℃ N2 atmosphere at a stirring speed of 180-220r / min, and 1.38g of IPDA dissolved in 10mL of DMF was slowly added using a constant pressure dropping funnel, and the dropping time exceeded 10min. The mixture was stirred for 12h under a 0℃ N2 atmosphere at a stirring speed of 180-220r / min, and then heated to 85℃±2℃ for 12h. After cooling to room temperature, 3mL of ethanol was added to remove residual isocyanate, and the reaction mixture was poured into a polytetrafluoroethylene (PTFE) mold, dried in a 90℃ oven for 48h, and then dried in a 90℃ vacuum oven for 12h to remove solvents and bubbles to obtain a polyurethane elastomer.
[0070] In summary, the above are only preferred embodiments of the present invention and are not intended to limit the protection scope of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A polyurethane elastomer with multiple dynamic hard segments, characterized in that: The structural formula of the polyurethane elastomer with multiple hard segments is: The value range of n is 24 to 28.
2. The polyurethane elastomer with multiple dynamic hard segments according to claim 1, characterized in that: The raw materials for preparing the polyurethane elastomer include component A, component B, component C and component D; Taking the total mass of component A as 100%, the components in component A and their mass fractions are as follows: Toluene diisocyanate 14% to 16%; Polypropylene glycol 84% to 86%; Component B is isophorone diamine; Component C is toluene diisocyanate; Component D includes an organic solvent, 0.1 mol / L dilute hydrochloric acid, isopropanol, bromocresol blue indicator and a toluene solution of di-n-butylamine, wherein the organic solvent is any one of N,N-dimethylformamide, anhydrous ethanol and tetrahydrofuran; The molecular weight of the polypropylene glycol is 1860-2080.
3. A method for preparing a polyurethane elastomer with multiple dynamic hard segments, characterized in that The steps of the method include: In the first step, toluene diisocyanate and polypropylene glycol in component A are dehydrated and then mixed, nitrogen environment protection is performed during the mixing, and then the temperature is increased and stirred to obtain a polyurethane prepolymer; The second step is to mix part of the polyurethane prepolymer obtained in the first step with isopropanol in a water bath environment, the mixed volume is L, and then add bromocresol blue indicator and di-n-butylamine toluene solution, and then use 0.1 mol / L dilute hydrochloric acid to titrate until the solution no longer changes color within 30 seconds, and then end the titration. After the titration, calculate the isocyanate content a in the polyurethane prepolymer, a=3.6-3.8wt%; The third step is to mix the polyurethane prepolymer obtained in the first step, component C and an organic solvent in a water bath environment, and stir them under a nitrogen atmosphere to obtain a mixture A; Step 4: Mix component B with an organic solvent to obtain a mixture B, wherein the concentration of the mixture B is 0.1-0.2 g / ml, and then slowly add the mixture into the mixture A in the third step using a constant pressure separatory funnel, and stir under a nitrogen atmosphere to obtain a mixture C; The fifth step is to heat the mixture C obtained in the fourth step to 83-87°C, stir, pour into a polytetrafluoroethylene mold, cure in a blast drying oven at 80-85°C for 36-48h, and then dry in a vacuum oven at 80-90°C for 24-36h to remove the organic solvent to obtain a polyurethane elastomer with multiple dynamic hard segments.
4. The method for preparing a polyurethane elastomer with multiple dynamic hard segments according to claim 3, characterized in that: The ratio of the polyurethane prepolymer, toluene diisocyanate and isophorone diamine satisfies: (m1×a) / 42+(m2 / 174)×2=R×(m3 / 170)×2 Wherein, m1 is the mass of polyurethane prepolymer, m2 is the mass of toluene diisocyanate (TDI), and m3 is the mass of isophorone diamine (IPDA); The sum of the isocyanate groups in the polyurethane prepolymer and toluene diisocyanate is defined as R1, and the value of the amine group in isophorone diamine is defined as R2, then R=R1 / R2, and R=1 to 1.
05.
5. The method for preparing a polyurethane elastomer with multiple dynamic hard segments according to claim 3, characterized in that: In the first step, the temperature is raised to 78-82° C., the stirring reaction time is 2-3 hours, and the stirring speed is 180-220 r / min.
6. The method for preparing a polyurethane elastomer with multiple dynamic hard segments according to claim 3, characterized in that: In the second step, the polyurethane prepolymer and isopropyl alcohol are mixed in a water bath at 45-55° C. for 10-15 minutes.
7. The method for preparing a polyurethane elastomer with multiple dynamic hard segments according to claim 3, characterized in that: In the third step, the polyurethane prepolymer, component C and organic solvent are mixed in a water bath environment at 0-10° C., the concentration of the mixture A is 0.3-0.4 g / ml, the stirring speed is 180-220 r / min, and the stirring time is 20-25 min.
8. The method for preparing a polyurethane elastomer with multiple dynamic hard segments according to claim 3, characterized in that: In the fourth step, the concentration of the mixture B is 0.1-0.2 g / ml, the mixing temperature is 0-10° C., the stirring speed is 180-220 r / min, and the stirring time is 12 h.
9. The method for preparing a polyurethane elastomer with multiple dynamic hard segments according to claim 3, characterized in that: In the fifth step, the stirring speed is 180-220 r / min, and the stirring time is 12-14 h.
Citation Information
Patent Citations
Amino compound modified polyurethane elastomer and preparation method thereof
CN118325031A
Polyurethane elastomer with high ultimate elongation
WO2019209348A1