Cross-linked polymer and preparation method thereof, electrolyte composition, polymer electrolyte and preparation method thereof, lithium ion battery and electric equipment

By using crosslinked polymers with hydrogen bond and covalent bond composite structures in lithium-ion batteries, the problem of taking into account both the mechanical properties and ionic conductivity of the polymer electrolyte of lithium-ion batteries is solved, and the improvement of high mechanical properties and electrochemical properties is achieved. Enhanced battery safety.

CN119060331AActive Publication Date: 2024-12-03BYD CO LTD

Patent Information

Application Number
CN202310640323.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-31
Publication Date
2024-12-03
Estimated Expiration
2043-05-31

AI Technical Summary

Technical Problem

The mechanical properties and ionic conductivity of existing lithium-ion batteries cannot be achieved with both the mechanical properties and the ionic conductivity, and there are safety hazards for leakage and explosion of liquid electrolytes.

Method used

Using crosslinked polymers with hydrogen bond and covalent bond composite structures, the hardness and toughness of polymer electrolytes are improved through the crosslinked structure of covalent bond and hydrogen bond, and the reversibility of hydrogen bonds is provided to enhance the mechanical properties of the electrolytes. and ionic conductivity.

Benefits of technology

It has achieved polymer electrolytes with high mechanical strength, high toughness, high elasticity, high ionic conductivity and good thermal stability, and enhanced the safety and electrochemical performance of lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060331A_ABST
    Figure CN119060331A_ABST
Patent Text Reader

Abstract

The invention relates to the field of lithium ion batteries, and discloses a cross-linked polymer which is characterized by comprising a macromolecular chain A from a compound a as shown in a formula (1), a cross-linked structure B from a compound b as shown in a formula (2), and a linking group-NH-connecting the macromolecular chain A and the cross-linked structure B, wherein the macromolecular chain A comprises a polyether flexible chain segment; the cross-linked polymer has a composite structure of a hydrogen bond and a covalent bond, the covalent bond is-CN-, and the hydrogen bond is formed by complexing a hydrogen atom of an amino group in a compound b and a double bond oxygen atom on a nitrogen-containing heterocyclic ring in a compound a; in the imgabs0 #, R1 and R2 are respectively and independently H, a C1-C6 straight chain alkyl group or a C3-C6 branched chain alkyl group; m is an integer from 1 to 100, and n is an integer from 1 to 100; the polymer electrolyte provided by the invention has the advantages of high mechanical strength, high toughness, high elasticity, high ionic conductivity, good thermal stability and high interface stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a cross-linked polymer and a preparation method thereof, an electrolyte composition, a polymer electrolyte and a preparation method thereof, a lithium ion battery and electrical equipment. Background Art

[0002] Lithium-ion batteries are ideal power sources for various electronic products and ideal light-weight, high-energy power sources for future electric vehicles due to their high operating voltage, high specific energy, no memory effect, long cycle life, and low self-discharge rate. Currently, commercial lithium-ion batteries have safety hazards such as poor affinity of the diaphragm to the electrolyte and leakage and explosion of the liquid electrolyte. Therefore, enhancing the affinity of the diaphragm and the electrolyte is one of the current research hotspots. Polymer electrolytes achieve the integration of diaphragms and electrolytes, which effectively avoids the occurrence of this problem. At the same time, polymer electrolytes have strong plasticity, which is convenient for battery shape design and assembly. It can meet the development requirements of miniaturization, thinness, and lightweight of electronic products.

[0003] Current research and technology mainly focus on improving the ionic conductivity of lithium batteries by changing the structure of polymers. Existing research uses grafted polymers with a main chain of polymethacrylate (MMA) and side chains of polyether segments (PEO) of different chain lengths. It is found that the ionic conductivity can be increased to 10 -4 -10 -5 S / cm. MMA monomer acts as an internal plasticizer, improving the flexibility of the chain and the movement of the free chain segments in the amorphous region of the polyether, increasing the distance between the PEO chains, and facilitating the migration of lithium ions. However, the improvement of ionic conductivity is achieved by reducing the crystallinity of the polymer by lowering the glass transition temperature (Tg) of the polymer, which inevitably reduces the mechanical properties of the polymer electrolyte.

[0004] The existing problem of polymer electrolyte technology is that mechanical properties and ionic conductivity cannot be achieved at the same time. Even if some solid polymer electrolytes achieve ideal mechanical strength, their ionic conductivity is only 10 -5 S / cm. In order to improve the ionic conductivity, small molecule additives and electrolytes are usually added to polymer electrolytes. However, this will cause deformation and breakage of solid polymer electrolytes. Therefore, new technologies are needed to prepare electrolyte materials with both strong mechanical strength and high ionic conductivity. Summary of the invention

[0005] The purpose of the present invention is to overcome the problems of low mechanical properties and ionic conductivity of polymer electrolytes in the prior art, and to provide a cross-linked polymer and a preparation method, an electrolyte composition, a polymer electrolyte and a preparation method, a lithium ion battery and electrical equipment.

[0006] In order to achieve the above object, the first aspect of the present invention provides a cross-linked polymer, wherein the cross-linked polymer comprises: a macromolecular chain A derived from a compound a represented by formula (1), a cross-linked structure B derived from a compound b represented by formula (2), and a connecting group -NH- connecting the macromolecular chain A and the cross-linked structure B;

[0007] Wherein, the macromolecular chain A comprises a polyether flexible segment;

[0008] The cross-linked polymer has a composite structure of hydrogen bonds and covalent bonds, wherein the covalent bond is -CN-, and the hydrogen bond is formed by the complexation of the hydrogen atom of the amino group in compound b and the double-bonded oxygen atom on the nitrogen-containing heterocyclic ring in compound a;

[0009]

[0010] Wherein, R1 and R2 are each independently H, C1-C6 straight chain alkyl or C3-C6 branched chain alkyl; m is an integer of 1-100, and n is an integer of 1-100.

[0011] The second aspect of the present invention provides a method for preparing a cross-linked polymer, wherein the preparation method comprises: subjecting a compound a represented by formula (1) and a compound b represented by formula (2) to a cross-linking reaction to obtain the cross-linked polymer; wherein the terminal group -OH in the compound a is bonded with the terminal group -NH2 in the compound b to form a connecting group -NH-; the hydrogen atom of the amino group in the compound b is complexed with the double-bonded oxygen atom on the nitrogen-containing heterocyclic ring in the compound a;

[0012]

[0013] Wherein, R1 and R2 are each independently H, C1-C6 straight chain alkyl or C3-C6 branched chain alkyl; m is an integer of 1-100, and n is an integer of 1-100.

[0014] The third aspect of the present invention provides a cross-linked polymer obtained by the preparation method.

