Supramolecular aggregate surfactant

The nano-aggregated surfactant prepared by supramolecular chemistry forms a lotus-like leaf structure on the surface of the substrate, solving the hydrophobicity and environmental protection problems of the substrate surface in traditional methods, and achieving efficient hydrophobic modification and fluorescence detection.

CN119060349AActive Publication Date: 2024-12-03BEIJING INST OF TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411173775.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-12-03
Estimated Expiration
2044-08-26

AI Technical Summary

Technical Problem

The prior art is difficult to effectively coat the surface of the substrate with low surface energy hydrophobic materials to form a microscopic hydrophobic structure that is imitated with lotus leaves, and the traditional method uses organic solvents to have environmental problems.

Method used

Using non-covalent interactions of supramolecular chemistry, the bonding ligand is prepared by 4-hydroxypyridine-2,6-diacarboxylic acid and malonic acid, and assembled with perfluorooctanoic acid and lanthanum chloride crosslinking agent to form nano-aggregated states. Supramolecular aggregate surfactant, self-assembled into micelles for substrate surface modification.

Benefits of technology

The base material surface is formed into a lotus leaf structure with good hydrophobicity, and the coating performance and detection ability are enhanced through the solubilization effect of the perfluorinated chain segment and the fluorescence effect of rare earth metals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060349A_ABST
    Figure CN119060349A_ABST
Patent Text Reader

Abstract

The invention relates to a supramolecular aggregate surfactant, and belongs to the technical field of supramolecular coordination chemistry, surface modification engineering and hydrophobic coatings. According to the preparation method, 4-hydroxypyridine-2, 6-dicarboxylic acid and malonic acid are used for preparing a bonding ligand, a supermolecule aggregate in a nano aggregation state is obtained under the help of coordination of carboxyl structures on the 4-hydroxypyridine-2, 6-dicarboxylic acid and perfluorooctanoic acid and lanthanum ions, and the supermolecule aggregate surfactant is formed through self-assembly. The active agent can solubilize fluoride and can also be applied to the field of hydrophobic coatings, and the coatings have the characteristics of lotus leaf imitating structures and hydrophobic waxiness and have good hydrophobic performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a supramolecular aggregate surfactant, and belongs to the fields of supramolecular coordination chemistry, surface modification engineering and hydrophobic coating. Background Art

[0002] Due to the fact that droplets on the hydrophobic surface are difficult to stay, the surface has the characteristics of waterproof, anti-icing, anti-fogging, and self-cleaning. In the field of aerospace, the hydrophobic coating on the surface of the aircraft can effectively prevent the fuselage from icing, ensure flight performance, and avoid air crashes; in the field of transportation, the hydrophobic coating can prevent the glass from fogging, ensure clear vision, and ensure driving safety; in the field of electronics and electrical, the hydrophobic coating can prevent water accumulation on the circuit board and prevent short circuits or rusting of electronic components; in daily life, the hydrophobic coating can prevent the bottom of the pot from sticking. Therefore, the hydrophobic surface has a very broad application prospect.

[0003] Imitation of lotus leaf structure has always been the research direction of researchers of hydrophobic coatings. The surface of lotus leaves has a dense micro-protrusion structure with a height of about 5 microns. Further magnification and observation can reveal that a layer of nano-scale papillae is attached to the surface of the micro-protrusions, with a height of about 200 nanometers. In addition, lotus leaves secrete a layer of biological wax on their surface to resist external invasion. It is precisely the characteristics of this surface micro-nano composite structure combined with biological wax that give lotus leaves unique hydrophobic properties, making it difficult for water droplets to stay on the surface of lotus leaves, and the droplets will carry away dust and debris on the surface during the rapid rolling process on its surface, achieving self-cleaning. At present, the ideas for preparing hydrophobic surfaces are mostly focused on the preparation and coating of biological wax, mainly through perfluorinated compounds or other low surface energy materials. From the perspective of the micro-nano structure of imitating lotus leaves, it is more difficult because the structural structure requires fine design.

