Preparation method and application of supramolecular self-assembly hydrophobic active agent
The nanoscale lotus leaf bionic structure is constructed by supramolecular chemistry, which solves the problem of the substrate surface covering low-surface energy hydrophobic materials, and realizes the preparation of a green and environmentally friendly hydrophobic coating, with good hydrophobic properties and imitation lotus leaf structure.
Patent Information
- Application Number
- CN202411173772.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-26
AI Technical Summary
The prior art is difficult to effectively coat the surface of the substrate with low surface energy hydrophobic materials, have a microscopic hydrophobic structure that imitates lotus leaves, and the traditional method uses organic solvents to have environmental problems.
Using non-covalent interactions of supramolecular chemistry, Schiff base ligands are synthesized through aldehyde groups and amino groups, and using non-covalent interactions of imidazole and zinc ions to combine the electron withdrawal effect of perfluoro compounds to construct nanoscale Bionic structure of lotus leaves.
A lotus leaf structure with good hydrophobicity is formed on the surface of the substrate, and the environmental protection problem of using organic solvents is avoided, and a green and environmentally friendly hydrophobic coating preparation method is provided.
Smart Images

Figure CN119060348A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a preparation method and application of a supramolecular self-assembly hydrophobic active agent, and belongs to the field of surface modification engineering and hydrophobic coating. Background Art
[0002] Due to the fact that droplets on the hydrophobic surface are difficult to stay, the surface has the characteristics of waterproof, anti-icing, anti-fogging, and self-cleaning. In the field of aerospace, the hydrophobic coating on the surface of the aircraft can effectively prevent the fuselage from icing, ensure flight performance, and avoid air crashes; in the field of transportation, the hydrophobic coating can prevent the glass from fogging, ensure clear vision, and ensure driving safety; in the field of electronics and electrical, the hydrophobic coating can prevent water accumulation on the circuit board and prevent short circuits or rusting of electronic components; in daily life, the hydrophobic coating can prevent the bottom of the pot from sticking. Therefore, the hydrophobic surface has a very broad application prospect.
[0003] Imitation of lotus leaf structure has always been the research direction of researchers of hydrophobic coatings. The surface of lotus leaves has a dense micro-protrusion structure with a height of about 5 microns. Further magnification and observation can reveal that a layer of nano-scale papillae is attached to the surface of the micro-protrusions, with a height of about 200 nanometers. In addition, lotus leaves secrete a layer of biological wax on their surface to resist external invasion. It is precisely the characteristics of this surface micro-nano composite structure combined with biological wax that give lotus leaves unique hydrophobic properties, making it difficult for water droplets to stay on the surface of lotus leaves, and the droplets will carry away dust and debris on the surface during the rapid rolling process on its surface, achieving self-cleaning. At present, the ideas for preparing hydrophobic surfaces are mostly focused on the preparation and coating of biological wax, mainly through perfluorinated compounds or other low surface energy materials. From the perspective of the micro-nano structure of imitating lotus leaves, it is more difficult because the structural structure requires fine design.
[0004] Early research mainly focuses on chemical synthesis methods. Fluoride is insoluble in water and conventional organic solvents, and is soluble in organic fluoride solvents. Therefore, when the material is subjected to hydrophobic surface treatment, it is necessary to infiltrate fluorinated organic solvents. This treatment method is considered to be not green enough because of the toxicity of organic solvents, and is limited in application. Therefore, it is increasingly emerging to prepare green and environmentally friendly water-based super-hydrophobic coatings by replacing volatile organic solvents with water-based solvents. So far, some preparation methods have been explored, such as wet chemical processes of polymer-particle dispersions, electrochemical deposition methods, template methods, etching methods, sol-gel methods, and hydrothermal methods. However, how to coat the substrate surface with both a hydrophobic material with low surface energy and a microscopic hydrophobic structure of imitating lotus leaves is a major problem at present. Summary of the invention
[0005] The technical solution of the present invention is: to overcome the shortcomings of the prior art, abandon the traditional single covalent interaction, use the non-covalent interaction of supramolecular chemistry, first use aldehyde groups and amino groups to synthesize Schiff base ligands, then use the non-covalent interaction of imidazole and zinc ions to realize the self-assembly of the first layer of micelles, and the electron-withdrawing effect of perfluorinated compounds to realize the self-assembly of the second layer of micelles, so as to construct a nano-scale lotus leaf bionic structure. The bionic structure material itself has hydrophobicity, and at the same time has a microscopic hydrophobic structure imitating lotus leaves, and has good hydrophobicity.