[0015] The fourth aspect of the present invention provides a polymer electrolyte raw material composition, which includes a lithium salt, a filler, a plasticizer and the cross-linked polymer.

[0016] A fifth aspect of the present invention provides a method for preparing a polymer electrolyte, wherein the preparation method comprises:

[0017] (1) reacting the filler and the cross-linked polymer to form a film to obtain a film-forming substance;

[0018] (2) The film-forming substance is mixed with a lithium salt solution and a plasticizer to obtain the polymer electrolyte.

[0019] A sixth aspect of the present invention provides a polymer electrolyte obtained by the preparation method.

[0020] A seventh aspect of the present invention provides a lithium ion battery, wherein the polymer lithium ion battery comprises the polymer electrolyte.

[0021] An eighth aspect of the present invention provides an electrical device comprising the lithium-ion battery.

[0022] Through the above technical scheme, the structure of the cross-linked polymer provided by the present invention is different from that of the traditional polymer in that hydrogen bonds and covalent bonds coexist to form a cross-linked polymer structure. The polymer is a cross-linked structure, and this cross-linked structure is formed by covalent bonds and hydrogen bonds, wherein the covalent bonds are -CN-, and the hydrogen bonds are formed by the complexation of hydrogen atoms and oxygen atoms. The characteristics of the cross-linked polymer are: the cross-linked structure is formed by covalent bonds and hydrogen bonds between the segments, and during the application of external force (lithium ion reaction process), the covalent bonds do not break, and the hydrogen bonds disappear; after the external force disappears, the covalent bonds remain stable and the hydrogen bonds recover. The presence of covalent bonds can improve and ensure the hardness and toughness of the polymer electrolyte, so that it can resist the lithium dendrites formed by the lithium metal negative electrode of the lithium ion battery, and prevent the lithium dendrites from penetrating the polymer electrolyte to cause internal short circuits; at the same time, the presence of reversible hydrogen bonds can provide elasticity for the cross-linked polymer, and the hydrogen bonds dissipate external forces without sacrificing the hardness and toughness provided by the covalent bonds, preventing the cross-linked polymer from breaking, and after the external force is removed, the hydrogen bonds recover, and the deformation recovers accordingly, which can resist the changes in the volume of the positive and negative electrode materials during the charging and discharging process of the lithium ion battery. The structure of the cross-linked polymer is conducive to improving the mechanical properties of the polymer electrolyte, overcoming the disadvantage of low mechanical strength of the polymer electrolyte in the prior art, and providing a polymer electrolyte with high mechanical strength, high toughness, high elasticity, high ionic conductivity, good thermal stability, high interface stability, simple preparation conditions, and easy industrialization, as well as a preparation method thereof and a lithium ion battery including the polymer electrolyte. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 is a schematic diagram of the structure of the reaction product of pyrrolopyrrole diketone polyether and bisthiopheneethylenetriamine;

[0024] Figure 2 is the thermogravimetric analysis curve of polymer electrolyte S1;

[0025] Figure 3 is the differential thermal analysis diagram of polymer electrolyte S1 and polyethylene oxide;

[0026] Figure 4 is the stress-strain curve of polymer electrolyte S1;

[0027] Figure 5 is the strain-time curve of polymer electrolyte S1;

[0028] Figure 6 is the SEM image of polymer electrolyte S1;

[0029] Figure 7 is the SEM image of the composite positive electrode C1;

[0030] Figure 8 is the electrochemical impedance spectrum of polymer electrolyte S1;

[0031] Fig. 9 is the ionic conductivity of polymer electrolyte S1;

[0032] Fig.10 is the cyclic voltammetry curve of polymer electrolyte S1. DETAILED DESCRIPTION

[0033] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0034] The first aspect of the present invention provides a cross-linked polymer, wherein the cross-linked polymer comprises: a macromolecular chain A derived from a compound a represented by formula (1), a cross-linked structure B derived from a compound b represented by formula (2), and a connecting group -NH- connecting the macromolecular chain A and the cross-linked structure B;

[0035] Wherein, the macromolecular chain A comprises a polyether flexible segment;

[0036] The cross-linked polymer has a composite structure of hydrogen bonds and covalent bonds, wherein the covalent bond is -CN-, and the hydrogen bond is formed by the complexation of the hydrogen atom of the amino group in compound b and the double-bonded oxygen atom on the nitrogen-containing heterocyclic ring in compound a;

[0037]

[0038] Wherein, R1 and R2 are each independently H, C1-C6 straight chain alkyl or C3-C6 branched chain alkyl; m is an integer of 1-100, and n is an integer of 1-100.

[0039] In the present invention, if Figure 1The schematic diagram of the compound structure shown in the figure shows that the hydroxyl group on the thiophene heterocycle in compound a is condensed with the amino group on the thiophene heterocycle in compound b to obtain a connecting group -NH-, wherein the macromolecular chain A is the part of compound a without the hydroxyl group on the thiophene heterocycle, and the cross-linked structure B is the part of compound b without the amino group on the thiophene heterocycle. Each compound b contains three amino groups, which can react with the hydroxyl groups on the thiophene heterocycles in three compounds a respectively. Each compound a has two hydroxyl groups. The hydroxyl groups on the remaining thiophene heterocycle in the cross-linked compound a can also be condensed with the amino groups on the thiophene heterocycles in other compounds b. The cross-linking and condensation are repeated to form a large cross-linked polymer. Among them, the condensation obtains the connecting group -NH- to form a covalent bonding site, the N atom can form the covalent bond with the C atom on the thiophene heterocycle in compound a as -CN-, the N atom can also form the covalent bond with the C atom on the thiophene heterocycle in compound b as -CN-, the hydrogen atom on the N atom can form a hydrogen bond with the double bonded oxygen atom on the pyrrolopyrrole heterocycle in the adjacent compound a segment, and the hydrogen atom on the N atom can also form a hydrogen bond with the double bonded oxygen atom on the pyrrolopyrrole heterocycle in the non-adjacent compound a segment.

[0040] In the present invention, the structure of the cross-linked polymer is different from that of the traditional polymer in that hydrogen bonds and covalent bonds coexist to form the cross-linked polymer, and the cross-linked polymer has a composite structure of hydrogen bonds and covalent bonds, wherein the covalent bond is -CN-, and the hydrogen bond is formed by the complexation of hydrogen atoms and oxygen atoms. The characteristics of the cross-linked polymer are: the segments form a cross-linked structure through covalent bonds and hydrogen bonds, and during the application of external force (lithium ion reaction process), the covalent bonds do not break and the hydrogen bonds disappear; after the external force disappears, the covalent bonds remain stable and the hydrogen bonds recover. The presence of covalent bonds can improve and ensure the hardness and toughness of the polymer electrolyte, so that it can resist the lithium dendrites formed by the lithium metal negative electrode of the lithium ion battery, and prevent the lithium dendrites from penetrating the polymer electrolyte to cause internal short circuits; at the same time, the presence of reversible hydrogen bonds can provide elasticity for the cross-linked polymer, and the hydrogen bonds dissipate external forces without sacrificing the hardness and toughness provided by the covalent bonds, preventing the cross-linked polymer from breaking, and after the external force is removed, the hydrogen bonds recover, and the deformation recovers accordingly, which can resist the changes in the volume of the positive and negative electrode materials during the charging and discharging process of the lithium ion battery.