[0004] Early research mainly focuses on chemical synthesis methods. Fluoride is insoluble in water and conventional organic solvents, and is soluble in organic fluoride solvents. Therefore, when the material is subjected to hydrophobic surface treatment, it is necessary to infiltrate fluorinated organic solvents. This treatment method is considered to be not green enough because of the toxicity of organic solvents, and is limited in application. Therefore, it is increasingly emerging to prepare green and environmentally friendly water-based super-hydrophobic coatings by replacing volatile organic solvents with water-based solvents. So far, some preparation methods have been explored, such as wet chemical processes of polymer-particle dispersions, electrochemical deposition methods, template methods, etching methods, sol-gel methods, and hydrothermal methods. However, how to coat the substrate surface with both a hydrophobic material with low surface energy and a microscopic hydrophobic structure of imitating lotus leaves is a major problem at present. Summary of the invention

[0005] The technical solution of the present invention is: to overcome the shortcomings of the prior art, and to prepare a supramolecular nano-aggregated surfactant by utilizing the non-covalent interaction of supramolecular chemistry. First, an adhesive ligand is prepared by utilizing 4-hydroxypyridine-2,6-dicarboxylic acid and malonic acid, and then a nano-aggregated supramolecular aggregate is obtained by utilizing the coordination effect of the carboxyl structure on 4-hydroxypyridine-2,6-dicarboxylic acid and perfluorooctanoic acid with metal ions. The active agent has a solubilizing effect on fluoride because the perfluoro chain segment of perfluorooctanoic acid is outside the aggregate. The active agent has a fluorescent effect when coordinated with rare earth metals, and can be used as a fluorescent active agent. At the same time, because of its nano size, the active agent can form a lotus leaf-like structure when used on the surface of a substrate, so that the surface of the substrate has hydrophobicity.

[0006] The technical solution of the present invention is:

[0007] A supramolecular aggregate surfactant, comprising a binding ligand, perfluorooctanoic acid, a lanthanum chloride crosslinking agent and anhydrous ethanol;

[0008] The adhesive ligand, perfluorooctanoic acid and lanthanum chloride crosslinker are self-assembled into micelles and dispersed in anhydrous ethanol;

[0009] The ratio of the lanthanum chloride crosslinking agent, the adhesive ligand, perfluorooctanoic acid and anhydrous ethanol is 1mmol:3-5mmol:4-5mmol:100ml.

[0010] The preparation method of the adhesive ligand is as follows:

[0011] A toluene solution of 4-hydroxypyridine-2,6-dicarboxylic acid and a toluene solution of malonic acid are mixed and reacted in the presence of cyclohexane as a water agent. After the reaction, the filtrate is dried in a vacuum oven at 85-95° C. for 4.5-5.5 hours to obtain a sticky ligand.

[0012] In the toluene solution of 4-hydroxypyridine-2,6-dicarboxylic acid, the ratio of 4-hydroxypyridine-2,6-dicarboxylic acid to toluene is 0.1 mol:20-30 ml;

[0013] In the toluene solution of malonic acid, the ratio of malonic acid to toluene is 0.05 mol:20-30 ml;

[0014] The volume ratio of the cyclohexane water-carrying agent to the total amount of toluene is 4:5, and the total amount of toluene refers to the volume sum of the toluene in the toluene solution of 4-hydroxypyridine-2,6-dicarboxylic acid and the toluene in the toluene solution of malonic acid;

[0015] The molar ratio of 4-hydroxypyridine-2,6-dicarboxylic acid to malonic acid is 2:1.

[0016] The reaction temperature is 100-120°C and the reaction time is 4-5h.

[0017] A method for preparing a supramolecular aggregate surfactant comprises the following steps:

[0018] The ethanol solution of the binding ligand, the ethanol solution of perfluorooctanoic acid and the ethanol solution of lanthanum chloride are mixed and stirred to obtain a supramolecular aggregate surfactant.