[0006] The technical solution of the present invention is:
[0007] A supramolecular self-assembly hydrophobic active agent, comprising a ligand, 1H,1H,2H,2H-perfluoro-1-alcohol, a zinc chloride crosslinking agent and anhydrous ethanol;
[0008] The zinc chloride crosslinking agent, the ligand, and 1H,1H,2H,2H-perfluoro-1-ol self-assemble into micelles and are dispersed in anhydrous ethanol;
[0009] The ratio of the zinc chloride cross-linking agent, the ligand, 1H,1H,2H,2H-perfluoro-1-alcohol and anhydrous ethanol is 1mmol:1-2mmol:1-3mmol:100ml.
[0010] The preparation method of the ligand is:
[0011] An anhydrous ethanol solution of 1,8-octanediamine, an anhydrous ethanol solution of 4-formylimidazole and glacial acetic acid are mixed for reaction, and the product obtained by the reaction is dried in a vacuum oven at 85-95° C. for 4.5-5.5 hours after the solvent is evaporated in a fume hood for 12-15 hours to obtain a ligand.
[0012] In the anhydrous ethanol solution of 1,8-octanediamine, the ratio of 1,8-octanediamine to anhydrous ethanol is 0.05 mol:20-30 ml;
[0013] In the anhydrous ethanol solution of 4-aldehyde imidazole, the ratio of 4-aldehyde imidazole to anhydrous ethanol is 0.1 mol: 15-25 ml;
[0014] The ratio of 1,8-octanediamine, 4-formylimidazole and glacial acetic acid is 0.05 mol:0.1 mol:3-5 ml.
[0015] The reaction temperature is 70-80°C and the reaction time is 4-5h.
[0016] A method for preparing a supramolecular self-assembled hydrophobic active agent, comprising the following steps:
[0017] The ethanol solution of the ligand, the anhydrous ethanol solution of 1H,1H,2H,2H-perfluoro-1-ol and the ethanol solution of zinc chloride are mixed and stirred to obtain a supramolecular self-assembled hydrophobic active agent.
[0018] The concentration of the anhydrous ethanol of the ligand is 25mmol / L;
[0019] The concentration of the anhydrous ethanol solution of zinc chloride is 25mmol / L;
[0020] The concentration of the anhydrous ethanol solution of 1H,1H,2H,2H-perfluoro-1-alcohol is 50mmol / L;
[0021] The volume ratio of the zinc chloride ethanol solution, the ligand ethanol solution and the 1H,1H,2H,2H-perfluoro-1-ol anhydrous ethanol solution is 2:1-2:1-3.
[0022] An application of a supramolecular self-assembled hydrophobic active agent in the field of hydrophobic coatings comprises the following steps:
[0023] The substrate is immersed in the supramolecular self-assembled hydrophobic active agent, and after the immersion is completed, the substrate is taken out and dried to obtain a hydrophobic substrate modified by the supramolecular self-assembled hydrophobic active agent.
[0024] The immersion time is 0.5-1h.
[0025] Beneficial Effects
[0026] The present invention utilizes the zinc ion coordination principle and the non-covalent interaction of low surface energy substances, firstly utilizes 4-aldehyde imidazole and 1,8-octanediamine to synthesize Schiff base ligands, then utilizes the imidazole group to coordinate with zinc ions to realize the first layer self-assembly, and the electron-withdrawing effect of the perfluorinated compound realizes the second layer self-assembly, thereby constructing a nano-scale lotus leaf bionic structure. The bionic structure material itself has hydrophobicity and also has a microscopic hydrophobic structure imitating the lotus leaf, and has good hydrophobicity. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 Schematic diagram of supramolecular self-assembled micelle;
[0028] Figure 2 This is a cryo-TEM image of micelles in water.
[0029] Figure 3 This is the contact angle test diagram of the substrate without hydrophobic treatment.
[0030] Figure 4 This is a SEM image of the lotus leaf structure on the substrate surface after surface modification by the active agent in Example 1.
[0031] Figure 5This is the contact angle test of the substrate after surface modification by the active agent in Example 1.
[0032] Figure 6 This is a SEM image of the lotus leaf structure on the substrate surface after surface modification by the active agent in Example 2.
[0033] Figure 7 This is the contact angle test of the substrate after surface modification by the active agent in Example 2. DETAILED DESCRIPTION
[0034] The present invention is further described below by way of examples, but the examples do not limit the protection scope of the present invention.