[0041] In the present invention, the cross-linked polymer has a composite structure of hydrogen bonds and covalent bonds. First, the hydrogen bonds can be dissipated under the action of applied pressure to respond to strain without breaking the covalent bonds to cause permanent deformation of the material. After the external pressure disappears, the hydrogen bonds are reformed and the shape of the material is restored, which is beneficial to improving the mechanical properties of the polymer electrolyte. Second, the hydrogen bonds are independent of the glass transition temperature. Lowering the glass transition temperature of the polymer can improve the ionic conductivity without affecting the structure of the cross-linked polymer. Therefore, it does not affect the improvement of the mechanical properties brought by the cross-linked polymer, and the ionic conductivity can be maintained at a high level while improving the mechanical properties of the polymer electrolyte.

[0042] In the present invention, the cross-linked polymer contains ether oxygen functional groups capable of complexing lithium ions, which are polyether segments contained in formula (1). The polyether can provide a sufficiently high electron-donating group density and has a flexible polyether segment, wherein m and n are repeating units of the flexible segment, wherein m is 1-100 and n is 1-100. Preferably, when m is 3-60 and n is 3-60, the obtained cross-linked polymer is beneficial to improving the mechanical properties of the polymer electrolyte, and obtaining a polymer electrolyte with high mechanical strength, high toughness, high elasticity, high ionic conductivity, good thermal stability and high interface stability.

[0043] In some specific embodiments of the present invention, in the polymer, the molar ratio of the macromolecular chain A: the cross-linked structure B is 1-10:1, preferably 3-5:1.

[0044] In some specific embodiments of the present invention, the weight average molecular weight of the polymer is 600,000-2,000,000 g / mol, which can make the room temperature ionic conductivity and migration number of lithium ions in the polymer electrolyte reach a high level.

[0045] The second aspect of the present invention provides a method for preparing a cross-linked polymer, wherein the preparation method comprises: subjecting a compound a represented by formula (1) and a compound b represented by formula (2) to a cross-linking reaction to obtain the cross-linked polymer; wherein the terminal group -OH in the compound a is bonded with the terminal group -NH2 in the compound b to form a connecting group -NH-; the hydrogen atom of the amino group in the compound b is complexed with the double-bonded oxygen atom on the nitrogen-containing heterocyclic ring in the compound a;

[0046]

[0047] Wherein, R1 and R2 are each independently H, C1-C6 straight chain alkyl or C3-C6 branched chain alkyl; m is an integer of 1-100, and n is an integer of 1-100.

[0048] In some specific embodiments of the present invention, the cross-linking reaction temperature is 100-150°C, preferably 120°C.

[0049] In some specific embodiments of the present invention, the cross-linking reaction time is 10-20 min, preferably 15 min.

[0050] In some specific embodiments of the present invention, the reaction is carried out in a solvent, and the solvent is chlorobenzene.

[0051] In some specific embodiments of the present invention, the molar ratio of compound a:compound b is 1-10:1, preferably 3-5:1.

[0052] In some specific embodiments of the present invention, the terminal group -OH in the compound a undergoes a condensation reaction with the terminal group -NH2 in the compound b to form a connecting group -NH-, and the connecting group -NH- is obtained by condensing the hydroxyl group on the thiophene heterocycle in the compound a with the amino group on the thiophene heterocycle in the compound b to form a covalent bond connection; the hydrogen atom of the amino group in the compound b is complexed with the double-bonded oxygen atom on the nitrogen-containing heterocycle in the compound a to form a hydrogen bond connection.

[0053] In the present invention, the composition and structure of the cross-linked polymer can be determined by NMR, IR, GPC, elemental analysis, etc., or by preparing and feeding.

[0054] The third aspect of the present invention provides a cross-linked polymer obtained by the preparation method.

[0055] The fourth aspect of the present invention provides a polymer electrolyte raw material composition, which includes a lithium salt, a filler, a plasticizer and the cross-linked polymer.

[0056] In addition to the cross-linked polymer and lithium salt, the polymer electrolyte provided by the present invention may also contain other dopants disclosed in the art for improving performance, such as adding SiO2 nanoparticles and small molecule liquid plasticizers to reduce the crystalline region content of the polymer matrix to improve ionic conductivity.

[0057] In some specific embodiments of the present invention, the lithium salt is selected from one or more of lithium bis(trifluoromethylsulfonyl)imide, lithium hexafluorophosphate, lithium perchlorate, lithium tetrafluoroborate, lithium hexafluoroarsenate, lithium hexafluorosilicate, lithium tetraphenylborate, lithium chloride, lithium bromide, lithium chloroaluminate, lithium fluoroalkylsulfonate, LiCH3SO3, LiN(SO2CF3)2, LiN(SO2C2F5)2; preferably selected from lithium bis(trifluoromethylsulfonyl)imide.

[0058] In some specific embodiments of the present invention, the filler is selected from one or more of TiO2, Al2O3, SiO2, MgO, ZrO2, LiNbO3, BaTiO3, PbTiO3, montmorillonite, and molecular sieves.

[0059] In some specific embodiments of the present invention, the plasticizer is selected from one or more of ethylene carbonate, propylene carbonate and vinylene carbonate.

[0060] In some specific embodiments of the present invention, the cross-linked polymer is 25-50 parts by weight, the lithium salt is 20-40 parts by weight, the filler is 1-4 parts by weight, and the plasticizer is 20-40 parts by weight.

[0061] The ratio of the number of oxygen atoms contained in the cross-linked polymer to the number of lithium ions in the lithium salt in the polymer electrolyte provided by the present invention ranges from 6 to 40:1. In order to maximize the ionic conductivity, 10:1 and 8:1 are preferred.

[0062] A fifth aspect of the present invention provides a method for preparing a polymer electrolyte, wherein the preparation method comprises:

[0063] (1) reacting the filler and the cross-linked polymer to form a film to obtain a film-forming substance;

[0064] (2) The film-forming substance is mixed with a lithium salt solution and a plasticizer to obtain the polymer electrolyte.

[0065] In some specific embodiments of the present invention, the preparation method comprises:

[0066] (1) reacting the cross-linked polymer and silicon dioxide to form a film to obtain a film-forming substance;

[0067] (2) adding the obtained film-forming substance to a lithium salt solution, adsorbing and drying to form a film, adding propylene carbonate, swelling and forming a film to obtain the polymer electrolyte.