[0019] The concentration of the ethanol solution of the binding ligand is 25 mmol / L;

[0020] The concentration of the lanthanum chloride ethanol solution is 25mmol / L;

[0021] The concentration of the ethanol solution of perfluorooctanoic acid is 25 mmol / L;

[0022] The volume ratio of the lanthanum chloride ethanol solution, the binding ligand ethanol solution and the perfluorooctanoic acid ethanol solution is 1:3-5:4-5.

[0023] The invention discloses an application of a supramolecular aggregate surfactant in the field of hydrophobic coating, comprising the steps of: dipping a substrate in the supramolecular aggregate surfactant, taking out the substrate after dipping, drying the substrate, and obtaining a hydrophobic substrate modified by the supramolecular aggregate surfactant. The dipping time is 0.5-1h.

[0024] The supramolecular surfactant is added into the insoluble fluoride perfluorodecanol and stirred, so that the insoluble perfluorodecanol can be dissolved.

[0025] The ratio of the mass of the insoluble fluoride to the added supramolecular aggregate surfactant is 0.1 g: 5-10 ml.

[0026] Beneficial Effects

[0027] In the present invention, a clamp-type adhesive ligand is prepared by esterification reaction of 4-hydroxypyridine-2,6-dicarboxylic acid and malonic acid, and the adhesive ligand can bond lanthanum ions to form supramolecular aggregates. The lanthanum ions in the supramolecular aggregates attract the carboxyl group of perfluorooctanoic acid, leaving the perfluoro chain segment in the shell of the aggregate, and self-assemble into a supramolecular aggregate surfactant. The coordination of the carboxyl group and the rare earth metal can make the supramolecular aggregate surfactant fluorescent, and the perfluoro chain of the aggregate shell can make the active agent produce a solubilizing effect on the perfluoro compound. At the same time, the active agent can form a lotus leaf-like structure when used on the surface of the substrate due to its nanoscale, so that the substrate surface has hydrophobicity. Therefore, this surfactant can be used in the field of hydrophobic coatings to increase the hydrophobicity of the material, and the degree of wear of the coating can be detected according to the fluorescence attenuation of the coating. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 Schematic diagram of self-assembly of supramolecular aggregates in nano-aggregate state;

[0029] Figure 2 This is a cryo-transmission electron microscopy image of nano-aggregated supramolecular aggregates in water.

[0030] Figure 3 This is the contact angle test diagram of the substrate without hydrophobic treatment. (73.3°)

[0031] Figure 4 This is a SEM image of the lotus leaf structure on the substrate surface after surface modification by the active agent in Example 1.

[0032] Figure 5 The contact angle test of the substrate after the surface modification of the active agent in Example 1. (147.6°)

[0033] Figure 6 This is a SEM image of the lotus leaf structure on the substrate surface after surface modification by the active agent in Example 2.

[0034] Figure 7 The contact angle test of the substrate after surface modification by the active agent in Example 2. (145.1°). DETAILED DESCRIPTION

[0035] The present invention is further described below by way of examples, but the examples do not limit the protection scope of the present invention.

[0036] A supramolecular aggregate surfactant, comprising a binding ligand, perfluorooctanoic acid, a lanthanum chloride crosslinking agent and anhydrous ethanol;

[0037] The adhesive ligand, perfluorooctanoic acid and lanthanum chloride crosslinker are self-assembled into micelles and dispersed in anhydrous ethanol, such as Figure 1 and Figure 2 As shown;

[0038] The ratio of the lanthanum chloride crosslinking agent, the adhesive ligand, perfluorooctanoic acid and anhydrous ethanol is 1mmol:3-5mmol:4-5mmol:100ml.

[0039] A supramolecular aggregate surfactant, the preparation raw materials include main raw materials and auxiliary raw materials, the main raw materials include 4-hydroxypyridine-2,6-dicarboxylic acid, malonic acid, anhydrous lanthanum chloride, perfluorooctanoic acid, the auxiliary raw materials are water-carrying agent and solvent.