[0035] A supramolecular self-assembly hydrophobic active agent, comprising a ligand, 1H,1H,2H,2H-perfluoro-1-alcohol, a zinc chloride crosslinking agent and anhydrous ethanol; Figure 1 and Figure 2 As shown;
[0036] The zinc chloride crosslinking agent, the ligand, and 1H,1H,2H,2H-perfluoro-1-ol self-assemble into micelles and are dispersed in anhydrous ethanol;
[0037] The ratio of the zinc chloride cross-linking agent, the ligand, 1H,1H,2H,2H-perfluoro-1-alcohol and anhydrous ethanol is 1mmol:1-2mmol:1-3mmol:100ml.
[0038] A supramolecular self-assembly hydrophobic active agent, the preparation raw materials include main raw materials and auxiliary raw materials, the main raw materials include 1H, 1H, 2H, 2H-perfluoro-1-ol, zinc chloride, 1, 8-octanediamine, 4-aldehyde imidazole, the auxiliary raw materials are catalysts and solvents.
[0039] The catalyst is glacial acetic acid and the solvent is anhydrous ethanol.
[0040] A method for preparing a ligand, comprising the steps of:
[0041] In the first step, 0.05 mol of 1,8-octanediamine was added to a beaker, and 25 ml of anhydrous ethanol was added to dissolve the 1,8-octanediamine anhydrous ethanol solution was prepared. Subsequently, the 1,8-octanediamine anhydrous ethanol solution was transferred to a 250 ml three-necked flask.
[0042] In the second step, 0.1 mol of 4-formyl imidazole is added to a beaker, and 20 ml of anhydrous ethanol is added to dissolve the mixture to prepare an anhydrous ethanol solution of 4-formyl imidazole. The anhydrous ethanol solution of 4-formyl imidazole is then transferred into a 25 ml constant pressure separatory funnel, and the separatory funnel is assembled into the three-necked flask described in the first step.
[0043] The third step is to heat and stir the three-necked flask until it reaches 70°C, then add 3-5 ml of glacial acetic acid, open the constant pressure separatory funnel, and allow the anhydrous ethanol solution of 4-aldehyde imidazole to be continuously added dropwise into the three-necked flask.
[0044] Step 4: After 5 hours of reaction, pour the product solution into a beaker, cover with plastic wrap, poke some holes in it, and place it in a fume hood to evaporate the solvent for 12-15 hours to obtain a viscous mixture of the ligand and glacial acetic acid.
[0045] The fifth step is to place the viscous mixture obtained in the fourth step into a vacuum oven and dry it at 90° C. for 5 hours to remove the glacial acetic acid and obtain the ligand.
[0046] A method for preparing a supramolecular self-assembled hydrophobic active agent, comprising the following steps:
[0047] In the first step, 10 ml of 25 mmol / L anhydrous ethanol solution of zinc chloride is added to a beaker, followed by 25 mmol / L anhydrous ethanol solution of the ligand (the volume ratio of the ligand solution to the zinc chloride solution is 1:1-2). The mixture is then stirred for 30 minutes and allowed to stand for 1 hour to obtain a preliminary coordination solution.
[0048] In the second step, a 50 mmol / L anhydrous ethanol solution of 1H,1H,2H,2H-perfluoro-1-ol (the volume ratio of 1H,1H,2H,2H-perfluoro-1-ol to zinc chloride solution is 1:1-3) is added to the preliminary coordination solution obtained in the first step. The portion of the solution less than 60 ml is supplemented with anhydrous ethanol. Stir for 10 minutes to obtain a supramolecular self-assembled hydrophobic active agent.
[0049] An application of a supramolecular self-assembled hydrophobic active agent in the field of hydrophobic coatings comprises the following steps:
[0050] In the first step, the substrate was immersed in the supramolecular self-assembled hydrophobic active agent and stirred continuously for 2 h.
[0051] In the second step, the substrate is taken out and placed in a forced air oven for 2 hours to dry the anhydrous ethanol on the surface of the substrate to obtain a substrate modified by a supramolecular self-assembled hydrophobic active agent.
[0052] Example 1
[0053] A method for preparing a ligand, comprising the steps of:
[0054] In the first step, 0.05 mol of 1,8-octanediamine was added to a beaker, and 25 ml of anhydrous ethanol was added to dissolve the 1,8-octanediamine anhydrous ethanol solution was prepared. Subsequently, the 1,8-octanediamine anhydrous ethanol solution was transferred to a 250 ml three-necked flask.