[0068] A sixth aspect of the present invention provides a polymer electrolyte obtained by the preparation method.

[0069] In some specific embodiments of the present invention, the ionic conductivity of the polymer electrolyte is 0.48-5.5S / cm, the electrochemical impedance is 470-540Ω, the elongation at break is 115-129%, the tensile strength is 0.33-0.51MPa, and the strain recovery rate is 63.4-82.3%. The polymer electrolyte has good elongation at break and tensile strength, so it is also called an elastic polymer electrolyte, and the cross-linked polymer is the elastic polymer matrix of the elastic polymer electrolyte.

[0070] In some specific embodiments of the present invention, the thickness of the polymer electrolyte is 100-500 μm, and the thickness of the polymer electrolyte is further optimized to achieve the best mechanical strength to avoid curling of the film when filling the conductor, and to achieve high ionic conductivity, preferably 400 μm.

[0071] The seventh aspect of the present invention provides a lithium ion battery, wherein the polymer lithium ion battery comprises the polymer electrolyte. The lithium ion battery comprises a positive electrode, a negative electrode and the polymer electrolyte provided by the present invention, wherein the polymer electrolyte is located between the positive electrode and the negative electrode.

[0072] The positive electrode includes a positive electrode current collector and a positive electrode active material loaded thereon. The positive electrode current collector may be an aluminum foil. The present invention has no particular restrictions on the positive electrode material. The positive electrode material generally includes a positive electrode active material, a binder, and a conductive agent. The positive electrode active material may be any commercially available positive electrode material, such as LiFePO4, LiMnO2, LiNiO2, LiCoO2, LiVPO4F, LiFeO2, or a ternary system.

[0073] The negative electrode includes a negative electrode current collector and a negative electrode active material loaded thereon. The negative electrode current collector may be a copper foil. The present invention has no particular restrictions on the negative electrode material. The negative electrode material generally includes a negative electrode active material, a binder, and a conductive agent. The negative electrode active material may be any negative electrode material commercially available to date, such as one or more mixtures of natural graphite, artificial graphite, hard carbon, soft carbon, lithium titanate, and the like.

[0074] The binder may be any binder known in the art, for example, one or more of polyvinylidene fluoride, polytetrafluoroethylene, styrene-butadiene rubber, and polyacrylate. The conductive agent may be any conductive agent known in the art, for example, one or more of graphite, carbon fiber, carbon black, metal powder, metal oxide, and fiber.

[0075] The present invention has no particular limitation on the preparation method of the lithium ion battery containing the polymer electrolyte, and the method known in the art can be adopted, for example: coating the solution of the polymer electrolyte on the surface of the positive electrode sheet and the negative electrode sheet of the battery, drying and removing the solvent to form a polymer electrolyte, then winding or stacking the positive electrode sheet and the negative electrode sheet coated with the polymer electrolyte to prepare a pole core, placing it in a battery shell, sealing, forming, sealing, and packaging; or first preparing the polymer electrolyte, then attaching a film to the surface of the positive electrode sheet or the negative electrode sheet, then winding or stacking the positive electrode sheet and the negative electrode sheet to prepare a pole core, placing it in a battery shell, sealing, forming, sealing, and packaging; or adding the prepared polymer electrolyte between the positive electrode sheet and the negative electrode sheet adhered with the polymer electrolyte provided by the present invention, then winding or stacking the positive electrode sheet and the negative electrode sheet to prepare a pole core, placing it in a battery shell, sealing, forming, sealing, and packaging, and the added polymer includes the polymer electrolyte provided by the present invention, and also includes other polymer electrolytes and diaphragm materials. The sealing and forming operations are carried out by methods known in the art.

[0076] An eighth aspect of the present invention provides an electrical device, which includes the above-mentioned lithium-ion battery.

[0077] The present invention will be described in detail below through examples.

[0078] In the following examples and comparative examples, if no specific conditions are specified, the experiments are carried out under conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used, if no manufacturer is specified, are conventional products that can be obtained through commercial channels. The composition and structure of the cross-linked polymers described in the following examples and comparative examples can be determined by nuclear magnetic resonance, infrared, GPC, elemental analysis, etc., or by preparing and feeding.

[0079] Example 1

[0080] (1) Preparation of cross-linked polymers

[0081] Compound a (wherein R1=R2=CH3, n=m=3) and compound b were mixed in a molar ratio of 3:1, and the mixture was heated to 120°C in a chlorobenzene solvent to cause polycondensation, wherein the weight average molecular weight of the cross-linked polymer was 800,000 g / mol.

[0082] At the same time, add an appropriate amount of SiO2 with a particle size of 14 nm, heat to 150°C, and stir until mixed evenly. Pour the prepolymer melt onto a glass sheet, heat to 150°C in a vacuum box overnight, remove the resulting film from the glass sheet, weigh it, and soak it in an ethyl acetate solution of lithium salt for 24 hours to swell. After swelling, dry the film at 60°C in a vacuum box overnight, and weigh it to calculate the amount of lithium salt. The prepared polymer electrolyte film is immediately transferred to a glove box filled with argon to avoid absorbing moisture from the air. In the glove box, propylene carbonate is added, and the film swells for at least two hours and reaches equilibrium to prepare the final polymer electrolyte S1.

[0083] (3) Preparation of polymer electrolyte composite electrodes

[0084] Take appropriate amounts of lithium iron phosphate (LiFePO4) (35wt%), single-walled carbon nanotubes (5wt%), the prepared polymer electrolyte S1 and N-methylpyrrolidone (NMP), mix them evenly, pour the mixture onto a block of polytetrafluoroethylene, vacuum, heat to 150°C, overnight, and obtain a polymer electrolyte composite electrode C1.

[0085] Example 2

[0086] (1) Preparation of cross-linked polymers

[0087] Compound a (wherein R1=R2=CH3, n=m=33) and compound b were mixed in a molar ratio of 3:1, and the mixture was heated to 120°C in a chlorobenzene solvent to cause polycondensation, wherein the weight average molecular weight of the cross-linked polymer was 1.2 million g / mol.

[0088] (2) Preparation of polymer electrolyte

[0089] Add an appropriate amount of SiO2 with a particle size of 14 nm to the cross-linked polymer, heat to 150°C, and stir until mixed evenly. Pour the prepolymer melt onto a glass sheet, heat to 150°C in a vacuum oven overnight, remove the resulting film from the glass sheet, weigh it, and soak it in an ethyl acetate solution of lithium salt for 24 hours to swell. After swelling, dry the film at 60°C in a vacuum oven overnight, and weigh it to calculate the amount of lithium salt. The prepared polymer electrolyte film is immediately transferred to a glove box filled with argon to avoid absorbing moisture from the air. In the glove box, propylene carbonate is added, and the film swells for at least two hours and reaches equilibrium to prepare the final polymer electrolyte S2.