[0040] The water-carrying agent is cyclohexane, and the solvent is toluene and anhydrous ethanol.

[0041] A method for preparing an adhesive ligand, comprising the following steps:

[0042] The first step is to add 0.05 mol of malonic acid into a beaker, dissolve it in 20 ml of toluene, and stir evenly to prepare a toluene solution of malonic acid.

[0043] In the second step, 0.1 mol of 4-hydroxypyridine-2,6-dicarboxylic acid is added to a beaker, dissolved in 20 ml of toluene, and stirred evenly to obtain a toluene solution of 4-hydroxypyridine-2,6-dicarboxylic acid. The toluene solution of 4-hydroxypyridine-2,6-dicarboxylic acid is then transferred to a three-necked flask.

[0044] In the third step, the malonic acid toluene solution obtained in the first step is transferred into a constant pressure separatory funnel and assembled with the three-necked flask in the second step.

[0045] Step 4: Add 10 ml of cyclohexane to the three-necked flask and heat to 110°C for 4 hours. During the reaction, keep one port open to facilitate the discharge of the mixed steam of cyclohexane and water, and add 7 ml of cyclohexane every hour.

[0046] Step 5. Observe the flask to see if bubbles appear. If so, continue heating at 110°C until no more bubbles appear.

[0047] In the sixth step, the solution obtained in the fifth step is transferred out and placed in a vacuum oven, and dried at 95° C. for 5 hours to obtain a bonding ligand.

[0048] A method for preparing a supramolecular aggregate surfactant comprises the following steps:

[0049] In the first step, the adhesive ligand is configured into a 25 mmol / L anhydrous ethanol solution, lanthanum chloride is configured into a 25 mmol / L anhydrous ethanol solution, and perfluorooctanoic acid is configured into a 25 mmol / L anhydrous ethanol solution as the coordination raw materials of the supramolecular aggregate surfactant.

[0050] In the second step, 10 ml of lanthanum chloride solution, adhesive ligand solution (volume ratio of lanthanum chloride solution to adhesive ligand solution is 1:3-5), and perfluorooctanoic acid solution (volume ratio of lanthanum chloride solution to perfluorooctanoic acid solution is 1:4-5) are added into a beaker, stirred for 20 minutes and allowed to stand for ten minutes to obtain a supramolecular aggregate surfactant.

[0051] An application of a supramolecular aggregate surfactant in the field of hydrophobic coatings comprises the following steps:

[0052] In the first step, the substrate was immersed in the supramolecular aggregate surfactant and stirred for 2 hours. The contact angle test of the substrate without hydrophobic treatment is shown in the figure below. Figure 3 As shown, the contact angle is 73.3°;

[0053] In the second step, the substrate is taken out and placed in a forced air oven for 2 hours to dry the substrate, thereby obtaining a material modified by a supramolecular aggregate surfactant.

[0054] Example 1

[0055] A method for preparing an adhesive ligand, comprising the following steps:

[0056] The first step is to add 0.05 mol of malonic acid into a beaker, dissolve it in 20 ml of toluene, and stir evenly to prepare a toluene solution of malonic acid.

[0057] In the second step, 0.1 mol of 4-hydroxypyridine-2,6-dicarboxylic acid is added to a beaker, dissolved in 20 ml of toluene, and stirred evenly to obtain a toluene solution of 4-hydroxypyridine-2,6-dicarboxylic acid. The toluene solution of 4-hydroxypyridine-2,6-dicarboxylic acid is then transferred to a three-necked flask.

[0058] In the third step, the malonic acid toluene solution obtained in the first step is transferred into a constant pressure separatory funnel and assembled with the three-necked flask in the second step.

[0059] Step 4: Add 10 ml of cyclohexane to the three-necked flask and heat to 110°C for 4 hours. During the reaction, keep one port open to facilitate the discharge of the mixed steam of cyclohexane and water, and add 7 ml of cyclohexane every hour.

[0060] Step 5. Observe the flask to see if bubbles appear. If so, continue heating at 110°C until no more bubbles appear.