[0055] In the second step, 0.1 mol of 4-formyl imidazole is added to a beaker, and 20 ml of anhydrous ethanol is added to dissolve the mixture to prepare an anhydrous ethanol solution of 4-formyl imidazole. The anhydrous ethanol solution of 4-formyl imidazole is then transferred into a 25 ml constant pressure separatory funnel, and the separatory funnel is assembled into the three-necked flask described in the first step.
[0056] The third step is to heat and stir the three-necked flask until it reaches 70°C, then add 5 ml of glacial acetic acid, open the constant pressure separatory funnel, and allow the anhydrous ethanol solution of 4-aldehyde imidazole to be continuously added dropwise into the three-necked flask.
[0057] Step 4: After 5 hours of reaction, pour the product solution into a beaker, cover with plastic wrap, poke some holes in it, and place it in a fume hood to evaporate the solvent for 15 hours to obtain a viscous mixture of the ligand and glacial acetic acid.
[0058] The fifth step is to place the viscous mixture obtained in the fourth step into a vacuum oven and dry it at 90° C. for 5 hours to remove the glacial acetic acid and obtain the ligand.
[0059] A method for preparing a supramolecular self-assembled hydrophobic active agent, comprising the following steps:
[0060] In the first step, 10 ml of a 25 mmol / L anhydrous ethanol solution of zinc chloride is added to a beaker, followed by 20 ml of a 25 mmol / L anhydrous ethanol solution of the ligand, followed by stirring for 30 minutes and standing for 1 hour to obtain a preliminary coordination solution.
[0061] In the second step, 30 ml of 50 mmol / L anhydrous ethanol solution of 1H,1H,2H,2H-perfluoro-1-ol was added to the preliminary coordination solution obtained in the first step, and stirred for 10 minutes to obtain a supramolecular self-assembled hydrophobic active agent.
[0062] An application of a supramolecular self-assembled hydrophobic active agent in the field of hydrophobic coatings comprises the following steps:
[0063] In the first step, the substrate was immersed in the supramolecular self-assembled hydrophobic active agent and stirred continuously for 2 h.
[0064] In the second step, the substrate is taken out and placed in a forced air oven for 2 hours to dry the anhydrous ethanol on the surface of the substrate to obtain a substrate modified by a supramolecular self-assembled hydrophobic active agent.
[0065] The contact angle test of the substrate without hydrophobic treatment is shown in the figure Figure 3 As shown, the contact angle is 73.3°; Figure 4 This is a SEM image of the lotus leaf structure on the substrate surface after the surface modification by the active agent in Example 1. Figure 5 The contact angle of the substrate after the surface modification of the active agent in Example 1 was 158.8°. Figure 4It can be seen that the surface of the substrate modified by the active agent in Example 1 has a lotus leaf-like structure. Figure 5 It can be seen that the substrate after surface modification by the active agent in Example 1 has good hydrophobicity.
[0066] Example 2
[0067] A method for preparing a ligand, comprising the steps of:
[0068] In the first step, 0.05 mol of 1,8-octanediamine was added to a beaker, and 25 ml of anhydrous ethanol was added to dissolve the 1,8-octanediamine anhydrous ethanol solution was prepared. Subsequently, the 1,8-octanediamine anhydrous ethanol solution was transferred to a 250 ml three-necked flask.
[0069] In the second step, 0.1 mol of 4-formyl imidazole is added to a beaker, and 20 ml of anhydrous ethanol is added to dissolve the mixture to prepare an anhydrous ethanol solution of 4-formyl imidazole. The anhydrous ethanol solution of 4-formyl imidazole is then transferred into a 25 ml constant pressure separatory funnel, and the separatory funnel is assembled into the three-necked flask described in the first step.
[0070] The third step is to heat and stir the three-necked flask until it reaches 70°C, then add 5 ml of glacial acetic acid, open the constant pressure separatory funnel, and allow the anhydrous ethanol solution of 4-aldehyde imidazole to be continuously added dropwise into the three-necked flask.
[0071] Step 4: After 5 hours of reaction, pour the product solution into a beaker, cover with plastic wrap, poke some holes in it, and place it in a fume hood to evaporate the solvent for 15 hours to obtain a viscous mixture of the ligand and glacial acetic acid.
[0072] The fifth step is to place the viscous mixture obtained in the fourth step into a vacuum oven and dry it at 90° C. for 5 hours to remove the glacial acetic acid and obtain the ligand.