[0090] (3) Preparation of polymer electrolyte composite electrodes

[0091] Take appropriate amounts of lithium iron phosphate (LiFePO4) (35wt%), single-walled carbon nanotubes (5wt%), the prepared polymer electrolyte S2, and N-methylpyrrolidone (NMP), mix them evenly, pour the mixture onto a block of polytetrafluoroethylene, vacuum, heat to 150°C, overnight, and obtain a polymer electrolyte composite electrode C2.

[0092] Example 3

[0093] (1) Preparation of cross-linked polymers

[0094] Compound a (wherein R1=R2=CH3, n=m=68) and compound b were mixed in a molar ratio of 3:1, and the mixture was heated to 120°C in a chlorobenzene solvent to cause polycondensation, wherein the weight average molecular weight of the cross-linked polymer was 1.8 million g / mol.

[0095] (2) Preparation of polymer electrolyte

[0096] Add an appropriate amount of SiO2 with a particle size of 14 nm to the cross-linked polymer, heat to 150°C, and stir until mixed evenly. Pour the prepolymer melt onto a glass sheet, heat to 150°C in a vacuum oven overnight, remove the resulting film from the glass sheet, weigh it, and soak it in an ethyl acetate solution of lithium salt for 24 hours to swell. After swelling, dry the film at 60°C in a vacuum oven overnight, and weigh it to calculate the amount of lithium salt. The prepared polymer electrolyte film is immediately transferred to a glove box filled with argon to avoid absorbing moisture from the air. In the glove box, propylene carbonate is added, and the film swells for at least two hours and reaches equilibrium to prepare the final polymer electrolyte S3.

[0097] (3) Preparation of polymer electrolyte composite electrodes

[0098] Take appropriate amounts of lithium iron phosphate (LiFePO4) (35wt%), single-walled carbon nanotubes (5wt%), the prepared polymer electrolyte S3, and N-methylpyrrolidone (NMP), mix them evenly, pour the mixture onto a block of polytetrafluoroethylene, vacuum, heat to 150°C, overnight, and obtain a polymer electrolyte composite electrode C3.

[0099] Example 4

[0100] (1) Preparation of cross-linked polymers

[0101] Compound a (wherein R1=R2=H, n=m=3) and compound b were mixed in a molar ratio of 3:1, and the mixture was heated to 120° C. in a chlorobenzene solvent to cause polycondensation, wherein the weight average molecular weight of the cross-linked polymer was 600,000 g / mol.

[0102] (2) Preparation of polymer electrolyte

[0103] Add an appropriate amount of SiO2 with a particle size of 14 nm to the cross-linked polymer, heat to 150°C, and stir until mixed evenly. Pour the prepolymer melt onto a glass sheet, heat to 150°C in a vacuum oven overnight, remove the resulting film from the glass sheet, weigh it, and soak it in an ethyl acetate solution of lithium salt for 24 hours to swell. After swelling, dry the film at 60°C in a vacuum oven overnight, and weigh it to calculate the amount of lithium salt. The prepared polymer electrolyte film is immediately transferred to a glove box filled with argon to avoid absorbing moisture from the air. In the glove box, propylene carbonate is added, and the film swells for at least two hours and reaches equilibrium to prepare the final polymer electrolyte S4.

[0104] (3) Preparation of polymer electrolyte composite electrodes

[0105] Take appropriate amounts of lithium iron phosphate (LiFePO4) (35wt%), single-walled carbon nanotubes (5wt%), the prepared polymer electrolyte S4, and N-methylpyrrolidone (NMP), mix them evenly, pour the mixture onto a block of polytetrafluoroethylene, vacuum, heat to 150°C, overnight, and obtain a polymer electrolyte composite electrode C4.

[0106] Example 5

[0107] (1) Preparation of cross-linked polymers

[0108] Compound a (wherein R1=R2=H, n=m=33) and compound b were mixed in a molar ratio of 3:1, and the mixture was heated to 120° C. in a chlorobenzene solvent to cause polycondensation, wherein the weight average molecular weight of the cross-linked polymer was 900,000 g / mol.

[0109] (2) Preparation of polymer electrolyte

[0110] Add an appropriate amount of SiO2 with a particle size of 14 nm to the cross-linked polymer, heat to 150°C, and stir until mixed evenly. Pour the prepolymer melt onto a glass sheet, heat to 150°C in a vacuum oven overnight, remove the resulting film from the glass sheet, weigh it, and soak it in an ethyl acetate solution of lithium salt for 24 hours to swell. After swelling, dry the film at 60°C in a vacuum oven overnight, and weigh it to calculate the amount of lithium salt. The prepared polymer electrolyte film is immediately transferred to a glove box filled with argon to avoid absorbing moisture from the air. In the glove box, propylene carbonate is added, and the film swells for at least two hours and reaches equilibrium to prepare the final polymer electrolyte S5.

[0111] (3) Preparation of polymer electrolyte composite electrodes

[0112] Take appropriate amounts of lithium iron phosphate (LiFePO4) (35wt%), single-walled carbon nanotubes (5wt%), the prepared polymer electrolyte S5, and N-methylpyrrolidone (NMP), mix them evenly, pour the mixture onto a block of polytetrafluoroethylene, vacuum, heat to 150°C, and leave overnight to obtain a polymer electrolyte composite electrode C5.

[0113] Example 6

[0114] (1) Preparation of cross-linked polymers

[0115] Compound a (wherein R1=R2=H, n=m=68) and compound b were mixed in a molar ratio of 3:1, and the mixture was heated to 120°C in a chlorobenzene solvent to cause polycondensation, wherein the weight average molecular weight of the cross-linked polymer was 1.45 million g / mol.

[0116] (2) Preparation of polymer electrolyte

[0117] Add an appropriate amount of SiO2 with a particle size of 14 nm to the cross-linked polymer, heat to 150°C, and stir until mixed evenly. Pour the prepolymer melt onto a glass sheet, heat to 150°C in a vacuum oven overnight, remove the resulting film from the glass sheet, weigh it, and soak it in an ethyl acetate solution of lithium salt for 24 hours to swell. After swelling, dry the film at 60°C in a vacuum oven overnight, and weigh it to calculate the amount of lithium salt. The prepared polymer electrolyte film is immediately transferred to a glove box filled with argon to avoid absorbing moisture from the air. In the glove box, propylene carbonate is added, and the film swells for at least two hours and reaches equilibrium to prepare the final polymer electrolyte S6.