[0061] In the sixth step, the solution obtained in the fifth step is transferred out and placed in a vacuum oven, and dried at 95° C. for 5 hours to obtain a bonding ligand.

[0062] A method for preparing a supramolecular aggregate surfactant comprises the following steps:

[0063] In the first step, the adhesive ligand is configured into a 25 mmol / L anhydrous ethanol solution, lanthanum chloride is configured into a 25 mmol / L anhydrous ethanol solution, and perfluorooctanoic acid is configured into a 25 mmol / L anhydrous ethanol solution as the coordination raw materials of the supramolecular aggregate surfactant.

[0064] In the second step, 10 ml of lanthanum chloride solution, 40 ml of binding ligand solution, and 40 ml of perfluorooctanoic acid solution were added to a beaker, followed by adding 10 ml of anhydrous ethanol, stirring for 20 minutes and standing for ten minutes to obtain a supramolecular aggregate surfactant.

[0065] An application of a supramolecular aggregate surfactant in the field of hydrophobic coatings comprises the following steps:

[0066] In the first step, the substrate was immersed in the supramolecular aggregate surfactant and stirred for 2 hours. The contact angle test of the substrate without hydrophobic treatment is shown in the figure below. Figure 3 As shown, the contact angle is 73.3°;

[0067] In the second step, the substrate is taken out and placed in a forced air oven for 2 hours to dry the substrate, thereby obtaining a material modified by a supramolecular aggregate surfactant. Figure 4 Example 1 SEM image of the lotus leaf structure on the substrate surface after surface modification by the active agent. Figure 5 The contact angle test of the substrate after the surface modification of the active agent in Example 1. Figure 4 It can be seen that the surface of the substrate after surface modification by the active agent in Example 1 has a lotus leaf-like structure. Figure 5 It can be seen that the contact angle of Example 1 is 147.6°, indicating that Example 1 has good hydrophobicity;

[0068] Example 2

[0069] A method for preparing an adhesive ligand, comprising the following steps:

[0070] The first step is to add 0.05 mol of malonic acid into a beaker, dissolve it in 20 ml of toluene, and stir evenly to prepare a toluene solution of malonic acid.

[0071] In the second step, 0.1 mol of 4-hydroxypyridine-2,6-dicarboxylic acid is added to a beaker, dissolved in 20 ml of toluene, and stirred evenly to obtain a toluene solution of 4-hydroxypyridine-2,6-dicarboxylic acid. The toluene solution of 4-hydroxypyridine-2,6-dicarboxylic acid is then transferred to a three-necked flask.

[0072] In the third step, the malonic acid toluene solution obtained in the first step is transferred into a constant pressure separatory funnel and assembled with the three-necked flask in the second step.

[0073] Step 4: Add 10 ml of cyclohexane to the three-necked flask and heat to 110°C for 4 hours. During the reaction, keep one port open to facilitate the discharge of the mixed steam of cyclohexane and water, and add 7 ml of cyclohexane every hour.

[0074] Step 5. Observe the flask to see if bubbles appear. If so, continue heating at 110°C until no more bubbles appear.

[0075] In the sixth step, the solution obtained in the fifth step is transferred out and placed in a vacuum oven, and dried at 95° C. for 5 hours to obtain a bonding ligand.

[0076] A method for preparing a supramolecular aggregate surfactant comprises the following steps:

[0077] In the first step, the adhesive ligand is configured into a 25 mmol / L anhydrous ethanol solution, lanthanum chloride is configured into a 25 mmol / L anhydrous ethanol solution, and perfluorooctanoic acid is configured into a 25 mmol / L anhydrous ethanol solution as the coordination raw materials of the supramolecular aggregate surfactant.

[0078] In the second step, 10 ml of lanthanum chloride solution, 30 ml of binding ligand solution, and 50 ml of perfluorooctanoic acid solution were added to a beaker, followed by adding 10 ml of anhydrous ethanol, stirring for 20 minutes and standing for ten minutes to obtain a supramolecular aggregate surfactant.