[0073] A method for preparing a supramolecular self-assembled hydrophobic active agent, comprising the following steps:
[0074] In the first step, 10 ml of a 25 mmol / L anhydrous ethanol solution of zinc chloride is added to a beaker, followed by 10 ml of a 25 mmol / L anhydrous ethanol solution of the ligand, followed by stirring for 30 minutes and standing for 1 hour to obtain a preliminary coordination solution.
[0075] In the second step, 20 ml of 50 mmol / L anhydrous ethanol solution of 1H,1H,2H,2H-perfluoro-1-ol was added to the preliminary coordination solution obtained in the first step, and 20 ml of anhydrous ethanol was added, and stirred for 10 minutes to obtain a supramolecular self-assembled hydrophobic active agent.
[0076] An application of a supramolecular self-assembled hydrophobic active agent in the field of hydrophobic coatings comprises the following steps:
[0077] In the first step, the substrate was immersed in the supramolecular self-assembled hydrophobic active agent and stirred continuously for 2 h.
[0078] In the second step, the substrate is taken out and placed in a forced air oven for 2 hours to dry the anhydrous ethanol on the surface of the substrate to obtain a substrate modified by a supramolecular self-assembled hydrophobic active agent.
[0079] Figure 6 This is a SEM image of the lotus leaf structure on the substrate surface after the surface modification by the active agent in Example 2. Figure 7 The contact angle of the substrate after the surface modification by the active agent in Example 2 was tested to be 146.5°. Figure 6 It can be seen that the surface of the substrate modified by the active agent in Example 2 has a lotus leaf-like structure. Figure 7 It can be seen that the substrate after surface modification by the active agent in Example 2 has good hydrophobicity.
[0080] In summary, the above are only preferred embodiments of the present invention and are not intended to limit the protection scope of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a supramolecular self-assembled hydrophobic active agent, characterized in that The steps are: The ethanol solution of the ligand, the anhydrous ethanol solution of 1H,1H,2H,2H-perfluoro-1-ol and the ethanol solution of zinc chloride are mixed and stirred to obtain a supramolecular self-assembled hydrophobic active agent; The preparation method of the ligand is: An anhydrous ethanol solution of 1,8-octanediamine, an anhydrous ethanol solution of 4-formylimidazole and glacial acetic acid are mixed for reaction, and the product obtained by the reaction is dried in a vacuum oven at 85-95° C. for 4.5-5.5 hours after the solvent is evaporated in a fume hood for 12-15 hours to obtain a ligand; In the anhydrous ethanol solution of 1,8-octanediamine, the ratio of 1,8-octanediamine to anhydrous ethanol is 0.05 mol:20-30 ml; In the anhydrous ethanol solution of 4-aldehyde imidazole, the ratio of 4-aldehyde imidazole to anhydrous ethanol is 0.1 mol: 15-25 ml; The ratio of 1,8-octanediamine, 4-formylimidazole and glacial acetic acid is 0.05 mol:0.1 mol:3-5 ml.
2. The method for preparing a supramolecular self-assembled hydrophobic active agent according to claim 1, characterized in that: The reaction temperature is 70-80°C and the reaction time is 4-5h.
3. The method for preparing a supramolecular self-assembled hydrophobic active agent according to claim 1, characterized in that: The concentration of the anhydrous ethanol of the ligand is 25mmol / L; The concentration of the anhydrous ethanol solution of zinc chloride is 25mmol / L; The concentration of the anhydrous ethanol solution of 1H,1H,2H,2H-perfluoro-1-alcohol is 50mmol / L; The volume ratio of the zinc chloride ethanol solution, the ligand ethanol solution and the 1H,1H,2H,2H-perfluoro-1-ol anhydrous ethanol solution is 2:1-2:1-3.
4. Application of a supramolecular self-assembled hydrophobic active agent in the field of hydrophobic coating, characterized in that The steps are: The substrate is immersed in the supramolecular self-assembled hydrophobic active agent, and after the immersion is completed, the substrate is taken out and dried to obtain a hydrophobic substrate modified by the supramolecular self-assembled hydrophobic active agent.
5. The use of a supramolecular self-assembly hydrophobic active agent in the field of hydrophobic coating according to claim 4, characterized in that: The immersion time is 0.5-1h.
Citation Information
Patent Citations
Preparation method of strong hydrophobic composite membrane
CN114870637A
Preparation and application of zinc-based bis-imidazole mixed ligand metal organic framework material
CN117487185A
Hydrophobic Property Surface Coating HavingSelf-Cleaning Function and Making Process threrof
KR1020060080642A