[0118] (3) Preparation of polymer electrolyte composite electrodes

[0119] Take appropriate amounts of lithium iron phosphate (LiFePO4) (35wt%), single-walled carbon nanotubes (5wt%), the prepared polymer electrolyte S6, and N-methylpyrrolidone (NMP), mix them evenly, pour the mixture onto a block of polytetrafluoroethylene, vacuum, heat to 150°C, overnight, and obtain a polymer electrolyte composite electrode C6.

[0120] Example 7

[0121] (1) Preparation of cross-linked polymers

[0122] Compound a (wherein R1=H, R2=CH3, n=m=3) and compound b were mixed in a molar ratio of 3:1, and the mixture was heated to 120°C in a chlorobenzene solvent to cause polycondensation, wherein the weight average molecular weight of the cross-linked polymer was 700,000 g / mol.

[0123] (2) Preparation of polymer electrolyte

[0124] Add an appropriate amount of SiO2 with a particle size of 14 nm to the cross-linked polymer, heat to 150°C, and stir until mixed evenly. Pour the prepolymer melt onto a glass sheet, heat to 150°C in a vacuum oven overnight, remove the resulting film from the glass sheet, weigh it, and soak it in an ethyl acetate solution of lithium salt for 24 hours to swell. After swelling, dry the film at 60°C in a vacuum oven overnight, and weigh it to calculate the amount of lithium salt. The prepared polymer electrolyte film is immediately transferred to a glove box filled with argon to avoid absorbing moisture from the air. In the glove box, propylene carbonate is added, and the film swells for at least two hours and reaches equilibrium to prepare the final polymer electrolyte S7.

[0125] (3) Preparation of polymer electrolyte composite electrodes

[0126] Take appropriate amounts of lithium iron phosphate (LiFePO4) (35wt%), single-walled carbon nanotubes (5wt%), the prepared polymer electrolyte S7, and N-methylpyrrolidone (NMP), mix them evenly, pour the mixture onto a block of polytetrafluoroethylene, vacuum, heat to 150°C, overnight, and obtain a polymer electrolyte composite electrode C7.

[0127] Example 8

[0128] (1) Preparation of cross-linked polymers

[0129] Compound a (wherein R1=H, R2=CH3, n=m=33) and compound b are mixed in a molar ratio of 3:1, and the mixture is heated to 120°C in a chlorobenzene solvent to cause condensation polymerization, wherein the weight average molecular weight of the cross-linked polymer is 1 million g / mol.

[0130] (2) Preparation of polymer electrolyte

[0131] Add an appropriate amount of SiO2 with a particle size of 14 nm to the cross-linked polymer, heat to 150°C, and stir until well mixed. Pour the prepolymer melt onto a glass sheet, heat to 150°C in a vacuum oven overnight, remove the resulting film from the glass sheet, weigh it, and soak it in an ethyl acetate solution of lithium salt for 24 hours to swell. After swelling, dry the film at 60°C in a vacuum oven overnight, and weigh it to calculate the amount of lithium salt. The prepared polymer electrolyte film is immediately transferred to a glove box filled with argon to avoid absorbing moisture from the air. In the glove box, propylene carbonate is added, and the film swells for at least two hours and reaches equilibrium to prepare the final polymer electrolyte S8.

[0132] (3) Preparation of polymer electrolyte composite electrodes

[0133] Take appropriate amounts of lithium iron phosphate (LiFePO4) (35wt%), single-walled carbon nanotubes (5wt%), the prepared polymer electrolyte S8, and N-methylpyrrolidone (NMP), mix them evenly, pour the mixture onto a block of polytetrafluoroethylene, vacuum, heat to 150°C, overnight, and obtain a polymer electrolyte composite electrode C8.

[0134] Example 9

[0135] (1) Preparation of cross-linked polymers

[0136] Compound a (wherein R1=H, R2=CH3, n=m=68) and compound b were mixed in a molar ratio of 3:1, and the mixture was heated to 120°C in a chlorobenzene solvent to cause polycondensation, wherein the weight average molecular weight of the cross-linked polymer was 1.6 million g / mol.

[0137] (2) Preparation of polymer electrolyte

[0138] Add an appropriate amount of SiO2 with a particle size of 14 nm to the cross-linked polymer, heat to 150°C, and stir until mixed evenly. Pour the prepolymer melt onto a glass sheet, heat to 150°C in a vacuum oven overnight, remove the resulting film from the glass sheet, weigh it, and soak it in an ethyl acetate solution of lithium salt for 24 hours to swell. After swelling, dry the film at 60°C in a vacuum oven overnight, and weigh it to calculate the amount of lithium salt. The prepared polymer electrolyte film is immediately transferred to a glove box filled with argon to avoid absorbing moisture from the air. In the glove box, propylene carbonate is added, and the film swells for at least two hours and reaches equilibrium to prepare the final polymer electrolyte S9.

[0139] (3) Preparation of polymer electrolyte composite electrodes

[0140] Take appropriate amounts of lithium iron phosphate (LiFePO4) (35wt%), single-walled carbon nanotubes (5wt%), the prepared polymer electrolyte S9, and N-methylpyrrolidone (NMP), mix them evenly, pour the mixture onto a block of polytetrafluoroethylene, vacuum, heat to 150°C, overnight, and obtain a polymer electrolyte composite electrode C9.

[0141] Example 10

[0142] (1) Preparation of cross-linked polymers

[0143] Compound a (wherein R1=H, R2=CH3, n=3, m=33) and compound b were mixed in a molar ratio of 3:1, and the mixture was heated to 120°C in a chlorobenzene solvent to cause polycondensation, wherein the weight average molecular weight of the cross-linked polymer was 1.1 million g / mol.

[0144] (2) Preparation of polymer electrolyte

[0145] Add an appropriate amount of SiO2 with a particle size of 14 nm to the cross-linked polymer, heat to 150°C, and stir until mixed evenly. Pour the prepolymer melt onto a glass sheet, heat to 150°C in a vacuum oven overnight, remove the resulting film from the glass sheet, weigh it, and soak it in an ethyl acetate solution of lithium salt for 24 hours to swell. After swelling, dry the film at 60°C in a vacuum oven overnight, and weigh it to calculate the amount of lithium salt. The prepared polymer electrolyte film is immediately transferred to a glove box filled with argon to avoid absorbing moisture from the air. In the glove box, propylene carbonate is added, and the film swells for at least two hours and reaches equilibrium to prepare the final polymer electrolyte S10.

[0146] (3) Preparation of polymer electrolyte composite electrodes

[0147] Take appropriate amounts of lithium iron phosphate (LiFePO4) (35wt%), single-walled carbon nanotubes (5wt%), the prepared polymer electrolyte S10, and N-methylpyrrolidone (NMP), mix them evenly, pour the mixture onto a block of polytetrafluoroethylene, vacuum, heat to 150°C, and leave overnight to obtain a polymer electrolyte composite electrode C10.