[0079] An application of a supramolecular aggregate surfactant in the field of hydrophobic coatings comprises the following steps:

[0080] In the first step, the substrate was immersed in the supramolecular aggregate surfactant and stirred for 2 hours. The contact angle test of the substrate without hydrophobic treatment is shown in the figure below. Figure 3 As shown, the contact angle is 73.3°;

[0081] In the second step, the substrate is taken out and placed in a forced air oven for 2 hours to dry the substrate, thereby obtaining a material modified by a supramolecular aggregate surfactant. Figure 6 Example 2 SEM image of the lotus leaf structure on the substrate surface after surface modification by the active agent. Figure 7 The contact angle test of the substrate after the surface modification of the active agent in Example 2. Figure 6 It can be seen that the surface of the substrate modified by the active agent in Example 2 has a lotus leaf-like structure. Figure 7 It can be seen that the contact angle of the substrate after surface modification by the active agent in Example 2 is 145.1°, indicating that Example 2 has good hydrophobicity.

[0082] A supramolecular aggregate surfactant is used as a solubilizer, comprising the following steps:

[0083] In the first step, 0.1 g of perfluorodecanol was placed in a beaker containing 20 ml of distilled water and stirred for 1 hour but did not dissolve.

[0084] In the second step, 10 ml of supramolecular aggregate surfactant was added to the beaker and stirred for 1 hour, and it was found that perfluorodecanol was dissolved. Since the solubilization effect of surfactants in the formulation range is almost the same, only the solubilization effect of Example 2 is characterized, which does not mean that other ratios in the formulation range do not have solubilization effect.

[0085] In summary, the above are only preferred embodiments of the present invention and are not intended to limit the protection scope of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A supramolecular aggregate surfactant, characterized in that: The supramolecular aggregate surfactant comprises a bonding ligand, perfluorooctanoic acid, a lanthanum chloride crosslinking agent and anhydrous ethanol; The adhesive ligand, perfluorooctanoic acid and lanthanum chloride crosslinker are self-assembled into micelles and dispersed in anhydrous ethanol; The ratio of the lanthanum chloride crosslinking agent, the adhesive ligand, perfluorooctanoic acid and anhydrous ethanol is 1mmol:3-5mmol:4-5mmol:100ml.

2. A supramolecular aggregate surfactant according to claim 1, characterized in that: The preparation method of the adhesive ligand is as follows: A toluene solution of 4-hydroxypyridine-2,6-dicarboxylic acid and a toluene solution of malonic acid are mixed and reacted in the presence of cyclohexane as a water agent. After the reaction, the filtrate is dried in a vacuum oven at 85-95° C. for 4.5-5.5 hours to obtain a sticky ligand.

3. A supramolecular aggregate surfactant according to claim 2, characterized in that: In the toluene solution of 4-hydroxypyridine-2,6-dicarboxylic acid, the ratio of 4-hydroxypyridine-2,6-dicarboxylic acid to toluene is 0.1 mol:20-30 ml; In the toluene solution of malonic acid, the ratio of malonic acid to toluene is 0.05 mol:20-30 ml; The volume ratio of the cyclohexane water-carrying agent to the total amount of toluene is 4:5, and the total amount of toluene refers to the volume sum of the toluene in the toluene solution of 4-hydroxypyridine-2,6-dicarboxylic acid and the toluene in the toluene solution of malonic acid; The molar ratio of 4-hydroxypyridine-2,6-dicarboxylic acid to malonic acid is 2:

1.

4. A supramolecular aggregate surfactant according to claim 2, characterized in that: The reaction temperature is 100-120°C and the reaction time is 4-5h.

Citation Information

Patent Citations

  • Preparation method for superhydrophobic self-cleaning fluorescent coating

    CN108409911A

  • Ten-core 3d-4f supramolecular nanocage material and preparation method thereof

    CN117801304A

  • Fluorine-containing block copolymer and preparation method thereof

    CN118240198A