[0148] Embodiment 11

[0149] (1) Preparation of cross-linked polymers

[0150] Compound a (wherein R1=H, R2=CH3, n=3, m=68) and compound b were mixed in a molar ratio of 3:1, and the mixture was heated to 120°C in a chlorobenzene solvent to cause polycondensation, wherein the weight average molecular weight of the cross-linked polymer was 1.3 million g / mol.

[0151] (2) Preparation of polymer electrolyte

[0152] Add an appropriate amount of SiO2 with a particle size of 14 nm to the cross-linked polymer, heat to 150°C, and stir until well mixed. Pour the prepolymer melt onto a glass sheet, heat to 150°C in a vacuum oven overnight, remove the resulting film from the glass sheet, weigh it, and soak it in an ethyl acetate solution of lithium salt for 24 hours to swell. After swelling, dry the film at 60°C in a vacuum oven overnight, and weigh it to calculate the amount of lithium salt. The prepared polymer electrolyte film is immediately transferred to a glove box filled with argon to avoid absorbing moisture from the air. In the glove box, propylene carbonate is added, and the film swells for at least two hours and reaches equilibrium to prepare the final polymer electrolyte S11.

[0153] (3) Preparation of polymer electrolyte composite electrodes

[0154] Take appropriate amounts of lithium iron phosphate (LiFePO4) (35wt%), single-walled carbon nanotubes (5wt%), the prepared polymer electrolyte S11, and N-methylpyrrolidone (NMP), mix them evenly, pour the mixture onto a block of polytetrafluoroethylene, vacuum, heat to 150°C, and leave overnight to obtain a polymer electrolyte composite electrode C11.

[0155] Example 12

[0156] (1) Preparation of cross-linked polymers

[0157] Compound a (wherein R1=H, R2=CH3, n=33, m=68) and compound b were mixed in a molar ratio of 3:1, and the mixture was heated to 120°C in a chlorobenzene solvent to cause polycondensation, wherein the weight average molecular weight of the cross-linked polymer was 1.65 million g / mol.

[0158] (2) Preparation of polymer electrolyte

[0159] Add an appropriate amount of SiO2 with a particle size of 14 nm to the cross-linked polymer, heat to 150°C, and stir until mixed evenly. Pour the prepolymer melt onto a glass sheet, heat to 150°C in a vacuum oven overnight, remove the resulting film from the glass sheet, weigh it, and soak it in an ethyl acetate solution of lithium salt for 24 hours to swell. After swelling, dry the film at 60°C in a vacuum oven overnight, and weigh it to calculate the amount of lithium salt. The prepared polymer electrolyte film is immediately transferred to a glove box filled with argon to avoid absorbing moisture from the air. In the glove box, propylene carbonate is added, and the film swells for at least two hours and reaches equilibrium to prepare the final polymer electrolyte S12.

[0160] (3) Preparation of polymer electrolyte composite electrodes

[0161] Take appropriate amounts of lithium iron phosphate (LiFePO4) (35wt%), single-walled carbon nanotubes (5wt%), the prepared polymer electrolyte S12, and N-methylpyrrolidone (NMP), mix them evenly, pour the mixture onto a block of polytetrafluoroethylene, vacuum, heat to 150°C, overnight, and obtain a polymer electrolyte composite electrode C12.

[0162] Comparative Example 1

[0163] Take 0.683g of lithium salt (LiTFSI) and 1g of polyethylene oxide (PEO) (weight average molecular weight of 400000g / mol), add them to an appropriate amount of anhydrous acetonitrile, stir at room temperature for 24h, cast into a film in polytetrafluoroethylene, and then vacuum dry at 50°C for 48h to obtain polymer electrolyte RS1, which is a polyethylene oxide electrolyte.

[0164] Test example:

[0165] The cross-linked polymers prepared in Examples 1-12 were subjected to infrared spectroscopy analysis to determine the presence of macromolecular chains A, cross-linked structures B, linking groups -NH-, covalent bonds -CN-, and hydrogen bonds in the cross-linked polymers prepared. The test instrument used was a Nicolet iS50 FT / IR spectrometer with a diamond attenuated total reflection accessory.

[0166] The polymer electrolytes S1-S12 prepared in Examples 1-12 and the comparative example RS1 were tested, and the results are shown in Table 1.

[0167] Thermogravimetric analysis: The instrument TAG-SDTA851 was used, and the temperature rise rate was 20℃ / min, and the temperature was raised to 600℃ in a nitrogen atmosphere. The test results of polymer electrolyte S1 are as follows Figure 2 shown.

[0168] Crystallinity and glass transition temperature: Differential scanning calorimetry (DSC-Q2000) was used, indium standard was used for calibration, sample weight was 8-10 mg, temperature range was -70℃ to 150℃, heating and cooling rates were 10℃ / min. The crystallinity and glass transition temperature of polymer electrolytes S1-S12 and RS1 were recorded. The differential thermal analysis of polymer electrolyte S1 is shown in Figure 3 .

[0169] Tensile strength and elongation at break: The tensile and compression test equipment Instron 5565 was used, and the strain rate of the instrument was 100% / min. The test results of polymer electrolyte S1 are shown in Figure 4 and Figure 5 shown.

[0170] Morphological analysis of polymer electrolyte and composite electrode: The morphology of polymer electrolyte S1 and composite electrode C1 of Example 1 was characterized and analyzed using a scanning electron microscope (FEI SL30SirionSEM). Figure 6 and 7 As shown, the lithium iron phosphate (LFP) particles are uniformly dispersed in the cross-linked polymer prepared in Example 1, and the carbon nanotubes play a connecting role between the components to form a conductive system, so that the composite electrode has good conductivity.

[0171] Electrochemical impedance test: The test frequency is 1MHz to 100mHz, and the temperature is adjusted in a constant temperature and humidity chamber. The temperature range is 20-80℃, and the disturbance signal is 50mV. The electrochemical impedance spectrum of polymer electrolyte S1 is shown in the figure. Figure 8 shown.

[0172] Conductivity: The polymer electrolytes S1-S12 prepared in Examples 1-12 and RS1 of the comparative example were cut into pieces with an area of ​​2 cm 2 The film is 0.4 mm thick. These polymer electrolyte membranes are sandwiched between two parallel stainless steel sheets in gloves to assemble into 2032 button batteries. The battery model is "stainless steel sheet | polymer electrolyte membrane | stainless steel sheet". The CHI660B electrochemical workstation of Shanghai Chenhua Instrument Co., Ltd. is used. The test frequency range is 1-100kHz, and the temperature is -20℃, -15℃, 20℃, 50℃, 80℃, and 110℃. The bulk resistance (R h ) is the intersection of the Nyquist curve and the real axis. According to the formula σ=I / (A·R h ) to calculate the ionic conductivity, where σ is the ionic conductivity, I is the thickness of the polymer electrolyte membrane, and A is the contact area between the polymer electrolyte membrane and the electrode. The test and calculation results are shown in Table 1 and Fig. 9 shown.

[0173] Electrochemical stability test: The polymer electrolyte was assembled into a 2032 button cell in a glove box filled with argon. The battery model was "lithium metal sheet | polymer electrolyte membrane | stainless steel sheet". Cyclic voltammetry was used, and the voltage scan was from the open circuit voltage down to -0.7V and then up to 5.5V at a rate of 1mV / s. The oxidation potential of the polymer electrolyte S1 was 4.3V (vs. Li). The test results are as follows: Fig.10 shown.

[0174] Table 1

[0175]

[0176]

[0177] From the results in Table 1, it can be seen that compared with traditional electrolytes, the electrolyte prepared by using the cross-linked polymer provided by the present invention has better ionic conductivity and lower electrochemical impedance, has excellent electrochemical performance, and is superior to traditional electrolytes in mechanical properties such as elongation at break, tensile strength and strain recovery rate, and can effectively improve the safety performance of lithium-ion batteries. Among them, the polymer electrolyte of Example 10 has the best comprehensive performance, which is manifested in high ionic conductivity and high tensile strength.

[0178] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A cross-linked polymer, characterized in that The cross-linked polymer comprises: a macromolecular chain A derived from compound a represented by formula (1), a cross-linked structure B derived from compound b represented by formula (2), and a connecting group -NH- connecting the macromolecular chain A and the cross-linked structure B; Wherein, the macromolecular chain A comprises a polyether flexible segment; The cross-linked polymer has a composite structure of hydrogen bonds and covalent bonds, wherein the covalent bond is -CN-, and the hydrogen bond is formed by the complexation of the hydrogen atom of the amino group in compound b and the double-bonded oxygen atom on the nitrogen-containing heterocyclic ring in compound a; Wherein, R1 and R2 are each independently H, C1-C6 straight chain alkyl or C3-C6 branched chain alkyl; m is an integer of 1-100, and n is an integer of 1-100.

2. The cross-linked polymer according to claim 1, characterized in that In the cross-linked polymer, the molar ratio of the macromolecular chain A: the cross-linked structure B is 1-10:1, preferably 3-5:1; Preferably, in the cross-linked polymer, m is an integer of 3-60, and n is an integer of 3-60.

3. The cross-linked polymer according to claim 1 or 2, characterized in that The weight average molecular weight of the cross-linked polymer is 600,000-2,000,000 g / mol.

4. A method for preparing a cross-linked polymer, characterized in that: The preparation method comprises: performing a cross-linking reaction on a compound a represented by formula (1) and a compound b represented by formula (2) to obtain the cross-linked polymer; wherein the terminal group -OH in the compound a is bonded with the terminal group -NH2 in the compound b to form a connecting group -NH-; the hydrogen atom of the amino group in the compound b is complexed with the double-bonded oxygen atom on the nitrogen-containing heterocyclic ring in the compound a; Wherein, R1 and R2 are each independently H, C1-C6 straight chain alkyl or C3-C6 branched chain alkyl; m is an integer of 1-100, and n is an integer of 1-100.

5. The preparation method according to claim 4, characterized in that: The cross-linking reaction temperature is 100-150°C; the cross-linking reaction time is 10-20min; Preferably, the cross-linking reaction is carried out in a solvent, and the solvent is chlorobenzene.

6. The preparation method according to claim 4 or 5, characterized in that: The molar ratio of compound a:compound b is 1-10:1, preferably 3-5:

1.

7. A cross-linked polymer obtained by the preparation method according to any one of claims 4 to 6.

8. A polymer electrolyte raw material composition, characterized in that: include: A lithium salt, a filler, a plasticizer and a cross-linked polymer as claimed in any one of claims 1 to 3 and 7.

9. The polymer electrolyte raw material composition according to claim 8, characterized in that: The lithium salt is selected from one or more of lithium bis(trifluoromethylsulfonyl)imide, lithium hexafluorophosphate, lithium perchlorate, lithium tetrafluoroborate, lithium hexafluoroarsenate, lithium hexafluorosilicate, lithium tetraphenylborate, lithium chloride, lithium bromide, lithium chloroaluminate, lithium fluoroalkylsulfonate, LiCH3SO3, LiN(SO2CF3)2, and LiN(SO2C2F5)2; preferably selected from lithium bis(trifluoromethylsulfonyl)imide; Preferably, the filler is selected from one or more of TiO2, Al2O3, SiO2, MgO, ZrO2, LiNbO3, BaTiO3, PbTiO3, montmorillonite, and molecular sieve; Preferably, the plasticizer is selected from one or more of ethylene carbonate, propylene carbonate and vinylene carbonate.

10. The polymer electrolyte raw material composition according to claim 8 or 9, characterized in that: The cross-linked polymer is 25-50 parts by weight, the lithium salt is 20-40 parts by weight, the filler is 1-4 parts by weight, and the plasticizer is 20-40 parts by weight.

11. A method for preparing a polymer electrolyte, characterized in that: The preparation method comprises: (1) reacting a filler with the cross-linked polymer according to any one of claims 1 to 3 and 7 to form a film to obtain a film-forming substance; (2) The film-forming substance is mixed with a lithium salt solution and a plasticizer to obtain the polymer electrolyte.

12. A polymer electrolyte obtained by the preparation method according to claim 11.

13. The polymer electrolyte according to claim 12, characterized in that The polymer electrolyte has an ion conductivity of 0.48-5.5 S / cm, an electrochemical impedance of 470-540Ω, a breaking elongation of 115-129%, a tensile strength of 0.33-0.51 MPa, and a strain recovery rate of 63.4-82.3%.

14. A lithium ion battery, characterized in that: The polymer lithium ion battery comprises the polymer electrolyte according to claim 12.

15. An electrical equipment, characterized in that: Including the lithium ion battery as claimed in claim 14.

Citation Information

Patent Citations

  • Organic coating layer, electrode active material containing coating layer and lithium ion battery

    CN113823799A

  • Polymer electrolyte matrix and preparation method thereof, polymer electrolyte and lithium ion battery

    CN115725056A

  • High performance battery anodes with polymeric coatings

    US20170062830A1

  • Polymer electrolyte for a lithium metal polymer battery having improved performance

    US20220029197A1

  • Polymer electrolyte membrane, electrode structure and electrochemical device including same, and method for manufacturing polymer electrolyte membrane

    US20220376295A1

Cited By

  • Polyformaldehyde halide composite solid electrolyte and preparation method thereof

    CN122267271A